Solid electrolyte material, preparation method, electrode and lithium ion battery
By doping Eu and Gd on the basis of Li2ZrCl6, and optimizing the selection and molar ratio of element N, a halide solid electrolyte material with the general chemical formula Li2+a+2bZr1-a-bMaNbX6 was developed, solving the problem of cost and ion The contradiction between conductivities enables the preparation of low-cost, high-ion conductivity solid electrolyte materials.
Patent Information
- Application Number
- CN202310158786.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-23
AI Technical Summary
There is a contradiction between cost and ionic conductivity of existing halide solid electrolyte materials, making it difficult to achieve low cost and high ionic conductivity at the same time.
A halide solid electrolyte material with the general chemical formula Li2+a+2bZr1-a-bMaNbX6 is used. The element M is selected from Eu and Gd. The value range of 2+a+2b is 2.15-2.65. The ionic radius of the element N is 60 -95pm, with diffraction peaks in a specific diffraction angle range through XRD analysis, combined with optimization of the molar ratio of element X, and the preparation method includes mixing and sintering processes.
The conductivity of lithium ions is improved, the microstructure and performance of the material are optimized through the synergistic effect of doping elements, and the development of solid electrolyte materials with low cost and high ionic conductivity is achieved.
Smart Images

Figure CN116315050B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a solid electrolyte material, a preparation method, an electrode, and a lithium-ion battery. Background Art
[0002] Lithium-ion batteries have been widely used in various portable electronic products and electric vehicles due to their high energy density. However, the safety of traditional lithium-ion batteries has always been criticized due to the use of flammable, explosive and toxic electrolytes, and the energy density of liquid batteries using electrolytes has approached the limit after years of development. Solid-state batteries that use solid electrolytes to replace the separators and electrolytes in traditional lithium-ion batteries are currently recognized as the next generation of new battery technology, among which solid electrolyte materials are the core technology of solid-state batteries.
[0003] At present, the main solid electrolyte materials include polymer solid electrolytes, sulfide solid electrolytes, oxide solid electrolytes, etc. All of the above materials have their own advantages and disadvantages. For example, although the sulfide solid electrolyte has high ion conductivity, it is too sensitive to moisture and air, and has high preparation costs and great difficulty in industrialization; although the oxide solid electrolyte has a simple preparation process and is easy to industrialize, its interface performance with the positive and negative electrodes is poor, which affects the overall performance of the battery.
[0004] Compared with oxide solid electrolytes and sulfide solid electrolytes, halide solid electrolytes are a new type of ceramic material, which has attracted attention because it has the advantages of both oxide solid electrolytes and sulfide solid electrolytes. The known halide solid electrolytes such as Li3InCl6 have high production costs due to the use of a large amount of rare earth elements. For example, patent document CN112204675B discloses a halide solid electrolyte with a chemical formula of Li 6-4a M a X6, wherein M is selected from the IVB group elements of Zr, Hf, and Ti. The embodiment part also recognizes the different properties exhibited by elements such as Zr and Hf under different doping and different ratios. In view of the low cost and relatively high ionic conductivity of Li2ZrCl6, the development of Li2ZrCl6 halide solid electrolyte materials has aroused the interest of some scholars, and it is very necessary to develop a new type of doped Li2ZrCl6 material. Summary of the invention
[0005] In order to solve one or more of the above-mentioned technical problems existing in the prior art, the embodiments of the present application provide a solid electrolyte material, a preparation method, an electrode, and a lithium-ion battery to solve the contradictory relationship between the ionic conductivity and cost of the current halide solid electrolyte, and prepare a solid electrolyte material with lower cost and higher ionic conductivity.
[0006] In order to solve the above problems, the present application provides a solid electrolyte material in the first aspect, wherein the solid electrolyte material comprises a halide solid electrolyte material, and the chemical formula of the halide solid electrolyte material is Li 2+a+2b Zr 1-a- b M a N b X6;
[0007] The element M is selected from one or both of Eu and Gd; and the value range of 2+a+2b is 2.15-2.65;
[0008] The element N is different from the element M, and the ionic radius r(N) of the element N is 60 picometers<r(N)<95 picometers;
[0009] The value range of a+b is 0.1-0.5, and the value range of a / b is 1-6;
[0010] X is one or more elements selected from F, Cl, Br and I.
[0011] In an optional embodiment, the value range of 2+a+2b is 2.2-2.45.
[0012] In an optional embodiment, the value range of a / b is 2-6.
[0013] In an optional embodiment, the ionic radius r(M) of the element M and the ionic radius r(N) of the element N satisfy 0.6<r(N) / r(M)<1.05.
[0014] In an optional embodiment, the halide solid electrolyte material is subjected to XRD analysis, and when irradiated with CuK α, has diffraction peaks in the range of diffraction angle 2θ of 25.3-26.2° and in the range of diffraction angle 2θ of 35.2-36.2°.
[0015] In an optional embodiment, the element N is selected from one or more of Co, Cu, Zn, Mg, and Cd.
[0016] In an optional embodiment, the element X is a mixture of multiple elements, and the element X includes element Cl, and the molar ratio of the element Cl in the element X is in the range of 80-99.99%; preferably, the molar ratio of the element Cl in the element X is in the range of 83-96%.
[0017] In an optional embodiment, the element M is a mixture of Eu and Gd, and the chemical formula Li 2+a+2b Zr 1-a-b M a N b X6 specifically Li2+a+2b Zr 1-a-b Eu a1 G a2 N b X6, a=a1+a2; preferably, 2<a1 / a2<5.
[0018] The second aspect of the present application provides a method for preparing the halide solid electrolyte material as described above, comprising the following steps:
[0019] S1. The lithium salt, the zirconium salt, the salt corresponding to the element M, and the salt corresponding to the element N are placed in a mixing device in a preset stoichiometric ratio to obtain an intermediate;
[0020] S2. Sintering the intermediate obtained in step S1 to obtain the halide solid electrolyte material;
[0021] The chemical formula of the halide solid electrolyte material is Li 2+a+2b Zr 1-a-b M a N b X6;
[0022] The element M is selected from one or both of Eu and Gd; and the value range of 2+a+2b is 2.15-2.65;
[0023] The element N is different from the element M, and the ionic radius r(N) of the element N is 60 picometers<r(N)<95 picometers;
[0024] The value range of a+b is 0.1-0.5, and the value range of a / b is 1-6;
[0025] X is one or more elements selected from F, Cl, Br, and I.
[0026] In an optional embodiment, the mixing device is a ball mill; further preferably, the mixing device is a ZrO2 ball mill.
[0027] In an optional embodiment, the ball milling speed of the ball mill is 200-800 rpm, and the ball milling time is 10-50h;
[0028] In an optional embodiment, the sintering temperature of step S2 is 150-350°C;
[0029] In an optional embodiment, the sintering time of step S2 is 0-40 hours.
[0030] In an optional embodiment, the value range of 2+a+2b is 2.2-2.45.
[0031] In an optional embodiment, the ionic radius r(M) of the element M and the ionic radius r(N) of the element N satisfy 0.6<r(N) / r(M)<1.05.
[0032] In an optional embodiment, the halide solid electrolyte material is subjected to XRD analysis, and when irradiated with CuKα, has diffraction peaks in the range of diffraction angle 2θ of 25.3-26.2° and in the range of diffraction angle 2θ of 35.2-36.2°.
[0033] In an optional embodiment, the element N is selected from one or more of Co, Cu, Zn, Mg, and Cd.
[0034] In an optional embodiment, the element X is a mixture of multiple elements, and the element X includes element Cl, and the molar ratio of the element Cl in the element X is in the range of 80-99.99%; preferably, the molar ratio of the element Cl in the element X is in the range of 83-96%.
[0035] In an optional embodiment, the element M is a mixture of Eu and Gd, and the chemical formula of the solid electrolyte material is Li 2+a+2b Zr 1- a -b M a N b X6 specifically Li 2+a+2b Zr 1-a-b Eu a1 G a2 N b X6, a=a1+a2.
[0036] In an optional embodiment, 2<a1 / a2<5.
[0037] The third aspect of the present application discloses an electrode, which comprises the solid electrolyte material as described above or the halide solid electrolyte material prepared by the preparation method as described above.
[0038] In an optional embodiment, the electrode comprises an active material layer, and the active material layer includes the halide solid electrolyte material.
[0039] In an optional embodiment, the electrode is a positive electrode, the positive electrode includes a positive electrode active material layer, the positive electrode active material layer includes a positive electrode solid electrolyte layer; the positive electrode solid electrolyte layer includes the halide solid electrolyte material.
[0040] In an optional embodiment, the electrode is a negative electrode, the negative electrode includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode solid electrolyte layer; the negative electrode solid electrolyte layer includes the halide solid electrolyte material.
[0041] In an optional embodiment, the solid electrolyte layer is composed of a composite solid electrolyte, and the composite solid electrolyte contains the halide solid electrolyte material.
[0042] In an optional embodiment, the positive electrode solid electrolyte layer or the negative electrode solid electrolyte layer only contains the halide solid electrolyte material.
[0043] In an optional embodiment, the thickness of the solid electrolyte layer is 0.1-100 microns; preferably, 1-30 microns.
[0044] A fourth aspect of the present application provides a lithium-ion battery, which includes a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte comprises the solid electrolyte material as described above or the halide solid electrolyte material obtained by the preparation method as described above.
[0045] In an optional embodiment, the electrolyte is composed only of the halide solid electrolyte material, and the lithium-ion battery includes a positive electrode, a negative electrode, and a halide solid electrolyte material. The halide solid electrolyte material is located between the positive electrode and the negative electrode to isolate the positive electrode and the negative electrode.
[0046] In an optional embodiment, the electrolyte includes the halide solid electrolyte material, and at least one of the positive electrode and the negative electrode includes the halide solid electrolyte material.
[0047] Beneficial effects:
[0048] The present application doped elements of different valence states to improve the conductivity of lithium ions, and further used Li2ZrCl6 as the basic structure, tetravalent Zr as the main element, and doped at least one of Eu and Gd to improve the conductivity of lithium ions. At the same time, by doping with an element N that is different from the elements Eu and Gd and has a suitable ionic radius, the complementary enhancement effect between multiple elements is achieved, and a small amount of N element doping can finely control the concentration of lithium elements, avoiding the side effects caused by excessive and large-scale control of the concentration of lithium elements. Further, by doping with element N, the synergistic effect between Eu, Gd and element N is achieved; at the same time, surprisingly, the microstructure of the halide solid electrolyte of the present application changes, and XRD observation can be performed, and two diffraction peaks can be observed under certain angle conditions, which has better ionic conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 : Impedance spectrum of Example 10;
[0050] Figure 2 :XRD comparison charts of various materials;
[0051] Figure 3 :Flowchart of the method of the embodiment of the present application. Detailed implementation mode
[0052] As described in the background art, in the existing halide solid electrolyte material Li2ZrCl6, Zr is used to replace rare earth elements, achieving low cost. At the same time, for the doping research of ceramic materials, doping different valence elements to adjust the carrier concentration is a known research method. However, the relevant research is only carried out under the existing theoretical system of heterovalent doping; when considering the mixing of multiple elements in a specific material system, the difference in heterovalent doping caused by the difference in the main elements is not considered; in this application, aiming at the characteristics of Zr as the main element in the Li2ZrCl6 structure, supplemented by the co-doping of Eu and Gd and elements with specific ionic radii, unexpectedly, this doping causes changes in the microstructure of the material, and this synergistic effect makes the overall performance of the Li2ZrCl6 material change significantly.
[0053] This embodiment provides a halide solid electrolyte material, the chemical general formula of which is Li 2+a+2b Zr 1-a-b M a N b X6.
[0054] Wherein the element M is selected from one or a mixed element of Eu and Gd.
[0055] Preferably, the ionic radius r(N) of the element N and the ionic radius r(M) of the element M satisfy the following relationship:
[0056] 0.6 < r(N) / r(M) < 1.05; and the element N is different from the element M.
[0057] In the prior art, there are three calculation methods for ionic radius, including contact radius, crystal radius and effective radius; the ionic radius in this application adopts the effective radius to reflect the ion size; the ionic radius in this application is based on the ionic radius of six-coordinated O 2- being 140 pm and the ionic radius of six-coordinated F - being 133 pm, and considering the coordination number (CN) of metal ions and the electron spin state of the first row transition. When there are two data of low spin and high spin, the low spin data is taken as the standard.
[0058] It can be understood that the ionic radii of all elements can be queried from the Lange's Handbook of Chemistry (LANG’SHANDBOOK OF CHEMISTRY, James G. Speightp, Ph.D. 1972, 1151-p1156, table 1.31, ISBN: 0-07-143220-5). Specifically, the element N that meets the requirements can be selected through this handbook. It can be understood that the ionic radii within the error range are not considered.
[0059] Through experimental observation, the ionic radius r(N) of element N and the ionic radius r(M) of element M have a certain influence on the ionic conductivity. When the relationship of 0.6<r(N) / r(M)<1.05 is satisfied, the conductivity is higher. As a mere guess, and not a limitation on the scope of protection, when there is a certain gap between the ionic radius of element N and element M but the gap is not too large, the doping effect of Eu and Gd is best. Surprisingly, the synergistic doping of the present application causes the microstructure of the halide solid electrolyte to change, and this change can be confirmed by XRD (X-ray diffraction). XRD (X-ray diffraction) can quantitatively and qualitatively analyze the microstructure of materials such as crystalline phases. The halide solid electrolyte material of the present application has diffraction peaks in the range of 25.3-26.2° and in the range of 35.2-36.2° for the diffraction angle 2θ when the structural analysis is performed by X-ray diffraction method and measured by θ-2θ method using Cu-Kα rays as X-rays.
[0060] Surprisingly, only the halide solid electrolyte to be protected by this application will show corresponding characteristic peaks in XRD characterization. The relevant microscopic explanation is unclear, but it can be determined that this structure is beneficial to the overall performance of the halide solid electrolyte. For the standard structure of Li2ZrCl6, the doping of appropriate types of M and N elements increases the stoichiometric ratio of lithium in Li2ZrCl6; the increase in lithium content increases the ionic conductivity of the halide solid electrolyte, but too high a lithium content may bring negative effects. In this application, the value range of (2+a+2b) is 2.15-2.65, and the preferred value range is 2.2-2.45. The stoichiometric ratio of lithium within the appropriate range can ensure the ionic conductivity of the halide solid electrolyte and will not have a negative impact on other properties.
[0061] In the present application, the doping of Eu and Gd plays a role in the main doping of Li2ZrCl6, the doping concentration of element N is less than that of element M, and the supplementary and reinforcing effect of element N on the doping of Eu and Gd makes it possible to further improve the doping effect of Eu and Gd after adding element N.
[0062] Preferably, the element N is selected from one or more of Co, Cu, Zn, Mg and Cd.
[0063] As an embodiment, the element M is selected from one of Eu and Gd; as another embodiment, the element M is a mixture of Eu and Gd.
[0064] It can be understood that when M is a mixture of Eu and Gd, the halide solid electrolyte is a mixed doping structure with a structural formula of Li2+a+2b Zr 1-a-b Eu a1 G a2 N b X6, wherein a=a1+a2. Preferably, 2<a1 / a2<5, and the value range of a+b is 0.1-0.5.
[0065] Li2ZrCl6 is a material with Zr as the main element. When the doping element is excessive, resulting in a decrease in the Zr content and loss of the qualification of the main element, the microstructure or macroscopic performance of the halide solid electrolyte will undergo unexpected changes. Even if this change is occasionally positive, it is also undesirable for industrial production and research, because it is not conducive to industrial production and corresponding quality control. The main purpose of this application is to dope and modify the Li2ZrCl6 halide solid electrolyte material with Zr as the main element to obtain a structural formula of Li 2+a+2b Zr 1-a-b M a N b X6 halide solid electrolyte, in which Zr as the main element exceeds 50% in the stoichiometric ratio, so as to finally obtain a material that combines electrochemical performance and cost issues of industrial production.
[0066] Preferably, the element X is one or more of F, Cl, Br, and I;
[0067] As an embodiment, the element X is one of F, Cl, Br, and I; as another embodiment, the element X is a mixture of two or more of F, Cl, Br, and I;
[0068] When the halogen is partially doped with F, Br and I, it helps to improve the comprehensive performance such as conductivity or electrochemical window, but too much doping will also have an unexpected negative effect, and the impact on the ionic conductivity of the solid electrolyte material is negative. Surprisingly, Cl and Zr have a good synergistic effect. Therefore, in a preferred embodiment, when the element X is a mixture, the element X contains Cl and contains at least one of F and I, and the molar ratio of the Cl element in the element X is in the range of 80-99.99%; further preferably, the molar ratio of the Cl element is in the range of 83-96%.
[0069] It can be understood that the molar fraction here means the molar fraction of a certain element in element X. For example, when element X is a mixture of two elements F and Cl, and the molecular structure is Cl 5.75 F 0.25 When , the molar proportion of Cl is 5.75 / 6=95.8%.
[0070] In the present application, the halide solid electrolyte is doped with Eu and Gd, and on this basis, a small amount of auxiliary elements are doped to improve the overall performance of the electrolyte material. Considering the overall effect, the auxiliary elements are as little as possible as compared to Eu and Gd, so the value range of a / b is 1-6; optionally, the value of a / b can be but is not limited to 1.5, 1.8, 2.0, 2.3, 2.5, 2.7, 2.9, 3.0, 3.1, 3.3, 3.5, 3.8, 4.0, 4.1, 4.4, 4.7, 5.0, 5.3, 5.5, 5.9, 6.0; preferably, the value range of a / b is 2-4.
[0071] Preferably, the halide solid electrolyte material is in any form of a glass phase, a glass-ceramic phase or a crystalline phase.
[0072] Corresponding to the above-mentioned solid electrolyte material, this embodiment further includes an electrode, and the electrode includes the above-mentioned solid electrolyte material.
[0073] Preferably, the electrode is a positive electrode, the positive electrode comprises a positive electrode active material layer, the positive electrode active material layer comprises a solid electrolyte layer; the solid electrolyte layer comprises the halide solid electrolyte material.
[0074] Preferably, the electrode is a negative electrode, the active material layer is a negative electrode active material layer, the negative electrode active material layer comprises a solid electrolyte layer; and the solid electrolyte layer comprises the halide solid electrolyte material.
[0075] Preferably, the solid electrolyte layer comprises only the halide solid electrolyte material;
[0076] Preferably, the solid electrolyte layer comprises two or more halide solid electrolyte materials.
[0077] It can be understood that the above two or more halide solid electrolyte materials are selected from the halide solid electrolyte materials mentioned above, that is, the solid electrolyte layer is only composed of the halide solid electrolyte material involved in this application.
[0078] Preferably, the solid electrolyte layer is composed of a composite solid electrolyte, and the composite solid electrolyte contains the halide solid electrolyte material.
[0079] It can be understood that a composite solid electrolyte refers to a solid electrolyte component composed of two or more solid electrolyte materials. The composite solid electrolyte in the present application can be understood as a solid electrolyte material composed of the halide solid electrolyte material of the present application and other types of solid electrolytes. The present application does not specifically limit the types of other types of solid electrolytes. Without violating the inventive concept of the present application, any known type of solid electrolyte can be used in the present application, including but not limited to oxide solid electrolytes, sulfide solid electrolytes, halide solid electrolytes, hydride solid electrolytes, boride solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.
[0080] As an embodiment, the oxide solid electrolyte may include one or more garnet ceramics, LISICON type oxides, NASICON type oxides and perovskite type ceramics. For example, the one or more garnet ceramics may be selected from the group consisting of: Li 6.5 LqCy 1.75 Te 0.25 O 12 、Li7La3Zr2O 12 , Li 6.2 Ga 0.3 La 2.9 R 0.05 Zr2O 12 , Li 6.85 La 2.9 Ca 0.1 Zr 1.75 Nb 0.25 O 12 , Li 6.25 Al 0.25 La3Zr2O 12 , Li 6.75 LqCy 1.75 Nb 0.25 O 12 And combinations thereof. One or more LISICON-type oxides may be selected from the group consisting of: Li 14 Zn(GeO4)4、Li 3+x (P 1-x Si x )O4 (where 0<x<1), Li 3+x Ge x V 1-x O4 (where 0<x<1) and combinations thereof. One or more NASICON-type oxides may be defined by LiMM′(PO4)3, where M and M′ are independently selected from Al, Ge, Ti, Sn, Hf, Zr and La. For example, in certain variations, one or more NASICON-type oxides may be selected from the group consisting of: Li1+x Al x Ge 2-x (PO4)3(LAGP)(where 0≤x≤2), Li 1+x Al x Ti 2-x (PO4)3(LATP)(where 0≤x≤2), Li 1+x Y x Zr 2-x (PO4)3(LYZP)(where 0≤x≤2), Li 1.a Al 0.3 Ti 1.7 (PO4)3, LiTi2(PO4)3, LiGeTi(PO4)3, LiGe2(PO4)3, LiHf2(PO4)3 and combinations thereof. One or more perovskite ceramics may be selected from the group consisting of: Li 3.3 La 0.53 TiO3、LiSr 1.65 Zr 1.3 Ta 1.7 O9, Li 2x-y Sr 1-x Ta y Zr 1-y O3 (where x = 0.75y and 0.60 < y < 0.75), Li 3 / 8 Sr 7 / 16 Nb 3 / 4Zr 1 / 4 O3, (where 0<x<0.25) and combinations thereof. In one variation, one or more oxide-based materials may have a value greater than or equal to about 10 -5 S / cm to less than or equal to about 10 -1 S / cm ionic conductivity.
[0081] As an embodiment, the sulfide solid electrolyte may include one or more sulfide-based materials selected from the following: Li2S-P2S5, Li2S-P2S5-MS X (where M is Si, Ge and Sn and 0≤x≤2), Li 3.4 Si 0.4 P 0.6 S4, Li 10 GeP2S 11.700.3 , Li 9.6 P3S 12 、Li7P3S 11 、Li9P3S9O3、Li 10.35 Si 1.35 P 1.65 S 12, Li 9.81 Sn 0.81 P 2.19 S 12 , Li 10 (Si 0.5 Ge 0.5 )P2S 12 、Li(Ge 0.5 Sn 0.5 )P2S 12 、Li(Si 0.5 Sn 0.5 )PsS 12 , Li 10 GeP2S 12 (LGPS), Li6PS5X (where X is Cl, Br or I), Li7P2S8I, Li 10.35 Ge 1.35 P 1.65 S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li 10 SnP2S 12 , Li 1o SiP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 、(1-x)P2S 5-x Li2S (where 0.5≤x≤0.7) and combinations thereof. In one variation, one or more sulfide-based materials may have a carbon content greater than or equal to about 10 -7 S / cm to an ionic conductivity of less than or equal to about 1 S / cm.
[0082] As an embodiment, the halide solid electrolyte may include one or more halide-based materials selected from the group consisting of Li2CdCl4, Li2MgCl4, Li2CdI4, Li2ZnI4, Li3OCl, LiI, Li5ZnI4, Li3OCl 1-x Br x (where 0<x<1) and combinations thereof. In one variation, one or more halide-based materials may have a value greater than or equal to about 10 -8 S / cm to less than or equal to about 10 -1 S / cm ionic conductivity, it can be understood that the halide solid electrolyte here is different from the halide solid electrolyte of the present application, that is, it does not include the halide solid electrolyte involved in the present application.
[0083] As an embodiment, the borate solid electrolyte may include one or more borate-based materials selected from the group consisting of: Li2B4O7, Li2O-(B2O3)-(P2O5), and combinations thereof. In one variation, the one or more borate-based materials may have a carbon content greater than or equal to about 10 -7 S / cm to less than or equal to about 10 -2 S / cm ionic conductivity.
[0084] As an embodiment, the nitride solid electrolyte may include one or more nitride-based materials selected from the group consisting of Li3N, Li7PN4, LiSi2N3, and combinations thereof. In one embodiment, the one or more nitride-based materials may have a carbon content greater than or equal to about 10 -9 S / cm to an ionic conductivity of less than or equal to about 1 S / cm.
[0085] As an embodiment, the hydride solid electrolyte may include one or more hydride-based materials selected from the group consisting of Li3AlH6, LiBH4, LiBH4-LiX (wherein X is one of Cl, Br and I), LiNH2, Li2NH, LiBH4-LiNH2, and combinations thereof. In one variation, the one or more hydride-based materials may have a carbon content greater than or equal to about 10 -7 S / cm to less than or equal to about 10 -2 S / cm ionic conductivity.
[0086] Further preferably, the mass content of the halide solid electrolyte in the solid electrolyte layer is 1-99.999 wt %.
[0087] The present application does not particularly limit the thickness of the solid electrolyte layer. The thickness of the solid electrolyte layer can be adjusted as necessary without violating the inventive concept of the present application. It can be understood that routine adjustments to the thickness of the solid electrolyte layer fall within the scope of protection of the present application.
[0088] It is known in the art that a solid electrolyte layer is arranged on the surface of the positive electrode active material layer to improve the safety of the battery. The solid electrolyte layer is different from the solid electrolyte membrane that acts as an electronic insulator between the positive electrode and the negative electrode. The main purpose of the solid electrolyte layer is to prevent the occurrence of side reactions of the positive electrode material.
[0089] As a mere illustrative example, and not a limitation on the scope of protection, the thickness of the solid electrolyte layer is 0.1-100 microns; preferably, 1-30 microns.
[0090] The present application does not have any particular limitation on the positive electrode active material and the negative electrode active material. Without violating the inventive concept of the present application, the types of known positive electrode active materials and negative electrode active materials can be used in the present application. It is only used as an illustrative example, not any limitation on the scope of protection. The negative electrode active material may include a lithium-based negative electrode active material, which includes, for example, lithium metal and / or lithium alloy. In other embodiments, the negative electrode is a silicon-based negative electrode active material, which includes silicon, such as a silicon alloy, silicon oxide, or a combination thereof, which may also be mixed with graphite in some cases. In other embodiments, the negative electrode may include a carbonaceous-based negative electrode active material, which includes one or more of graphite, graphene, carbon nanotubes (CNTs), and combinations thereof. In yet another embodiment, the negative electrode includes one or more negative electrode active materials that accept lithium, such as lithium titanium oxide (Li4Ti5O 12 ), one or more transition metals (e.g., tin (Sn)), one or more metal oxides (e.g., vanadium oxide (V2O5), tin oxide (SnO), titanium dioxide (TiO2)), titanium niobium oxide (Ti x Nb y O z , wherein 0≤x≤2, 0≤y≤24 and 0≤z≤64), a metal alloy (such as copper tin alloy (Cu6Sn5)) and one or more metal sulfides (such as iron sulfide (FeS)); the positive electrode electroactive material layer is one of a layered oxide cathode, a spinel cathode and a polyanion cathode. For example, the layered oxide cathode (e.g., a rock salt layered oxide) comprises one or more lithium-based positive electrode electroactive materials selected from the following: LiCoO2 (LCO), LiNi x Mn y Co 1-x-y O2 (where 0≤x≤1 and 0≤y≤1), LiNi 1-x-y Co x Al y O2 (where 0≤x≤1 and 0≤y≤1), LiNi x Mn 1-x O2 (where 0≤x≤1), and Li 1+x MO2 (wherein M is one of Mn, Ni, Co and Al and 0≤x≤1). The spinel cathode comprises one or more lithium-based positive electroactive materials selected from the group consisting of LiMn2O4 (LMO) and LiNi x Mn 1.5 O4. The olivine-type cathode comprises one or more lithium-based positive electrode electroactive materials LiMPO4 (wherein M is at least one of Fe, Ni, Co and Mn). The polyanion cation comprises, for example, a phosphate such as LiV2(PO4)3 and / or a silicate such as LiFeSiO4.
[0091] The positive electrode active material layer and the negative electrode active material layer may be optionally mixed with a binder: such as polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), nitrile rubber (NBR), styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-butadiene-styrene copolymer (SBS), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate or a combination thereof. At the same time, the positive electrode active material layer and the negative electrode active material layer may optionally add a conductive agent to provide a conductive path, and the conductive agent may include a carbon-based material, powdered nickel or other metal particles, or a conductive polymer. Carbon-based materials may include particles such as carbon black, graphite, acetylene black (such as KETCHENTM black or DENKATM black), carbon fibers and nanotubes, graphene, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, etc.
[0092] This embodiment also includes a lithium-ion battery, which includes a positive electrode, a negative electrode and an electrolyte, and the electrolyte contains the above-mentioned halide solid electrolyte material.
[0093] It is understandable that the electrolyte can be composed only of the above-mentioned halide solid electrolyte material, that is, the lithium-ion battery includes a positive electrode, a negative electrode, and a halide solid electrolyte, and the halide solid electrolyte is located between the positive electrode and the negative electrode to isolate the positive electrode and the negative electrode.
[0094] As an embodiment, the electrolyte may also include other electrolyte materials. It is understood that any suitable electrolyte capable of conducting lithium ions between the positive electrode and the negative electrode can be used in the battery, whether in solid, liquid, solid-liquid mixed or gel form. The present application does not particularly limit the electrolyte system of the battery. On the basis of not violating the inventive concept of the present application, lithium-ion batteries can apply known electrolyte systems; based on the understanding of the prior art knowledge in the field, the solid-liquid mixed electrolyte system is a mixture of a non-aqueous electrolyte and a solid electrolyte, while the solid electrolyte system is composed only of a solid electrolyte. It should be understood that the solid electrolyte can be composed of a solid electrolyte material, or it can be composed of two or more materials, and the two or more solid electrolyte materials can be the same type of solid electrolyte material, or they can be different types of solid electrolyte materials.
[0095] In some specific embodiments, the electrolyte may include an organic solvent and a lithium salt. The organic solvent here can use any organic solvent without particular limitation, as long as it can act as a medium through which the ions participating in the electrochemical reaction of the battery can move. Specifically, as an organic solvent, ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone can be used; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol solvents such as ethanol and isopropanol; nitrile such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group, and may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolanes; or cyclopentane sulfone. Among the above-mentioned solvents, it is preferred to use carbonate solvents, and a mixture of cyclic carbonates (such as ethylene carbonate or propylene carbonate) with high ion conductivity and high dielectric constant and low viscosity linear carbonate compounds (such as ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) that can increase the charge / discharge performance of the battery is more preferred. In this case, when the cyclic carbonate and the linear carbonate are mixed with a volume ratio of about 1: 1 to about 1: 9, the performance of the electrolyte may be excellent.
[0096] Any compound may be used as the lithium salt without particular limitation as long as it can provide lithium ions used in a lithium secondary battery. Specifically, lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrachloroaluminate (LiAlCl4), lithium iodide (Lil), lithium bromide (LiBr), lithium thiocyanate (LiSCN), lithium tetrafluoroborate (LiBF4), lithium difluorooxalatoborate (LiBF2(C2O4))(LiODFB), lithium tetraphenylborate (LiB(C6H5)4), lithium bis(oxalate)borate (LiB(C2O4)2)(LiBOB), lithium tetrafluorooxalatophosphate (LiPF4(C2O4))(LiFOP), lithium nitrate (LiNO3), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonyl imide) (LITFSI)(LiN(CF3SO2)2), lithium bis(fluorosulfonyl imide) (LiN(FSO2)2)(LIFSI) and combinations thereof. In certain variations, a lithium salt selected from lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) (LiN(CF3SO2)2), lithium bis(fluorosulfonyl imide) (LiN(FSO2)2) (LiFSI), lithium fluoroalkyl phosphonate (LiFAP), lithium phosphate (Li3PO4) and combinations thereof can be used as the lithium salt. The lithium salt can be used in a concentration range of 0.1-2.0M, such as 0.1M, 0.3M, 0.5M, 0.7M, 0.8M, 1M, 1.2M, 1.3M, 1.5M, 1.6M, 1.8M or 2.0M, etc. When the concentration of the lithium salt is within the above range, the electrolyte has suitable conductivity and viscosity, thereby exhibiting excellent performance, and lithium ions can be effectively moved.
[0097] As just one embodiment, the other electrolyte may be a non-aqueous electrolyte, and when the electrolyte is a non-aqueous electrolyte, it also includes a separator, such as a diaphragm; the non-aqueous electrolyte includes a lithium salt dissolved in an organic solvent or a mixture of organic solvents. In some variations, the separator may be formed of a microporous insulating material, in which a liquid or semi-solid electrolyte can be absorbed into the pores.
[0098] Solid electrolyte materials can be used as ion conductors to transport and conduct lithium ions and as electrical insulators to prevent charge or current from flowing from the negative electrode to the positive electrode. Therefore, the membrane composed of solid electrolyte materials can replace the separator. In addition to the halide solid electrolyte involved in this application, this application does not specifically limit other related solid electrolyte materials. Without violating the inventive concept of this application, any known solid electrolyte material can be used in this application, including but not limited to oxide solid electrolytes, sulfide solid electrolytes, halide solid electrolytes, polymer solid electrolytes, nitride solid electrolytes, and boride solid electrolytes. For details, please refer to the above description.
[0099] The present application also includes a method for preparing the above-mentioned halide solid electrolyte material, such as Figure 3 As shown, the following steps are included:
[0100] S1. The lithium salt, the zirconium salt, the salt corresponding to the element M, and the salt corresponding to the element N are placed in a mixing device in a preset stoichiometric ratio to obtain an intermediate;
[0101] S2. Sintering the obtained intermediate to obtain the halide solid electrolyte material.
[0102] The general chemical formula of the halide solid electrolyte material is Li 2+a+2b Zr 1-a-b M a N b X6;
[0103] The element M is selected from one or both of Eu and Gd; and the value range of 2+a+2b is 2.15-2.65;
[0104] The element N is different from the element M, and the ionic radius r(N) of the element N is 60 picometers<r(N)<95 picometers;
[0105] The value range of a+b is 0.1-0.5, and the value range of a / b is 1-6;
[0106] X is one or more elements selected from F, Cl, Br, and I.
[0107] In an optional embodiment, the mixing device is a ball mill; further preferably, the mixing device is a ZrO2 ball mill.
[0108] In an optional embodiment, the ball milling speed of the ball mill is 200-800 rpm, and the ball milling time is 10-50h;
[0109] In an optional embodiment, the sintering temperature of step S2 is 150-350°C;
[0110] In an optional embodiment, the sintering time of step S2 is 0-40 hours.
[0111] The present application and its effects are described in more detail with reference to the following examples.
[0112] Example 1
[0113] LiCl, ZrCl4, EuCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball milling beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 Eu 0.1 Mg 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.712 mS / cm.
[0114] Example 2
[0115] LiCl, ZrCl4, EuCl3, and CdCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball milling beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 Eu 0.1 Cd 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.705 mS / cm.
[0116] Example 3
[0117] LiCl, ZrCl4, GdCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball milling beads in a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 G 0.1 Mg 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.693 mS / cm.
[0118] Example 4
[0119] LiCl, ZrCl4, GdCl3, and CdCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball mill beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 G 0.1 Cd 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.627 mS / cm.
[0120] Example 5
[0121] LiCl, ZrCl4, EuCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.16:0.88:0.08:0.04, and ZrO2 ball milling beads in a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.16 Zr 0.88 Eu 0.08 Mg 0.04 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.650 mS / cm.
[0122] Example 6
[0123] LiCl, ZrCl4, EuCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.4:0.7:0.1:0.1, and ZrO2 ball milling beads in a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.4 Zr 0.7 Eu 0.2 Mg 0.1 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.815 mS / cm.
[0124] Example 7
[0125] LiCl, ZrCl4, EuCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.64:0.5:0.32:0.16, and ZrO2 ball milling beads of a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.64 Zr 0.52 Eu 0.32 Mg 0.16Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.638 mS / cm.
[0126] Example 8
[0127] LiCl, ZrCl4, EuCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.45:0.7:0.15:0.15, and ZrO2 ball milling beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.45 Zr 0.7 Eu 0.15 Mg 0.15 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.775 mS / cm.
[0128] Example 9
[0129] LiCl, ZrCl4, EuCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.35:0.7:0.25:0.05, and ZrO2 ball milling beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.35 Zr 0.7 Eu 0.25 Mg 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.799 mS / cm.
[0130] Example 10
[0131] LiCl, ZrCl4, EuCl3, MgCl2, and LiF were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.15:0.7:0.2:0.1:0.25, and ZrO2 ball milling beads in a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.4 Zr 0.7 Eu 0.2 Mg 0.1 Cl 5.75 F 0.25 The room temperature ionic conductivity of the obtained electrolyte was measured to be 1.001 mS / cm.
[0132] Embodiment 11
[0133] LiCl, ZrCl4, EuCl3, MgCl2, and LiF were added to a ZrO2 ball mill in a glove box at a molar ratio of 1.4:0.7:0.2:0.1:1, and ZrO2 ball mill beads of a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.4 Zr 0.7 Eu 0.2 Mg 0.1 Cl5F1. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.837 mS / cm.
[0134] Example 12
[0135] LiCl, ZrCl4, EuCl3, MgCl2, and LiF were added to a ZrO2 ball mill in a glove box at a molar ratio of 1.2:0.7:0.2:0.1:1.2, and ZrO2 ball milling beads in a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.4 Zr 0.7 Eu 0.2 Mg 0.1 Cl 4.8 F 1.2 The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.803 mS / cm.
[0136] Example 13
[0137] LiCl, ZrCl4, EuCl3, MgCl2, and Lil were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.15:0.7:0.2:0.1:0.25, and ZrO2 ball milling beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.4 Zr 0.7 Eu 0.2 Mg 0.1 Cl 5.75 I 0.25 The room temperature ionic conductivity of the obtained electrolyte was measured to be 1.110 mS / cm.
[0138] Embodiment 14
[0139] LiCl, ZrCl4, EuCl3, MgCl2, and LiBr were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.15:0.7:0.2:0.1:0.25, and ZrO2 ball milling beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li2.4 Zr 0.7 Eu 0.2 Mg 0.1 Cl 5.75 Br 0.25 The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.800 mS / cm.
[0140] Embodiment 15
[0141] LiCl, ZrCl4, EuCl3, and BaCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball milling beads in a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 Eu 0.1 Ba 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.355 mS / cm.
[0142] Comparative Example 1
[0143] LiCl and ZrCl4 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2:1, and ZrO2 ball mill beads of a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and ball milled at a speed of 560 rpm for 45 hours to obtain Li2ZrCl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.371 mS / cm.
[0144] Comparative Example 2
[0145] LiCl, ZrCl4, LaCl3, and CuCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball mill beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 La 0.1 Mg 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.463 mS / cm.
[0146] Comparative Example 3
[0147] LiCl, ZrCl4, LaCl3, and CdCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball mill beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 La 0.1 Cd 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.443 mS / cm.
[0148] Comparative Example 4
[0149] LiCl, ZrCl4, AlCl3, and MgCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball mill beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 Al 0.1 Mg 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.561 mS / cm.
[0150] Comparative Example 5
[0151] LiCl, ZrCl4, AlCl3, and CdCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball mill beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 Al 0.1 Cd 0.05 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.489 mS / cm.
[0152] Comparative Example 6
[0153] LiCl, ZrCl4, EuCl3, and CaCl2 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.2:0.85:0.1:0.05, and ZrO2 ball milling beads of the corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.2 Zr 0.85 Eu 0.1 Ca 0.05Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.609 mS / cm.
[0154] Comparative Example 7
[0155] LiCl, ZrCl4, and EuCl3 were added to a ZrO2 ball mill in a glove box at a molar ratio of 2.1:0.9:0.1, and ZrO2 ball mill beads of a corresponding proportion were added and sealed. Then, the ball mill was placed in a high-energy ball mill and milled at a speed of 560 rpm for 45 hours to obtain Li 2.1 Zr 0.9 Eu 0.1 Cl6. The room temperature ionic conductivity of the obtained electrolyte was measured to be 0.614 mS / cm.
[0156] Test method:
[0157] 1) Conductivity related tests:
[0158] Specific test method:
[0159] In the glove box, weigh 100±10 mg of the sample, then pour the sample into a solid-state battery mold with an inner diameter of 1 cm and assemble the mold. Take the mold out of the glove box, apply 3T of pressure to it, and hold it for 1 minute. Then connect the mold to the electrochemical workstation and perform an impedance test to obtain the volume impedance value of the sample. Take out the sample from the mold and press it into a tablet, and test the thickness of the tablet. According to the formula σ=I / (AR b ) to calculate the final conductivity, where σ is the conductivity in S / cm, I is the thickness of the tablet in cm, and A is the area of the tablet in cm 2 ; R b is the body impedance of the sample, in Ω). Figure 1 This is the impedance spectrum of the powder prepared in Example 10.
[0160] All impedance spectra were measured at room temperature (25°C).
[0161] Table 1 Ionic conductivity of each embodiment and comparative example
[0162] Serial number Halide composition formula Room temperature ionic conductivity mS / cm Example 1 <![CDATA[Li 2.2 Zr 0.85 I 0.1 Mg 0.05 Cl6]]> 0.712 Example 2 <![CDATA[Li 2.2 zr 0.85 I 0.1 CD 0.05 Cl6]]> 0.705 Example 3 <![CDATA[Li 2.2 Zr 0.85 GD 0.1 Mg 0.05 Cl6]]> 0.693 Example 4 <![CDATA[Li 2.2 Zr 0.85 GD 0.1 CD 0.05 Cl6]]> 0.627 Example 5 <![CDATA[Li 2.16 Zr 0.88 I 0.08 Mg 0.04 Cl6]]> 0.650 Example 6 <![CDATA[Li 2.4 zr 0.7 I 0.2 Mg 0.1 Cl6]]> 0.815 Example 7 <![CDATA[Li 2.64 Zr 0.52 I 0.32 Mg 0.16 Cl6]]> 0.638 Example 8 <![CDATA[Li 2.45 Zr 0.7 I 0.15 Mg 0.15 Cl6]]> 0.775 Example 9 <![CDATA[Li 2.35 Zr 0.7 I 0.25 Mg 0.05 Cl6]]> 0.799 Example 10 <![CDATA[Li 2.4 Zr 0.7 I 0.2 Mg 0.1 Cl 5.75 F 0.25 ]]> 1.001 Embodiment 11 <![CDATA[Li 2.4 Zr 0.7 I 0.2 Mg 0.1 Cl5F1]]> 0.837 Example 12 <![CDATA[Li 2.4 Zr 0.7 I 0.2 Mg 0.1 C1 4.8 F 1.2 ]]> 0.803 Example 13 <![CDATA[Li 2.4 Zr 0.7 I 0.2 Mg 0.1 Cl 5.75 I 0.25 ]]> 1.110 Embodiment 14 <![CDATA[Li 2.4 Zr 0.7 I 0.2 Mg 0.1 Cl 5.75 Br 0.25 ]]> 0.800 Embodiment 15 <![CDATA[Li 2.2 Zr 0.85 I 0.1 Ba 0.05 Cl6]]> 0.355 Comparative Example 1 <![CDATA[Li2ZrCl6]]> 0.371 Comparative Example 2 <![CDATA[Li 2.2 Zr 0.85 There 0.1 Mg 0.05 Cl6]]> 0.463 Comparative Example 3 <![CDATA[Li 2.2 Zr 0.85 La 0.1 Contd 0.05 Cl6]]> 0.443 Comparative Example 4 <![CDATA[Li 2.2 Zr 0.85 Al 0.1 Mg 0.05 Cl6]]> 0.561 Comparative Example 5 <h2 style=";text-align:left;direction:ltr"><![CDATA[Li <h2 style=";text-align:left;direction:ltr"> 2.2 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 0.85 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> CD<h2 style=";text-align:left;direction:ltr"> 0.05 <h2 style=";text-align:left;direction:ltr"> Cl6]]><h2 style=";text-align:left;direction:ltr"> 0.489 Comparative Example 6 <![CDATA[Li 2.2 Zr 0.85 I 0.1 Here 0.05 Cl6]]> 0.609 Comparative Example 7 <![CDATA[Li 2.1 Zr 0.9 I 0.1 Cl6]]> 0.614
[0163] Note: Ionic radius, Eu-94.7pm, Mg-72pm, Gd-93.8pm, Cd-95pm, La-103.2pm, Al-53.5pm;
[0164] By comparing the examples of the present application with the comparative examples, it can be seen that compared with the doping effect of other doping elements, the halide solid electrolyte obtained by composite doping of Eu and Gd with other elements has a better Figure 2The XRD characterization shows a significantly different structure. When measured by the θ-2θ method using Cu-Kα rays as X-rays, the halide solid electrolytes doped with Eu and Gd and other elements have diffraction peaks in the range of 25.3-26.2° and the diffraction angle 2θ value is in the range of 35.2-36.2°, while this characteristic peak does not appear in the halide solid electrolytes doped with other elements; and the detection of ionic conductivity shows that the composite doping effect of Eu and Gd is higher than that of other elements.
[0165] At the same time, by comparing Example 1, Example 5, Example 6 and Example 9, it can be found that the increase in the doping ratio of Eu and Gd elements is beneficial to improving the ionic conductivity of the halide solid electrolyte material, but the content of Eu and Gd as doping elements should not be too high. When the content of the doping element is too high and affects the content of the main element Zr, it is also detrimental to the material performance.
[0166] By comparing Example 1 and Example 15, it can be seen that the combination of ion radii that meet the corresponding conditions can further improve the performance of the halide solid electrolyte, especially when there is a certain gap between the two but the gap is not too large, the effect is more obvious.
[0167] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A solid electrolyte material, characterized in that: The solid electrolyte material comprises a halide solid electrolyte material, and the chemical formula of the halide solid electrolyte material is Li 2+a+2b Zr 1-a-b M a N b X6; Element M is selected from one or two of Eu and Gd; and the value range of 2 + a + 2b is 2.15 - 2.65; Element N is different from the said element M, and the ionic radius r(N) of the said element N is 60 picometers < r(N) < 95 picometers; The said element N is selected from one or several of Co, Cu, Zn, Mg, and Cd; The value range of a + b is 0.1 - 0.5, and the value range of a / b is 1 - 6; X is one or several elements of F, Cl, Br, and I.
2. The solid electrolyte material according to claim 1, characterized in that The value range of 2 + a + 2b is 2.2 - 2.
45.
3. The solid electrolyte material according to claim 1, characterized in that The ionic radius r(M) of the said element M and the ionic radius r(N) of the said element N satisfy 0.6 < r(N) / r(M) < 1.
05.
4. The solid electrolyte material according to claim 1, characterized in that When the halide solid electrolyte material is analyzed by XRD, when using CuKα radiation, diffraction peaks exist in the range where the value of diffraction angle 2θ is 25.3 - 26.2° and in the range where the value of diffraction angle 2θ is 35.2 - 36.2°.
5. The solid electrolyte material according to claim 1, characterized in that The said element X is a mixture of multiple elements, and the said element X contains element Cl and the molar proportion of the said element Cl in the said element X ranges from 80 - 99.99%.
6. The solid electrolyte material according to claim 5, characterized in that The molar proportion of the said element Cl in the said element X ranges from 83 - 96%.
7. The solid electrolyte material according to claim 1, characterized in that The element M is a mixture of Eu and Gd, and the chemical formula Li 2+a+2b Zr 1-a-b M a N b X6 specifically Li 2+a+2b Zr 1-a-b Eu a1 Cd a2 N b X6, a=a1+a2.
8. The solid electrolyte material according to claim 7, characterized in that 2 < a1 / a2 < 5.
9. A method for preparing a halide solid electrolyte material according to any one of claims 1 to 8, characterized in that: It includes the following steps: S1. Place lithium salt, zirconium salt, the salt corresponding to element M, and the salt corresponding to element N in a mixing device according to a preset stoichiometric ratio and mix to obtain an intermediate; S2. Sinter the intermediate obtained in step S1 to obtain the halide solid electrolyte material; The chemical formula of the halide solid electrolyte material is Li 2+a+2b Zr 1-a-b M a N b X6; Element M is selected from one or two of Eu and Gd; and the value range of 2 + a + 2b is 2.15 - 2.65; The said element N is selected from one or several of Co, Cu, Zn, Mg, and Cd; element N is different from the said element M, and the ionic radius r(N) of the said element N is 60 picometers < r(N) < 95 picometers; The value range of a + b is 0.1 - 0.5, and the value range of a / b is 1 - 6; X is one or several elements of F, Cl, Br, and I.
10. The method for preparing a halide solid electrolyte material according to claim 9, characterized in that: The value range of 2 + a + 2b is 2.2 - 2.
45.
11. The method for preparing a halide solid electrolyte material according to claim 9, characterized in that: The said mixing device is a ball milling tank.
12. The method for preparing a halide solid electrolyte material according to claim 11, characterized in that: The said mixing device is a ZrO2 ball milling tank.
13. The method for preparing a halide solid electrolyte material according to claim 11, characterized in that: The ball milling speed of the ball mill is 200-800 rpm, and the ball milling time is .
14. The method for preparing a halide solid electrolyte material according to claim 9, characterized in that: The sintering temperature of the said step S2 is 150 - 350 °C.
15. The method for preparing a halide solid electrolyte material according to claim 9, characterized in that: The sintering time of the said step S2 is 0 - 40 h.
16. An electrode, characterized in that: The said electrode contains the solid electrolyte material as described in any one of claims 1 - 8 or the halide solid electrolyte material prepared by the preparation method as described in any one of claims 9 - 15.
17. The electrode according to claim 16, characterized in that The said electrode contains an active material layer, and the said solid electrolyte material is included in the active material layer.
18. The electrode according to claim 16, characterized in that The said electrode is a positive electrode, the positive electrode includes a positive electrode active material layer, and the positive electrode active material layer contains a positive electrode solid electrolyte layer; the positive electrode solid electrolyte layer contains the said solid electrolyte material.
19. The electrode according to claim 18, characterized in that The positive electrode solid electrolyte layer only contains the halide solid electrolyte material.
20. The electrode according to claim 16, characterized in that The electrode is a negative electrode, the negative electrode includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode solid electrolyte layer; the negative electrode solid electrolyte layer includes the solid electrolyte material.
21. The electrode according to claim 20, characterized in that The negative electrode solid electrolyte layer contains only the halide solid electrolyte material.
22. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte comprises the solid electrolyte material according to any one of claims 1 to 8 or the halide solid electrolyte material prepared by the preparation method according to any one of claims 9 to 15.