A hydrogenation catalyst carrier and preparation method thereof

By constructing a multi-level pore structure in the hydrogenation catalyst carrier and using multi-level pore SAPO-34 molecular sieve, modified Y molecular sieve, amorphous silica alumina and alumina, the problem of small pore channels and simple structure in the existing technology is solved, and the problem is improved. It improves the conversion and heat transfer efficiency of macromolecular reactants and improves the overall performance of the catalyst.

CN116328852BActive Publication Date: 2024-10-15PETROCHINA CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202111588831.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-23
Publication Date
2024-10-15
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

The pore size of the existing hydrogenation catalyst carrier is small and the structure is simple, making it difficult to effectively transfer mass and heat. In particular, the conversion efficiency of macromolecular reactants and products is low.

Method used

Multi-stage porous SAPO-34 molecular sieve, modified Y molecular sieve, amorphous silica alumina and alumina are used as carriers, and a microporous-mesoporous-macroporous channel structure is constructed through a specific preparation method to improve the richness and pore volume of the reaction channel. .

Benefits of technology

It significantly improves the conversion and heat transfer efficiency of macromolecular reactants and products, alleviates carbon deposition and life problems, and improves the overall performance of the catalyst.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing a hydrogenation catalyst carrier, wherein the raw materials of the preparation method include multi-level porous SAPO-34 molecular sieve, amorphous silicon aluminum, modified Y molecular sieve and aluminum oxide, and in the preparation process, chitosan oligosaccharide and soluble starch are added in a total amount of 8 to 25wt% by weight of the aluminum source. The hydrogenation catalyst carrier synthesized by the preparation method of the present invention improves the conversion, mass transfer and heat transfer of reactants and products in a reaction containing macromolecules, and alleviates the problems of carbon deposition and life span.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a catalyst carrier and a preparation method thereof, and in particular to a hydrogenation catalyst carrier and a preparation method thereof. Background Art

[0002] As the responsibility and efforts for environmental protection gradually increase, the National Five Standard for domestic refined oil products is fully implemented. However, in the face of the increasing degree of crude oil heaviness, the increasing content of impurities such as nitrogen, sulfur and metals in crude oil, and the contradictory relationship between clean high-value-added oil products and inferior raw materials, more advanced hydrogenation technology is needed to solve. As one of the core technologies of hydrogenation, the preparation and synthesis of hydrogenation catalyst carriers has always been the focus and attention of scientific researchers.

[0003] The main function of conventional supported hydrogenation catalyst carriers is to provide suitable acidity during the catalytic reaction and to provide a rich specific surface area and pore structure for the metal active center. Al2O3 has extremely high hydrothermal stability and a large specific surface area and is often used as a carrier matrix. Molecular sieves are often used as the main acidic component and have received extensive attention in the fields of petroleum and chemical industry. However, the molecular sieves prepared by the existing methods have small pore sizes and simple structures, which are obviously not conducive to mass transfer and heat transfer of macromolecular reactants and products. In addition, the types of carrier acidic components are single, and the components are simply mechanically mixed, with poor dispersibility, making it difficult to achieve optimal performance.

[0004] CN104646073B provides a hydrogenation catalyst carrier, the molecular sieve used in this carrier is a multi-level pore composite molecular sieve of mesoporous amorphous silicon-aluminum coated microporous Beta molecular sieve, which improves the reaction catalytic activity and promotes the selective generation of intermediate distillate oil, but does not adjust the molecular sieve pores.

[0005] CN106669863B provides a method for modifying a hydrogenation catalyst carrier. During the synthesis process, water-soluble silicone oil and a soluble zirconium-containing compound are introduced into the hydrogenation-modified catalyst carrier in sequence or simultaneously, so that the modified carrier can provide more B acid centers, reduce strong acid centers, and adjust the distribution of acid centers and hydrogenation active centers so that they can coordinate with each other and improve the comprehensive performance of the catalyst. However, the diffusion rate of macromolecular reactants in the active centers is slow.

[0006] CN106140251B provides a hydrogenation catalyst carrier and a preparation method thereof. The invention adopts a β molecular sieve with high crystallinity, high silicon-aluminum ratio and good stability as the acid component of the carrier, and matches it with amorphous silicon-aluminum. The obtained carrier is made into a hydrogenation catalyst with high activity, but the molecular sieve pores are not adjusted.

[0007] WO2020119754A1 provides a method for preparing a hydrogenation catalyst carrier and its application, wherein a multi-level pore SAPO-34 molecular sieve is synthesized by adding silane as a silicon source of the SAPO-34 molecular sieve, and the carrier contains Y molecular sieve and SAPO-34 molecular sieve. The catalyst carrier prepared by this method can improve the yield of jet fuel; however, the cost of silane raw materials is too high.

[0008] CN105536855A discloses a method for preparing a hydrogenation catalyst carrier containing Y molecular sieve. This method uses Y molecular sieve, amorphous silicon aluminum and / or aluminum oxide as a carrier, and has good temperature increase sensitivity and operational flexibility; however, the carrier pore size is small and is not conducive to macromolecular reactions.

[0009] CN105709845B provides a hydrogenation catalyst carrier, the molecular sieve used in this carrier is a multi-level pore composite molecular sieve of mesoporous amorphous silicon-aluminum coated microporous Beta molecular sieve, which improves the reaction catalytic activity and promotes the selective generation of intermediate distillate oil; however, the molecular sieve pores are not adjusted, and the diffusion rate of macromolecular reactants in the active center is slow. Summary of the invention

[0010] The technical problem to be solved by the present invention is to construct multi-level pores in the microporous molecular sieve of the carrier active center to solve the mass transfer and heat transfer problems of macromolecular reactants and products.

[0011] In view of the shortcomings of the prior art, the present invention provides a method for preparing a hydrogenation catalyst carrier. The carrier is characterized in that it contains a certain proportion of multi-level channel SAPO-34 as a part of the acidic component, and the carrier includes Y molecular sieve, SAPO-34 molecular sieve, amorphous silica-alumina and alumina. The acid center of the carrier can provide relatively abundant micropore-mesopore-macroporous channels as reaction channels. The hydrogenation catalyst carrier synthesized by the preparation method of the present invention improves the conversion, mass transfer and heat transfer of reactants and products in reactions containing macromolecules, and alleviates the problems of carbon deposition and life.

[0012] To achieve the above-mentioned purpose, the present invention provides a method for preparing a hydrogenation catalyst carrier. The raw materials of the preparation method include multi-level pore SAPO-34 molecular sieve, amorphous silica-alumina, modified Y molecular sieve and alumina. During the preparation process of the multi-level pore SAPO-34 molecular sieve, chitosan oligosaccharide and soluble starch are added in a total amount of 8 to 25 wt% based on the weight of the aluminum source.

[0013] Furthermore, based on the weight of the hydrogenation catalyst carrier, the content of the modified Y molecular sieve and the multi-level pore SAPO-34 molecular sieve is 5wt% to 35wt%, wherein the mass ratio of the modified Y molecular sieve to the multi-level pore SAPO-34 molecular sieve is 1:3 to 5:1; the content of amorphous silicon aluminum is 10wt% to 45wt%, and the content of aluminum oxide is 20wt% to 85wt%.

[0014] Furthermore, the silicon oxide content of the amorphous silicon aluminum is 20-57 wt %.

[0015] Furthermore, the silicon-aluminum ratio of the modified Y molecular sieve is 8-25, and the unit cell parameter is 2.43-2.45 nm.

[0016] Furthermore, the preparation method can be carried out by the following specific steps: adding an auxiliary agent to a mixture including multi-level porous SAPO-34 molecular sieve, amorphous silica-alumina, modified Y molecular sieve, and alumina, kneading, extruding wet strips, drying and calcining the wet strips to obtain a hydrogenation catalyst carrier.

[0017] Furthermore, the preparation method can also be carried out by the following specific steps: first, the multi-level porous SAPO-34 molecular sieve and amorphous silica-alumina are mixed, and then a mixture including modified Y molecular sieve and alumina is added, and then an auxiliary agent is added, and the mixture is fully kneaded, and wet strips are extruded, and the wet strips are dried and calcined to obtain a hydrogenation catalyst carrier.

[0018] Furthermore, the mixture also includes methyl cellulose in an amount of 1-6 wt %.

[0019] Furthermore, the auxiliary agent is an acidic solution prepared from water, nitric acid and citric acid.

[0020] Furthermore, the drying temperature is 90-110° C. and the drying time is 2-8 h.

[0021] Furthermore, the calcination temperature is 400-600°C and the calcination time is 2-8h.

[0022] Furthermore, based on the weight of the aluminum source, the amount of chitosan oligosaccharide added is 7-20wt%, and the amount of soluble starch added is 1-5wt%.

[0023] Preferably, the preparation method of the multi-level pore SAPO-34 molecular sieve specifically comprises the following steps:

[0024] (1) dissolving chitosan oligosaccharide in water to obtain a chitosan oligosaccharide solution;

[0025] (2) adding an aluminum source, a silicon source and a phosphorus source to the chitosan oligosaccharide solution of step (1), mixing evenly, and stirring to obtain a mixture;

[0026] (3) adding a template to the mixture of step (2), and then adding soluble starch, and crystallizing to obtain a molecular sieve slurry containing multi-level pores;

[0027] (4) Filtering, drying and calcining the molecular sieve slurry obtained in step 3) to obtain a multi-level pore SAPO-34 molecular sieve.

[0028] Furthermore, in step (3), after adding the template, soluble starch is added under alkaline conditions.

[0029] Furthermore, the aluminum source is one or more of pseudo-boehmite, aluminum sulfate, aluminum chloride, and aluminum nitrate, preferably pseudo-boehmite.

[0030] Furthermore, the silicon source is one or more of active silicon dioxide, white carbon black, sodium silicate, ethyl orthosilicate, silica sol, water glass, and white carbon black, preferably water glass.

[0031] Furthermore, the template agent is one or more of diethylamine, triethylamine, morpholine, diisopropylamine, di-n-propylamine, diethanolamine, triethanolamine, tetraethylammonium hydroxide, and N,N-diethylethanol, preferably diethylamine.

[0032] Furthermore, the phosphorus source is phosphoric acid or metaphosphoric acid.

[0033] Furthermore, in step (1), the dissolution temperature is 10 to 100° C., preferably 30 to 70° C.; and the dissolution time is 0 to 280 min, preferably 10 to 160 min.

[0034] Furthermore, in step (3), the molar ratio of the aluminum source, phosphorus source, silicon source, template and water in the molecular sieve slurry is (0.5-2.1):(2-4.5):(0.4-2.2):(1-8):(50-190).

[0035] Furthermore, in step (3), the crystallization temperature is 40 to 400° C., preferably 50 to 280° C.; the crystallization time is 0 to 14400 min, preferably 10 to 4320 min.

[0036] Furthermore, in step (4), the drying temperature is 90-110° C., the drying time is 2-8 h, the calcination temperature is 400-600° C., and the calcination time is 2-8 h.

[0037] The invention also provides a hydrogenation catalyst carrier, which comprises a multi-level pore SAPO-34 molecular sieve, and the multi-level pore SAPO-34 molecular sieve comprises chitosan oligosaccharide and soluble starch in a total amount of 8 to 25 wt%.

[0038] The present invention has the following beneficial effects:

[0039] (1) The preparation method of the present invention increases the macro-mesoporous channel structure, thereby improving the conversion, mass transfer and heat transfer of wax oil macromolecular reactants and products in the hydrogenation reaction of wax oil containing macromolecules.

[0040] (2) The preparation method of the present invention increases the pore volume and specific surface area of ​​the carrier. DETAILED DESCRIPTION

[0041] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments that do not specify specific conditions are usually based on conventional conditions. The wt% of the present invention represents mass percentage.

[0042] Evaluation and analysis method: The specific surface area and pore volume of the samples were measured using a Quantachrome autosorb-analyzer.

[0043] Example 1

[0044] (1) Preparation of hierarchical pore SAPO-34 molecular sieve

[0045] Weigh 2.23g of chitosan oligosaccharide and add it to 50.02g of deionized water, stir it thoroughly at 50°C until it is completely dissolved for 15min; add 11.15g of pseudo-boehmite, 15.65g of phosphoric acid, and 5.86g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 9.72g of diethylamine and 70.10g of deionized water to the mixture, and then add 0.55g of water-soluble starch, stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle lined with polytetrafluoroethylene, place it in an oven at 180°C for crystallization for 4021min to obtain a crystallization solution; centrifuge the crystallization solution at a speed of 3000r / min for 30min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and roast them at 550°C for 5h to obtain a multi-level pore SAPO-34 molecular sieve S-1;

[0046] (2) Preparation of hydrogenation catalyst carrier

[0047] 25.8g of molecular sieve S-1, 31.4g of Y molecular sieve, 80.0g of alumina, 71.3g of amorphous silica-alumina and 7.8g of methyl cellulose are mixed and put into a kneader for mixing and grinding for 15 minutes. 136.5g of an acidic solution prepared by water, nitric acid and citric acid is added to the dry powder at one time. The mixture is first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2mm for three times, and finally formed into a cylindrical strip with a diameter of 2mm. The obtained wet strip is dried in an oven at 120°C for 12h, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4h to obtain the carrier Z-1.

[0048] Example 2

[0049] (1) Preparation of hierarchical pore SAPO-34 molecular sieve

[0050] Weigh 1.51g chitosan oligosaccharide and add it to 50.02g deionized water, stir it thoroughly at 50°C for 15min until it is completely dissolved; add 11.15g alumina, 15.65g phosphoric acid, and 5.86g water glass to the obtained solution, mix them evenly, and stir them for 1h; continue to add 12.72g triethylamine and 70.10g deionized water to the mixture, and then add 0.32g water-soluble starch, stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle with a polytetrafluoroethylene liner, place it in a 180°C oven for crystallization for 4021min to obtain a crystallization solution; centrifuge the crystallization solution at a speed of 3000r / min for 30min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and roast them at 550°C for 5h to obtain a multi-level pore SAPO-34 molecular sieve S-2;

[0051] (2) Preparation of hydrogenation catalyst carrier

[0052] 15.6 g of molecular sieve S-1, 35.4 g of Y molecular sieve, 75.0 g of alumina, 81.3 g of amorphous silica-alumina and 7.8 g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 15 minutes. 136.5 g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste-like substance, and then extruded through a cylindrical orifice plate with a diameter of 2 mm for three times, and finally formed into a cylindrical strip with a diameter of 2 mm. The obtained wet strip was dried in an oven at 120°C for 12 hours, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4 hours to obtain the carrier Z-2.

[0053] Example 3

[0054] (1) Preparation of hierarchical pore SAPO-34 molecular sieve

[0055] Weigh 1.31g of chitosan oligosaccharide and add it to 50.02g of deionized water, stir it thoroughly at 50°C for 15min until it is completely dissolved; add 11.15g of pseudo-boehmite, 15.65g of phosphoric acid, and 5.86g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 9.72g of diethylamine and 70.10g of deionized water to the mixture, and then add 0.31g of water-soluble starch, stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle containing a polytetrafluoroethylene liner, place it in a 180°C oven for crystallization for 5021min to obtain a crystallization solution; centrifuge the crystallization solution at a speed of 3000r / min for 30min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and roast them at 550°C for 5h to obtain a multi-level pore SAPO-34 molecular sieve S-3;

[0056] (2) Preparation of hydrogenation catalyst carrier

[0057] 10.6 g of molecular sieve S-1, 39.3 g of Y molecular sieve, 75.0 g of alumina, 90.1 g of amorphous silica-alumina and 7.8 g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 15 minutes. 136.5 g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2 mm for three times, and finally formed into a cylindrical strip with a diameter of 2 mm. The obtained wet strip was dried in an oven at 120°C for 12 hours, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4 hours to obtain the carrier Z-3.

[0058] Comparative Example 1

[0059] (1) Preparation of SAPO-34 molecular sieve

[0060] Weigh 0.00g of chitosan oligosaccharide and add it to 50.02g of deionized water, and stir it thoroughly at 50°C; add 11.15g of pseudo-boehmite, 15.65g of phosphoric acid, and 5.86g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 9.72g of diethylamine and 70.10g of deionized water to the mixture, and then add 0.00g of water-soluble starch, and stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle containing a polytetrafluoroethylene liner, place it in a 180°C oven for crystallization for 4021min to obtain a crystallization solution; centrifuge the crystallization solution at a speed of 3000r / min for 30min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and roast them at 550°C for 5h to obtain SAPO-34 molecular sieve S-4;

[0061] (2) Preparation of hydrogenation catalyst carrier

[0062] 25.8g of molecular sieve S-4, 31.4g of Y molecular sieve, 80.0g of alumina, 71.3g of amorphous silica-alumina and 7.8g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 15 minutes. 136.5g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2mm for three times, and finally formed into a cylindrical strip with a diameter of 2mm. The obtained wet strip was dried in an oven at 120°C for 12h, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4h to obtain the carrier Z-4.

[0063] Comparative Example 2

[0064] 15.6 g of molecular sieve S-4, 35.4 g of Y molecular sieve, 75.0 g of alumina, 81.3 g of amorphous silica-alumina and 7.8 g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 15 minutes. 136.5 g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste-like substance, and then extruded through a cylindrical orifice plate with a diameter of 2 mm for three times, and finally formed into a cylindrical strip with a diameter of 2 mm. The obtained wet strip was dried in an oven at 120°C for 12 hours, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4 hours to obtain a carrier Z-5.

[0065] Comparative Example 3

[0066] 10.6 g of molecular sieve S-4, 39.3 g of Y molecular sieve, 75.0 g of alumina, 90.1 g of amorphous silica-alumina and 7.8 g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 15 minutes. 136.3 g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste-like substance, and then extruded through a cylindrical orifice plate with a diameter of 2 mm for three times, and finally formed into a cylindrical strip with a diameter of 2 mm. The obtained wet strip was dried in an oven at 120°C for 12 hours, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4 hours to obtain a carrier Z-6.

[0067] Comparative Example 4:

[0068] (1) Weigh 0.00 g of chitosan oligosaccharide and add it to 50.02 g of deionized water, and stir thoroughly at 50 °C;

[0069] (2) Add 11.15 g of pseudo-boehmite, 15.65 g of phosphoric acid, and 5.86 g of silica sol to the solution obtained in step (1), mix well, and stir for 1 hour;

[0070] (3) adding 9.72 g of diethylamine and 70.10 g of deionized water to the solution obtained in step (2), and then adding 0.55 g of water-soluble starch, and stirring thoroughly to obtain a uniform mixture;

[0071] (4) transferring the mixture obtained in step (3) into a stainless steel kettle lined with polytetrafluoroethylene, and placing it in an oven at 180° C. for crystallization for 4021 min to obtain a crystallized solution;

[0072] (5) Centrifuge the crystallization solution of step (4) at a rotation speed of 3000 r / min for 30 min, wash the crystals until the pH is less than 8, dry the crystals at 110° C., and then place the crystals in a muffle furnace and calcine at 550° C. for 5 h to obtain SAPO-34 molecular sieve S-5.

[0073] Comparative Example 5:

[0074] (1) Weigh 0.53 g of chitosan oligosaccharide and add it to 50.02 g of deionized water, and stir thoroughly at 50 °C;

[0075] (2) Add 11.15 g of pseudo-boehmite, 15.65 g of phosphoric acid, and 5.86 g of silica sol to the solution obtained in step (1), mix well, and stir for 1 hour;

[0076] (3) adding 9.72 g of diethylamine and 70.10 g of deionized water to the solution obtained in step (2), and then adding 0.33 g of water-soluble starch, and stirring thoroughly to obtain a uniform mixture;

[0077] (4) transferring the mixture obtained in step (3) into a stainless steel kettle lined with polytetrafluoroethylene, and placing it in an oven at 180° C. for crystallization for 4021 min to obtain a crystallized solution;

[0078] (5) Centrifuge the crystallization solution of step (4) at a rotation speed of 3000 r / min for 30 min, wash the crystals until the pH is less than 8, dry the crystals at 110° C., and then place the crystals in a muffle furnace and calcine at 550° C. for 5 h to obtain SAPO-34 molecular sieve S-6.

[0079] Comparative Example 6:

[0080] (1) Weigh 3.38 g of chitosan oligosaccharide and add it to 50.02 g of deionized water, and stir thoroughly at 50 °C;

[0081] (2) Add 11.15 g of pseudo-boehmite, 15.65 g of phosphoric acid, and 5.86 g of silica sol to the solution obtained in step (1), mix well, and stir for 1 hour;

[0082] (3) adding 9.72 g of diethylamine and 70.10 g of deionized water to the solution obtained in step (2), and then adding 0.55 g of water-soluble starch, and stirring thoroughly to obtain a uniform mixture;

[0083] (4) transferring the mixture obtained in step (3) into a stainless steel kettle lined with polytetrafluoroethylene, and placing it in an oven at 180° C. for crystallization for 4021 min to obtain a crystallized solution;

[0084] (5) Centrifuge the crystallization solution of step (4) at a rotation speed of 3000 r / min for 30 min, wash the crystals until the pH is less than 8, dry the crystals at 110° C., and then place the crystals in a muffle furnace and calcine at 550° C. for 5 h to obtain SAPO-34 molecular sieve S-7.

[0085] The molecular sieves and carriers obtained in the examples and comparative examples were evaluated and analyzed, and the results are shown in Tables 1 and 2.

[0086] Table 1 Molecular sieve properties

[0087] project S-1 S-2 S-3 S-4 S-5 S-6 S-7 <![CDATA[Specific surface area m 2 / g]]> 459.6 447.3 435.7 249.2 225.3 243.8 299.8 <![CDATA[Micropore volume cm 3 / g]]> 0.212 0.240 0.225 0.115 0.123 0.152 0.147 <![CDATA[Intermediate - macropore volume cm 3 / g]]> 0.225 0.243 0.213 0.006 0.022 0.095 0.136

[0088] Table 2 Carrier properties

[0089] project Z-1 Z-2 Z-3 Z-4 Z-5 Z-6 <![CDATA[Specific surface area, m 2 / g]]> 423 453 482 415 421 451 <![CDATA[Pore volume, cm 3 / g]]> 0.76 0.72 0.71 0.72 0.68 0.69 SAPO-34 molecular sieve, wt% 12.4 7.5 5.1 12.4 7.5 5.1 Y molecular sieve, wt% 15.1 17.0 18.8 15.1 17.0 18.8 Amorphous silicon aluminum, wt% 34.2 39.1 43.6 34.2 39.1 43.6 Alumina, wt% margin margin margin margin margin margin

[0090] It can be seen from the results in Table 1 that the properties of the multi-level pore SAPO-34 molecular sieve synthesized by the preparation method of the present invention are doubled in specific surface area and pore volume compared with the SAPO-34 molecular sieve of the comparative example. At the same time, the multi-level pore SAPO-34 molecular sieve of the present invention has a pore volume greater than 0.2 cm 3 Table 2 shows the properties of the hydrogenation catalyst carrier synthesized from the multi-level pore SAPO-34 molecular sieve. The specific surface area and pore volume of the hydrogenation catalyst carrier synthesized by the preparation method of the present invention are higher than those of the comparative example.

[0091] The above embodiments are typical examples listed to illustrate the technical solutions of the present invention in detail. The present invention is subject to the protection scope of the claims and the content of the invention and is not limited by the implementation scheme. Simple replacement or modification of the present invention is still within the protection scope of the present invention.

Claims

1. A method for preparing a hydrogenation catalyst carrier, wherein the raw materials of the preparation method include multi-level pore SAPO-34 molecular sieve, amorphous silica-alumina, modified Y molecular sieve and alumina, characterized in that: The preparation method of the multi-level pore SAPO-34 molecular sieve specifically comprises the following steps: (1) dissolving chitosan oligosaccharide in water to obtain a chitosan oligosaccharide solution; (2) adding an aluminum source, a silicon source and a phosphorus source to the chitosan oligosaccharide solution of step (1), mixing evenly, and stirring to obtain a mixture; (3) adding a template to the mixture of step (2), and then adding soluble starch, and crystallizing to obtain a molecular sieve slurry containing multi-level pores; (4) filtering, drying, and calcining the molecular sieve slurry obtained in step (3) to obtain a multi-level pore SAPO-34 molecular sieve; During the preparation of the multi-level pore SAPO-34 molecular sieve, chitosan oligosaccharide and soluble starch are added in a total amount of 8 to 25 wt % based on the weight of the aluminum source.

2. The preparation method according to claim 1, characterized in that: Based on the weight of the hydrogenation catalyst carrier, the content of the modified Y molecular sieve and the multi-level pore SAPO-34 molecular sieve is 5wt% to 35wt%, wherein the mass ratio of the modified Y molecular sieve to the multi-level pore SAPO-34 molecular sieve is 1:3 to 5:1; the content of amorphous silicon aluminum is 10wt% to 45wt%, and the content of aluminum oxide is 20wt% to 85wt%.

3. The preparation method according to claim 1, characterized in that: The silicon oxide content in the amorphous silicon aluminum is 20-57wt%; the silicon aluminum ratio of the modified Y molecular sieve is 8-25, and the unit cell parameter is 2.43-2.45nm.

4. The preparation method according to claim 1, characterized in that: The added amount of the chitosan oligosaccharide is 7-20 wt %, and the added amount of the soluble starch is 1-5 wt %.

5. The preparation method according to claim 1, characterized in that: In step (3), after adding the template, soluble starch is added under alkaline conditions.

6. The preparation method according to claim 1, characterized in that: The aluminum source is one or more of pseudo-boehmite, aluminum sulfate, aluminum chloride, and aluminum nitrate; the silicon source is one or more of active silicon dioxide, white carbon black, sodium silicate, tetraethyl orthosilicate, silica sol, water glass, and white carbon black; the template is one or more of diethylamine, triethylamine, morpholine, diisopropylamine, di-n-propylamine, diethanolamine, triethanolamine, tetraethylammonium hydroxide, and N,N-diethylethanolamine; and the phosphorus source is phosphoric acid or metaphosphoric acid.

7. The preparation method according to claim 6, characterized in that: The aluminum source is pseudo-boehmite.

8. The preparation method according to claim 6, characterized in that: The silicon source is water glass.

9. The preparation method according to claim 6, characterized in that: The template agent is diethylamine.

10. The preparation method according to claim 1, characterized in that: In step (3), the molar ratio of aluminum source, phosphorus source, silicon source, template and water in the molecular sieve slurry is (0.5-2.1):(2-4.5):(0.4-2.2):(1-8):(50-190); the crystallization temperature is 40-400°C; the crystallization time is 0-14400 min, and is not 0.

11. The preparation method according to claim 10, characterized in that: In step (3), the crystallization temperature is 50 to 280° C. and the crystallization time is 10 to 4320 min.

12. A hydrogenation catalyst carrier obtained by the preparation method according to any one of claims 1 to 11, characterized in that: The hydrogenation catalyst carrier comprises a multi-level porous SAPO-34 molecular sieve. During the preparation process of the multi-level porous SAPO-34 molecular sieve, a total amount of 8 to 25 wt% of chitosan oligosaccharide and soluble starch is added based on the weight of the aluminum source.

Citation Information

Patent Citations

  • A hydrogenation catalyst support

    CN104646073B

  • Preparation method of hydrocracking catalyst containing Y molecular sieve

    CN105536855A

  • Hydrocracking catalyst carrier and preparation method thereof

    CN105709845B

  • Hydrocracking catalyst carrier and preparation method thereof