A preparation method of multi-spectral suppression ceramic material
Through the optimization of calcining temperature and ion doping of samarium chromate ceramic materials, the problem of difficult preparation of visible-near-infrared-laser multispectral compatible materials in the prior art is solved, and compatibility of low reflectivity and green peak effect at 1064nm is achieved Absorption, simplifies the process and is suitable for large-scale production.
Patent Information
- Application Number
- CN202310379561.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-12
- Filing Date
- 2023-04-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-11
AI Technical Summary
It is difficult to develop ceramic materials that are visible-near-infrared-laser multispectral compatible, especially materials that have a low reflectivity at 1064nm and have little impact on the visible light band, and the preparation process is complex and difficult to produce on a large scale.
Using samarium chromate ceramic material as the basis, the ratio optimization is performed by calcining temperature and ion doping method to prepare a multi-spectral suppression ceramic material with adjustable spectral performance, achieving low reflectivity and green peak effect at 1064nm. Compatible with absorption.
The compatible absorption of visible-near-infrared-laser is achieved, the process flow is simplified, suitable for large-scale production, and the absorption effect is further optimized through sintering temperature and ion doping.
Smart Images

Figure CN116332632B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a multi-spectrum suppression ceramic material, belonging to the technical field of functional ceramic materials. Background Art
[0002] With the continuous development of modern spectral detection technology, higher requirements are placed on spectral protection materials. Traditional single-band protection methods can hardly meet the actual needs, and gradually begin to turn to the direction of multi-band compatible protection. At present, a lot of research has been done on spectral compatible materials for radar and infrared, infrared and laser, infrared and visible light at home and abroad, and these materials have played a good role in spectral compatibility. However, there are fewer studies on the compatibility of visible light-near infrared-laser, and a big reason is that they have different requirements for reflectivity. Usually, the near-infrared band overlaps with the 1064nm laser band. Laser suppression requires the material to have a lower reflectivity here, while near-infrared compatibility requires a higher plain. In other words, the prepared material has a lower reflectivity only at 1064nm to achieve the effect of "spectral digging".
[0003] Therefore, it is necessary to study an integrated material that can produce a narrow low reflectivity band near the laser operating band while having little effect on the visible light band.
[0004] Depending on the type of material, spectrally compatible materials are usually classified into photonic crystals, metamaterials, and ceramic materials. Photonic crystals achieve spectral compatibility mainly through the two major characteristics of photon bandgap and photon localization. One-dimensional photonic crystals (Procedia Engineering, 15 (2011) 1668-1672) and photonic crystal films (Laser & Optoelectronocs progress, 56 (2019) 214-219) prepared by researchers can achieve the effect of compatible absorption. However, photonic crystals have poor stability and are difficult to apply in practice. Metamaterials achieve the effect of compatible absorption of different bands by reasonably designing the size and performance of artificial "atoms". Some researchers have used metamaterials to prepare Ti-SiO2 cubic absorbers (Optics Express, 26 (2018) 5696) and Hehmloltz resonant cavity arrays (Optics Express, 26 (2018) 5696) to achieve multi-band absorption. However, the preparation process of metamaterials is complicated and it is difficult to use them on a large scale. Ceramic materials use their own characteristics and the conversion effect of rare earth ions to achieve spectral compatibility. Among them, chrome green (Materials, 13 (2020) 1540) and cobalt green materials (Ceramics International, 42 (2016) 8198-8205) are often used in the study of spectral characteristics.
[0005] Samarium chromate ceramic materials, as a multiferroic material with an orthogonal structure, have been widely used in many fields such as electricity, magnetism and optics (Journal of Alloys and Compounds, 792 (2019) 1122-1131). It also has great development prospects in practical applications such as electrodes and sensors (CN 108387628A). As a green spectral characteristic ceramic material, samarium chromate also has the upconversion effect of rare earth ions, so it is expected to be used for laser compatible absorption. However, there are few reports on the use of samarium chromate materials for visible light-near infrared-laser compatible suppression, and there is also an urgent need for preparation process optimization technology for its multi-spectral compatible characteristics. Summary of the invention
[0006] The purpose of the present invention is to meet the needs of visible light-near infrared-laser multi-spectral compatibility characteristics, propose a preparation method of a multi-spectral suppression ceramic material, prepare a samarium chromate spectrum suppression ceramic material with adjustable spectral performance, and use it as a template, combine the calcination temperature and ion doping means, optimize its ratio, and finally achieve visible light-near infrared-laser compatible absorption. The material has a lower reflectivity at 1064nm and has the effect of green peak, and has very good practical value. In addition, the present invention has a short operation time, a simple process, and can achieve large-scale batch production.
[0007] The technical solution of the present invention is: a method for preparing a multi-spectral suppression ceramic material, and the specific steps thereof are: (1) pretreatment of samarium chromate material: adding samarium oxide and chromium oxide powder as a matrix material according to a set molar mass ratio, and then adding a metal oxide as an additive material, and grinding the powder sufficiently to make the color uniform; (2) primary calcination treatment: calcining the pretreated samarium chromate powder at a high temperature, and naturally cooling the powder to obtain a samarium chromate crystal phase;
[0008] (3) Secondary grinding and calcination: The powder containing the samarium chromate crystal phase is ground to form a dense ceramic sheet, which is then subjected to secondary calcination and naturally cooled to obtain a multi-spectrum suppression ceramic material.
[0009] Preferably, the molar mass ratio of samarium oxide to chromium oxide in step (1) is 0.8-1.2:1.
[0010] Preferably, the metal oxide in step (1) is one or both of cobalt oxide and iron oxide; and the molar mass ratio of the metal oxide to chromium oxide is 0.005-0.04:1.
[0011] Preferably, the calcination temperature T1 of the high-temperature calcination in step (2) is 1200-1400° C., the holding time is 4-6 hours, and the heating rate is 4-7° C. / min.
[0012] Preferably, the secondary calcination in step (3) is as follows: first, the temperature is raised to a calcination temperature T1 of 1200-1400°C at a heating rate of 4-7°C / min and kept at that temperature for 1-2h; then, the temperature is raised from the calcination temperature T1 to a secondary calcination temperature T2 of 1300-1500°C at a heating rate of 2-4°C / min and kept at that temperature for 4-6h.
[0013] Beneficial effects:
[0014] Compared with the prior art, the present invention verifies the value of samarium chromate ceramic materials in the field of spectral compatibility, making them useful for the compatible absorption of visible light, near infrared light and laser light, and also provides a theoretical basis for subsequent ratio optimization. On the other hand, the present invention further optimizes its ratio by controlling the sintering temperature and ion doping, thereby obtaining the best absorption effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 A flow chart was prepared for Comparative Example 1.
[0016] Figure 2 This is the spectrum curve of samarium chromate prepared at 1400°C in Comparative Example 1.
[0017] Figure 3 This is a photo of the object of Comparative Example 1 before secondary calcination.
[0018] Figure 4 This is a photo of the comparative example 1 after secondary calcination.
[0019] Figure 5 This is the spectrum curve of 2% cobalt oxide doped with samarium chromate in Example 3.
[0020] Figure 6 This is a spectrum curve of 4% cobalt oxide doped samarium chromate in Example 4.
[0021] Figure 7 This is the spectrum curve of 2% iron oxide doped with samarium chromate in Example 6.
[0022] Figure 8 This is a spectrum curve of samarium chromate co-doped with cobalt oxide and iron oxide in Example 7. DETAILED DESCRIPTION
[0023] The present invention will be further described with reference to the embodiments:
[0024] The preparation flow chart of the following Examples 1-7 is as follows Figure 1 shown.
[0025] Comparative Example 1:
[0026] (1) Grind 1.7436 g (0.005 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly until the color is uniform.
[0027] (2) The sample in step 1 was calcined once at a calcination temperature of 1300°C, a holding time of 5 h, and a heating rate of 5°C / min.
[0028] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0029] (4) The sample in step 3 was subjected to secondary calcination by heating the temperature to 1300°C at a heating rate of 5°C / min and keeping the temperature for 1 h, and then heating the temperature to 1400°C at a heating rate of 3°C / min and keeping the temperature for 5 h.
[0030] Figure 2 The spectrum curve of samarium chromate at 1400°C of Comparative Example 1 shows that, without adding metal oxide, samarium chromate will produce a green peak, which has a certain absorption effect on the reflectivity at 1064nm, and the reflectivity can reach 44.93%. This shows that samarium chromate ceramic materials can be used for compatible absorption of visible light, near infrared light and laser.
[0031] Embodiment 1:
[0032] (1) Grind 1.7436 g (0.005 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly until the color is uniform, and then add 0.00829 g (0.00005 mol) of cobalt oxide and grind again.
[0033] (2) The sample in step 1 was calcined once at a calcination temperature of 1300°C, a holding time of 5 h, and a heating rate of 5°C / min.
[0034] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0035] (4) The sample in step 3 was subjected to secondary calcination, with the temperature increased to 1300°C at a heating rate of 5°C / min, kept at that temperature for 1 hour, and then increased to 1400°C at a heating rate of 3°C / min, kept at that temperature for 5 hours. The photos of the actual objects before and after the secondary calcination are as follows: Figure 3 and Figure 4 As shown in the figure, it can be seen that after the second calcination, the color of the sample changes from dark green to light green, which is conducive to laser absorption.
[0036] The addition of metal oxide (cobalt oxide) can produce a certain gain effect on the absorption of laser light, while ensuring the green peak, the reflectivity at 1064nm is reduced from 44.93% to 43.82%.
[0037] Embodiment 2:
[0038] (1) Grind 2.0225 g (0.0058 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly, then add 0.00829 g (0.00005 mol) of cobalt oxide and grind until the color is uniform.
[0039] (2) The sample in step 1 was calcined once at a calcination temperature of 1300°C, a holding time of 5 h, and a heating rate of 5°C / min.
[0040] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0041] (4) The sample in step 3 was subjected to secondary calcination by heating the temperature to 1300°C at a heating rate of 5°C / min and keeping the temperature for 1 h, and then heating the temperature to 1400°C at a heating rate of 3°C / min and keeping the temperature for 4 h.
[0042] By optimizing the molar ratio of the matrix material, a certain gain effect can be produced on the absorption of the laser, and while ensuring the green peak, the reflectivity at 1064nm is reduced from 44.93% to 44.17%.
[0043] Embodiment 3:
[0044] (1) Grind 2.0225 g (0.0058 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly, then add 0.001658 g (0.0001 mol) of cobalt oxide and grind until the color is uniform.
[0045] (2) The sample in step 1 was calcined once at a calcination temperature of 1250°C, a holding time of 6 h, and a heating rate of 4°C / min.
[0046] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0047] (4) The sample in step 3 was subjected to secondary calcination by heating the temperature to 1250°C at a heating rate of 4°C / min and keeping the temperature for 1 h, and then heating the temperature to 1350°C at a heating rate of 2°C / min and keeping the temperature for 6 h.
[0048] Figure 5 The spectrum curve of 2% cobalt oxide doped samarium chromate shows that 2% cobalt oxide doping can form a flatter near-infrared plateau compared with undoped metal oxides, and the green peak has no obvious position change, and the reflectivity at 1064nm has also decreased. The reduction in the heating rate makes the structure denser, which is conducive to the reduction of reflectivity and optimizes the compatible absorption effect of visible light-near infrared-laser.
[0049] Embodiment 4:
[0050] (1) Grind 1.4646 g (0.0042 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly, then add 0.003316 g (0.0002 mol) of cobalt oxide and grind until the color is uniform.
[0051] (2) The sample in step 1 was calcined once at a calcination temperature of 1350°C, a holding time of 4 h, and a heating rate of 7°C / min.
[0052] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0053] (4) The sample in step 3 was subjected to secondary calcination by heating the temperature to 1350°C at a heating rate of 7°C / min and keeping the temperature for 2 h, and then heating the temperature to 1450°C at a heating rate of 4°C / min and keeping the temperature for 4 h.
[0054] Figure 6 This is a spectrum curve of 4% cobalt oxide doped samarium chromate. It can be seen that the doping of 4% cobalt oxide greatly reduces the reflectivity at 1064nm, which has a good effect on laser absorption.
[0055] Embodiment 5:
[0056] (1) Grind 2.0225 g (0.0058 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly, then add 0.007975 g (0.00005 mol) of iron oxide and grind until the color is uniform.
[0057] (2) The sample in step 1 was calcined once at a calcination temperature of 1350°C, a holding time of 5 h, and a heating rate of 6°C / min.
[0058] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0059] (4) The sample in step 3 was subjected to secondary calcination by heating the temperature to 1350°C at a heating rate of 6°C / min and keeping the temperature for 1 h, and then heating the temperature to 1450°C at a heating rate of 3°C / min and keeping the temperature for 5 h.
[0060] Example 5 shows that the addition of metal oxide (iron oxide) can produce a certain gain effect on the absorption of laser light, while ensuring the green peak, the reflectivity at 1064 nm is reduced from 44.93% to 43.71%.
[0061] Embodiment 6:
[0062] (1) Grind 2.0225 g (0.0058 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly, then add 0.001595 g (0.0001 mol) of iron oxide and grind until the color is uniform.
[0063] (2) The sample in step 1 was calcined once at a calcination temperature of 1300°C, a holding time of 5 h, and a heating rate of 4°C / min.
[0064] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0065] (4) The sample in step 3 was subjected to secondary calcination by heating the temperature to 1300°C at a heating rate of 4°C / min and keeping the temperature for 2 h, and then heating the temperature to 1400°C at a heating rate of 3°C / min and keeping the temperature for 5 h.
[0066] Figure 7 The spectrum curve of 2% iron oxide doped samarium chromate shows that compared with the undoped metal oxide, the 2% iron oxide doping reduces the reflectivity at 1064nm while ensuring the green peak. In addition, the increase in the molar ratio of the matrix material is also conducive to the absorption of lasers, optimizing the compatible absorption effect of visible light, near infrared and lasers.
[0067] Embodiment 7:
[0068] (1) Grind 2.0225 g (0.0058 mol) of samarium oxide and 0.75995 g (0.005 mol) of chromium oxide thoroughly, then add 0.00829 g (0.00005 mol) of cobalt oxide and 0.001595 g (0.0001 mol) of iron oxide and grind until the color is uniform.
[0069] (2) The sample in step 1 was calcined once at a calcination temperature of 1300°C, a holding time of 5 h, and a heating rate of 4°C / min.
[0070] (3) Grind the sample in step 2 again to make a dense ceramic sheet.
[0071] (4) The sample in step 3 was subjected to secondary calcination by heating the temperature to 1300°C at a heating rate of 4°C / min and keeping the temperature for 1 h, and then heating the temperature to 1400°C at a heating rate of 2°C / min and keeping the temperature for 5 h.
[0072] Figure 8 This is the spectrum curve of samarium chromate doped with 1% cobalt oxide and 2% iron oxide. It can be seen that the dual-ion co-doping can not only ensure the platform, but also achieve compatible absorption of visible light, near-infrared and laser, reducing the reflectivity at 1064nm to 41.56%.
Claims
1. A method for preparing a multi-spectral suppression ceramic material, the specific steps of which are: (1) Pretreatment of samarium chromate material: according to the set molar mass ratio, samarium oxide and chromium oxide powder are added as the base material, and then metal oxide is added as the additive material, and after sufficient grinding, the color is uniform; the metal oxide is one or both of cobalt oxide and iron oxide; the molar ratio of metal oxide to chromium oxide is 0.005-0.04:1; (2) primary calcination treatment: the pretreated samarium chromate powder is subjected to high temperature calcination and naturally cooled to obtain a samarium chromate crystal phase; wherein the high temperature calcination temperature T1 is 1200-1400°C and the holding time is 4-6h; (3) Secondary grinding and calcination: The powder containing the samarium chromate crystal phase is ground to form a green dense ceramic sheet, which is then subjected to secondary calcination and naturally cooled to obtain a dense green multi-spectrum suppression ceramic material; the secondary calcination is as follows: first, the calcination temperature T1 is raised to 1200-1400°C and kept warm for 1-2 hours; then, the calcination temperature T1 is raised to the secondary calcination temperature T2 of 1300-1500°C and kept warm for 4-6 hours.
2. The preparation method according to claim 1, characterized in that: In the step (1), the molar ratio of samarium oxide to chromium oxide is 0.8-1.2:
1.
3. The preparation method according to claim 1, characterized in that: The heating rate in step (2) is 4-7°C / min.
4. The preparation method according to claim 1, characterized in that: The secondary calcination in step (3) is as follows: firstly, the temperature is raised to the calcination temperature T1 at a heating rate of 4-7°C / min; and then, the temperature is raised from the calcination temperature T1 to the secondary calcination temperature T2 at a heating rate of 2-4°C / min.
Citation Information
Patent Citations
Mixed-potential type triethylamine sensor adopting SmMO3 as sensitive electrode material and preparation method of mixed-potential triethylamine sensor
CN108387628A
Rare earth ReCrO3 magnetic wave-absorbing material and preparation method thereof
CN104402417A
Perovskite structure nano ceramic material and preparation method thereof
CN111548160A
Visible light / laser / infrared / radar compatible stealth material and preparation method thereof
CN114716148A
Ceramic composite material for optical conversion and use thereof