A method and device for preparing polyaluminium chloride using aluminium ash

During the process of preparing polymer aluminum chloride in aluminum ash, secondary aluminum ash is mixed with activated carbon and added hydrochloric acid in batches, combined with microelectrolysis and exhaust gas treatment, the heavy metal removal and safety problems are solved, and high efficiency and low cost are achieved Production of polyaluminum chloride.

CN116354377BActive Publication Date: 2024-11-08JIAOZUO AIERFUKE CHEM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310349481.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-11-08
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

In the prior art, when using aluminum ash to prepare polymer aluminum chloride, heavy metal removal is difficult, high treatment cost, and there is a risk of explosion and the risk of violent reactions, which cannot meet the qualified standards of water purifiers.

Method used

By mixing the secondary aluminum ash with activated carbon and adding hydrochloric acid in batches, microelectrolytic purification is carried out, and metal aluminum of the aluminum ash itself is used to reduce the addition of aluminum chips. Batch addition and crushing are used, combined with fixed bed absorption tower and spray drying The tower processes exhaust gas, achieving heavy metal removal and safe treatment of exhaust gas.

Benefits of technology

The heavy metal content produced by polymer aluminum chloride is reduced, the reaction time and raw material cost is saved, the treatment strength is reduced, the safety and production efficiency of the product are improved, and the preparation of qualified polymer aluminum chloride is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116354377B_ABST
    Figure CN116354377B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing polyaluminium chloride using aluminium ash, comprising the following steps: 1) mixing secondary aluminium ash with activated carbon, and obtaining a mixed raw material after ball milling; 2) adding hydrochloric acid to a reactor, and then adding the mixed raw material in batches to react, adjusting the basicity of the reactants, obtaining a polyaluminium chloride solution after filtration, and obtaining polyaluminium chloride after drying. The method of the present invention can reduce heavy metal ions in the polyaluminium chloride solution by micro-electrolysis, and adsorb them on the surface of coke particles, and remove them by filtration, so as to achieve the purpose of purifying heavy metals in the polyaluminium chloride solution, thereby realizing the preparation of qualified polyaluminium chloride by using aluminium ash.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method and a device for preparing polyaluminium chloride by using aluminium ash, belonging to the technical field of aluminium ash treatment. Background Art

[0002] In the electrolytic aluminum, aluminum processing and other industries, a large amount of aluminum ash is produced. Aluminum ash is a hazardous solid waste and is difficult to handle. Aluminum ash is divided into primary aluminum ash and secondary aluminum ash. The content of elemental aluminum in primary aluminum ash is as high as 70-80%. The residue after the primary aluminum ash is recovered from the metal aluminum is called secondary aluminum ash. After aluminum extraction, the secondary aluminum ash still contains about 10-20% elemental aluminum, 15-50% aluminum nitride, 20-40% aluminum oxide, and some fluoride salts.

[0003] Aluminum ash has a high aluminum content, and recycling aluminum ash to prepare polyaluminum chloride can generate greater economic value. The technical difficulty is that aluminum ash contains a lot of heavy metal elements, which are difficult to remove. The heavy metals in the polyaluminum chloride used for preparation are likely to exceed the standard and cannot meet the qualified standards of water purifiers.

[0004] In the prior art, a measure of using a chelating agent to purify heavy metal ions in an acid-dissolved polyaluminium chloride solution is disclosed, but the treatment cost is relatively high.

[0005] Patent CN1114563C discloses a method for purifying polyaluminium chloride by using aluminium-carbon micro-electrolysis, which has a low processing cost. This scheme adds a purification process, and the micro-electrolysis reaction time is generally 1 to 2 hours, which reduces the production efficiency of polyaluminium chloride. In addition, this method requires the addition of aluminium chips.

[0006] In addition, when using aluminum ash to prepare polyaluminium chloride, the handling of the aluminum ash is very dangerous. When aluminum ash is ball-milled, aluminum dust will be produced, posing a risk of explosion. During acid dissolution, the elemental aluminum in the aluminum ash reacts violently with hydrochloric acid to produce a large amount of hydrogen, which accumulates in the reactor and is very dangerous. The hydrolysis of aluminum nitride will produce a large amount of irritating ammonia. Summary of the invention

[0007] In view of the above problems, the present invention provides a method and device for preparing polyaluminium chloride using aluminium ash, and the specific scheme is as follows:

[0008] A method for preparing polyaluminium chloride using aluminium ash comprises the following steps:

[0009] 1) Mixing the secondary aluminum ash and activated carbon, and ball milling to obtain a mixed raw material;

[0010] 2) Add hydrochloric acid to the reaction kettle, and then add the mixed raw materials in batches to react, adjust the basicity of the reactants, filter to obtain a polyaluminium chloride solution, and dry to obtain polyaluminium chloride.

[0011] Furthermore, in step 2), the interval time for adding the mixed raw materials in batches is 30 minutes.

[0012] An improved method for preparing polyaluminium chloride using aluminium ash comprises the following steps: firstly crushing secondary aluminium ash to obtain aluminium ash particles, mixing the aluminium ash particles with activated carbon, and absorbing tail gas generated when a polyaluminium chloride solution is dried to obtain a hydrolysis mixture; and then ball milling the hydrolysis mixture to obtain a mixed raw material.

[0013] Furthermore, the amount of activated carbon added is 1 to 10% of the mass of the secondary aluminum ash.

[0014] Furthermore, the filter residue obtained by filtration in step 2) is used to prepare calcium aluminate, and the calcination temperature is not less than 1400°C when preparing calcium aluminate. The filtered filter residue contains aluminum oxide and carbon powder, which is calcined to prepare calcium aluminate after adding calcium carbonate, and the carbon powder can be used as a reducing agent during the reaction. The heavy metals in the secondary aluminum ash are enriched in the filter residue, and there are more chlorides remaining in the filter residue. When calcining to prepare calcium aluminate, the heavy metals combine with chlorine to form chloride salts with lower boiling points, which become gaseous under high temperature conditions and are discharged with the exhaust gas. After the exhaust gas is cooled, heavy metal dust is formed, which can be collected and treated in the exhaust gas treatment system, thereby solving the problem of heavy metal treatment. The prepared calcium aluminate can be reused to prepare polyaluminum chloride.

[0015] A device for preparing polyaluminium chloride by using aluminium ash, used for realizing the method of the present invention, comprises a crusher, an agitator, a ball mill, a reactor, a plate and frame filter press, a concentrating tower and a spray drying tower, wherein the agitator is connected to the ball mill, the ball mill is connected to the reactor, the reactor is connected to the plate and frame filter press, the plate and frame filter press is connected to the concentrating tower, and the concentrating tower is connected to the spray drying tower.

[0016] A device for preparing polyaluminium chloride using aluminium ash, used for realizing an improved method, comprises a crusher, an agitator, a fixed-bed absorption tower, a ball mill, a reactor, a plate-and-frame filter press, a concentrating tower and a spray drying tower, wherein the crusher is connected to the agitator, the agitator is connected to the fixed-bed absorption tower, the fixed-bed absorption tower is connected to the ball mill, the ball mill is connected to the reactor, the reactor is connected to the plate-and-frame filter press, the plate-and-frame filter press is connected to the concentrating tower, the concentrating tower is connected to the spray drying tower, and the exhaust port of the spray drying tower is connected to the fixed-bed absorption tower.

[0017] The method of the present invention can reduce heavy metal ions in the polyaluminium chloride solution by micro-electrolysis, adsorb them on the surface of coke particles, and remove them by filtration, so as to achieve the purpose of purifying heavy metals in the polyaluminium chloride solution, thereby realizing the preparation of qualified polyaluminium chloride by using aluminium ash. Compared with the prior art, the present method directly adds carbon to the aluminium ash, and performs micro-electrolysis reaction while the aluminium ash is acid-dissolved, thereby saving reaction time, and at the same time utilizing the metallic aluminium contained in the aluminium ash itself, without adding aluminium chips, thereby saving raw material costs.

[0018] In addition, in the improved method, aluminum ash is used to absorb the acidic tail gas generated during the drying of polyaluminium chloride, which not only reduces the treatment intensity of the tail gas from the drying of polyaluminium chloride, but also uses the acidic tail gas to slowly react with the aluminum ash to slowly hydrolyze the aluminum nitride in the aluminum ash. Since the aluminum ash contains elemental aluminum, it absorbs the acid mist in the tail gas after mixing with coke. In this stage, an aluminum-carbon micro-electrolysis reaction can also be produced, which has a deammoniation effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of the device for preparing polyaluminium chloride in Example 1;

[0020] Figure 2 This is a schematic diagram of the device for preparing polyaluminium chloride in Example 2. DETAILED DESCRIPTION

[0021] The scheme of the present invention is described in detail below with reference to specific examples.

[0022] Example 1

[0023] A method for preparing polyaluminium chloride using aluminium ash comprises the following steps:

[0024] 1) Mixing the secondary aluminum ash and activated carbon, and ball milling to obtain a mixed raw material;

[0025] 2) Add hydrochloric acid to the reaction kettle, and then add the mixed raw materials in batches to react, adjust the basicity of the reactants, filter to obtain a polyaluminium chloride solution, and dry to obtain polyaluminium chloride.

[0026] In this scheme, the reaction conditions can adopt the conventional polyaluminium chloride production process, such as a hydrochloric acid mass concentration of 20%, a reaction temperature of 100-110°C, and a total reaction time of 2 hours.

[0027] In this scheme, the difference from the conventional process is that the aluminum ash activated carbon mixture is added in batches. Through experiments, it is found that mixing the aluminum ash activated carbon mixture with hydrochloric acid once and then reacting it cannot achieve the purpose of reducing the heavy metal content in the solution. It may be that after the one-time feeding, the aluminum element in the raw material reacts with hydrochloric acid first, and when the heavy metals in the aluminum ash are dissolved into the solution, there is no remaining aluminum to participate in the micro-electrolysis reaction. Experimental comparison shows that the heavy metal content in the polyaluminum chloride solution can be reduced by adding the mixed raw materials in batches.

[0028] When the batch adding method is adopted, the addition amount of activated carbon is within 10%. As the addition amount increases, the removal effect of heavy metals increases. Therefore, in further experiments, 10% activated carbon is chosen to be added to the aluminum ash.

[0029] The experimental method is to use a one-time feeding method and a batch feeding method in a small reactor with a volume of 1L, use the aluminum ash activated carbon mixture and hydrochloric acid to react, adjust the basicity, filter to obtain a polyaluminum chloride solution, and obtain polyaluminum chloride after drying. The changes in the contents of the main heavy metal elements Pb, Cd, and Cr before and after the reaction are detected, as shown in the following table:

[0030]

[0031] According to the above comparison, when the interval time of adding mixed raw materials in batches is 30 minutes, the removal effect of heavy metals is better.

[0032] The device used to implement this embodiment is as follows: Figure 1 , including a crusher, an agitator, a ball mill, a reactor, a plate and frame filter press, a concentrating tower, and a spray drying tower. The agitator is connected to the ball mill, the ball mill is connected to the reactor, the reactor is connected to the plate and frame filter press, the plate and frame filter press is connected to the concentrating tower, and the concentrating tower is connected to the spray drying tower.

[0033] Example 2

[0034] Based on Example 1, an improved method is proposed, wherein the secondary aluminum ash is first crushed to obtain aluminum ash particles, which are mixed with activated carbon to absorb the tail gas generated when the polyaluminum chloride solution is dried to obtain a hydrolysis mixture; the hydrolysis mixture is then ball-milled to obtain a mixed raw material. The mixed raw material is then reacted with hydrochloric acid to prepare polyaluminum chloride.

[0035] When the polyaluminium chloride solution is dried, the tail gas generated is mainly water vapor and contains hydrogen chloride, which cannot be discharged directly. The conventional treatment method is to use water spray and alkali spray for secondary treatment. This scheme uses a mixture of aluminium ash and activated carbon particles to absorb the tail gas. Aluminium nitride undergoes hydrolysis after absorbing moisture to produce ammonia. At the same time, under acidic conditions, aluminium and activated carbon produce a micro-electrolysis reaction to absorb hydrogen chloride and achieve a deammoniation effect.

[0036] The device used to implement this embodiment is as follows: Figure 2 , including a crusher, an agitator, a fixed bed absorption tower, a ball mill, a reactor, a plate and frame filter press, a concentrating tower, and a spray drying tower. The crusher is connected to the agitator, the agitator is connected to the fixed bed absorption tower, the fixed bed absorption tower is connected to the ball mill, the ball mill is connected to the reactor, the reactor is connected to the plate and frame filter press, the plate and frame filter press is connected to the concentrating tower, the concentrating tower is connected to the spray drying tower, and the exhaust port of the spray drying tower is connected to the fixed bed absorption tower.

Claims

1. A method for preparing polyaluminium chloride using aluminium ash, characterized in that: The following steps are involved: 1) Mixing secondary aluminum ash and activated carbon, and ball milling to obtain a mixed raw material; the amount of activated carbon added is 1-10% of the mass of the secondary aluminum ash; 2) Add hydrochloric acid to the reaction kettle, and then add the mixed raw materials in batches to react, adjust the basicity of the reactants, filter to obtain a polyaluminium chloride solution, and dry to obtain polyaluminium chloride.

2. The method for preparing polyaluminium chloride using aluminium ash according to claim 1, characterized in that: In step 2), the interval time for adding the mixed raw materials in batches is 30 minutes.

3. The method for preparing polyaluminium chloride using aluminium ash according to claim 1, characterized in that: The secondary aluminum ash is first crushed to obtain aluminum ash particles, which are then mixed with activated carbon to absorb tail gas generated when the polyaluminum chloride solution is dried to obtain a hydrolysis mixture; the hydrolysis mixture is then ball-milled to obtain a mixed raw material.

4. The method for preparing polyaluminium chloride using aluminium ash according to claim 1, characterized in that: The filter residue obtained by filtration in step 2) is used to prepare calcium aluminate.