A tread rubber composite material for a vehicle transporting inflammable and explosive goods, and a preparation method and application thereof

By introducing carbon nanotubes and iron-based catalytic butylene rubber into the tire tread rubber, the problem of the existing tread rubber lacks electrostatic conduction function is solved, and the effect of reducing resistance, improving mechanical and rolling performance is achieved, and the tires are improved safety and durability.

CN116355295BActive Publication Date: 2024-11-26SHANDONG HAOHUA TIRE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310200507.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-06
Publication Date
2024-11-26
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

The existing tire tread glue lacks the static conduction function, which leads to the safety hazards of spontaneous combustion or explosion when static electricity accumulates.

Method used

Using a flammable and explosive transport vehicle tread glue composite material, the formula includes olefin rubber, carbon nanotubes, zinc oxide, stearic acid, plasticizer, coupling agent, tackifying resin, sulfur, accelerator and anti-prevention The coke agent is plasticized and kneaded by a dense mixer to prepare a tread glue with conductive properties.

Benefits of technology

While ensuring the processing performance of rubber composite materials, the resistance of the tread rubber is reduced, the mechanical properties, tear resistance and slip resistance are improved, the rolling resistance and wear are reduced, and the safety and fuel economy of the tire are improved. and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004108892090000071
    Figure BDA0004108892090000071
  • Figure BDA0004108892090000081
    Figure BDA0004108892090000081
Patent Text Reader

Abstract

A tread rubber composite material for a vehicle transporting inflammable and explosive goods, and a preparation method and application thereof. The present invention belongs to the field of rubber materials and their preparation. The purpose of the present invention is to solve the technical problem that the existing tire tread rubber does not have the function of conducting static electricity. The material of the present invention is prepared from olefin rubber, reinforcing filler, carbon nanotubes, zinc oxide, stearic acid, plasticizer, coupling agent, tackifying resin, sulfur, accelerator, antioxidant, and anti-scorch agent. The olefin rubber is a mixture of natural rubber, butadiene rubber, styrene-butadiene rubber, and butadiene-butadiene-vinyl rubber. The present invention introduces iron-catalyzed butadiene-vinyl rubber and carbon nanotubes into the rubber formula. While ensuring the processing performance of the rubber composite material, under the same test conditions, the resistance of the tire tread rubber is reduced to 8×10 3 Ω, thereby improving the safety, fuel economy and durability of tire use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of rubber materials and preparation thereof, and in particular relates to a tread rubber composite material for a vehicle for transporting inflammable and explosive goods, and a preparation method and application thereof. Background Art

[0002] When a car is driving, friction between internal parts, between the surface of the car body and dry air, and between the tires and the ground will generate static electricity. Static electricity accumulates in a short period of time, forming a high potential difference, which is discharged instantly. For vehicles transporting flammable and explosive goods, it can cause significant damage to the internal structure of electronic components and special sensitive electronic components. High-level static electricity can cause spontaneous combustion or explosion of the vehicle, affecting the normal operation of electronic equipment and posing a major safety hazard.

[0003] The anti-static grounding belt for vehicles has the problem of falling off during use, and cannot provide effective protection. Tires are the only way for vehicles to contact the ground, and they are in real-time contact with the ground. If the tires have the function of conducting static electricity, this problem can be completely eliminated. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problem that the existing tire tread rubber does not have the static electricity conductive function, and to provide a tread rubber composite material for a vehicle transporting inflammable and explosive goods, and a preparation method and application thereof.

[0005] One of the purposes of the present invention is to provide a tread rubber composite material for a vehicle transporting inflammable and explosive goods, wherein the tread rubber composite material for a vehicle transporting inflammable and explosive goods is prepared from the following components in parts by weight:

[0006] 100 parts of olefin rubber;

[0007] Reinforcing filler 20-90 parts;

[0008] 0.5-5 parts of carbon nanotubes;

[0009] Zinc oxide 1-5 parts;

[0010] 0.5-5 parts of stearic acid;

[0011] Plasticizer 0.5-30 parts;

[0012] 0.5-15 parts of coupling agent;

[0013] 0.5-10 parts of tackifying resin;

[0014] Sulfur 1-20 parts;

[0015] 1-5 parts of accelerator;

[0016] 1-5 parts of antioxidant;

[0017] Anti-scorch agent 0.1-3 parts;

[0018] The olefin rubber is mixed by weight with 0-70 parts of natural rubber, 0-30 parts of butadiene rubber, 5-70 parts of styrene-butadiene rubber and 15-75 parts of butadiene-elastomer rubber, wherein the parts of natural rubber and butadiene rubber are not both 0.

[0019] It is further defined that the number average molecular weight of the butadiene-ethylene rubber is 92.4w, the molar ratio of the monomers butadiene and isoprene during the preparation process is 3:7, the molar content of 1,2-butadiene in the butadiene structural unit is 20%, the molar content of 1,4-butadiene is 80%, the molar content of 3,4-isoprene in the isoprene structural unit is 86%, and the molar content of 1,4-isoprene is 14%.

[0020] It is further defined that the carbon nanotubes are single-layer carbon nanotubes, double-layer carbon nanotubes and multi-layer carbon nanotubes with a diameter of 1-500 nm, or a mixture of any of the above-mentioned.

[0021] It is further defined that the reinforcing filler is one of carbon black and white carbon black or a mixture of the two in any ratio.

[0022] It is further defined that the carbon black is one or a mixture of any proportions of contact carbon black, furnace carbon black, thermal carbon black and new process carbon black.

[0023] It is further defined that white carbon black is a mixture of one or more of fumed white carbon black and precipitated white carbon black in any ratio.

[0024] It is further defined that the plasticizer is one or a mixture of any proportion of aromatic oil, cyclohexane oil, paraffin oil, coal tar, paraffin, microcrystalline wax and naphtha.

[0025] It is further defined that the coupling agent is one or a mixture of several of silanes, phthalates, phosphates and aluminates in any ratio.

[0026] It is further defined that the tackifying resin is one or a mixture of any ratio of coumarone-indene resin, terpene resin, petroleum resin, natural resin, alkylphenol-formaldehyde resin and xylene resin.

[0027] It is further defined that the accelerator is one or a mixture of several of the following in any ratio: sulfonamides, thiazoles, thiurams, thioureas, dithiocarbamates, aldehyde amines, guanidines and xanthates.

[0028] It is further defined that the antioxidant is one or a mixture of several of quinoline, p-phenylenediamine, naphthylamine and phenol in any ratio.

[0029] It is further defined that the scorch retarder is one or a mixture of several of sulfur and nitrogen, organic acids and nitroso compounds in any ratio.

[0030] The second object of the present invention is to provide a method for preparing a composite material of a tread rubber for a vehicle transporting inflammable and explosive goods. The method for preparing the composite material of a tread rubber for a vehicle transporting inflammable and explosive goods is carried out according to the following steps:

[0031] Step 1: Add olefin rubber into an internal mixer for plasticization to obtain plasticized rubber;

[0032] Step 2: Put the plasticized rubber that has been parked for more than 4 hours, the reinforcing filler, the carbon nanotubes, stearic acid, zinc oxide, the plasticizer, the coupling agent, the tackifying resin, the antioxidant and the anti-scorch agent into an internal mixer for mixing to obtain a mixed rubber;

[0033] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

[0034] Compared with the prior art, the present invention has the following significant effects:

[0035] The present invention introduces iron-catalyzed butyl-pentane rubber and carbon nanotubes into the rubber formula, while ensuring the processing performance of the rubber composite material, under the same test conditions, the tire tread rubber resistance is reduced to 8×10 3 Ω, and at the same time, the mechanical properties of rubber materials are improved, the tensile properties are improved by about 15.32%, the tear resistance is improved by about 12.63%, the anti-slip performance of rubber composite materials is improved by about 8.32%, the rolling resistance of rubber composite materials is reduced by about 10.29%, and the wear is reduced by 7.89%, thereby improving the safety, fuel economy and durability of tire use. The specific advantages are as follows:

[0036] 1) The abundant side groups (vinyl and propylene) in the iron-catalyzed butyl-pentane rubber have a large spatial volume. The carbon nanotubes dispersed in the composite material can effectively reduce the distance between the molecular chain and the carbon nanotubes, enhance the continuous distribution between the carbon nanotubes and the rubber matrix within the system, enhance the tunneling effect and field emission effect, and enhance the conductivity of the system; at the same time, due to the large specific surface area, thin layer, and small particle size of the carbon nanotubes, they can be evenly dispersed in the rubber to connect with each other, forming an electron migration path, increasing the compatibility with the iron-catalyzed butyl-pentane rubber and enhancing the synergistic effect between the two. In addition, in the system, the adjacent atoms in the carbon nanotubes are connected by covalent bonds, and the delocalized π bonds in their structure allow electrons to move freely in them, increasing the electron mobility, and evenly dispersing in the rubber matrix, effectively improving the mechanical properties of the rubber composite material.

[0037] 2) The electron-donating side methyl group is connected to the double bond carbon in the 3,4-propylene group, which increases the activity of α-H and reduces the double bond dissociation energy, forming carbon anions that interact with the surface of the reinforcing filler. The dispersion effect of carbon nanotubes and reinforcing fillers in the rubber matrix is ​​improved, the agglomeration between fillers is destroyed, and the filler-filler grid is reduced. When the tire is deformed under stress, the friction between fillers is reduced, the resistance to movement between molecules is reduced, and the rolling resistance is reduced. At the same time, the addition of carbon nanotubes increases the modulus of the entire system. Under the same external force, the deformation amount is reduced, thereby reducing the internal friction of the material and further reducing the rolling resistance. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail, clearly and completely in conjunction with the embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0039] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0040] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained by those skilled in the art through commercial channels. For process parameters not specifically specified, conventional conditions can be referred to.

[0041] The terms "comprising," "including," "having," "containing," or any other variations thereof, as used in the following examples, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.

[0042] The "one embodiment" or "embodiment" referred to in the following embodiments refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.

[0043] When equivalent, concentration or other value or parameter is represented by the range limited by range, preferred range or a series of upper preferred value and lower preferred value, this should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the scope is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, range limitation can be combined and / or interchanged, if these ranges are not otherwise stated, include all sub-ranges contained therein.

[0044] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.

[0045] Example 1: The formula of the tread rubber composite material of the inflammable and explosive goods transport vehicle of this example is shown in Table 1, and the performance test results are shown in Table 2;

[0046] The number average molecular weight of the butadiene-vinyl rubber is 92.4w, the molar ratio of monomers butadiene to isoprene during the preparation process is 3:7, and the microstructure composition of the prepared butadiene-vinyl rubber is as follows: the molar content of 1,2-butadiene in the butadiene structural unit is 20%, the molar content of 1,4-butadiene is 80%, the molar content of 3,4-isoprene in the isoprene structural unit is 86%, and the molar content of 1,4-isoprene is 14%, which is recorded as BIR-7369.

[0047] The carbon nanotubes are 5-layer carbon nanotubes with a diameter of 158 nm.

[0048] The preparation method of the tread rubber composite material for a vehicle transporting inflammable and explosive goods is carried out according to the following steps:

[0049] Step 1: In an internal mixer, natural rubber, solution-polymerized styrene-butadiene rubber, cis-butadiene rubber and butadiene-pentadiene rubber are added at a filling factor of 0.72, and plasticized at 130° C. for 240 seconds to obtain a plasticized rubber;

[0050] Step 2: Put the plasticized rubber, reinforcing filler, carbon nanotubes, stearic acid, zinc oxide, plasticizer, coupling agent, tackifying resin, antioxidant and anti-scorch agent, which have been parked for more than 4 hours, into an internal mixer with a filling factor of 0.73, and mix at 144° C. for 300 seconds to obtain a mixed rubber;

[0051] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

[0052] Example 2: The formula of the tread rubber composite material of the inflammable and explosive goods transport vehicle of this example is shown in Table 1, and the performance test results are shown in Table 2;

[0053] The number average molecular weight of the butadiene-vinyl rubber is 92.4w, the molar ratio of monomers butadiene to isoprene during the preparation process is 3:7, and the microstructure composition of the prepared butadiene-vinyl rubber is as follows: the molar content of 1,2-butadiene in the butadiene structural unit is 20%, the molar content of 1,4-butadiene is 80%, the molar content of 3,4-isoprene in the isoprene structural unit is 86%, and the molar content of 1,4-isoprene is 14%, which is recorded as BIR-7369.

[0054] The carbon nanotubes are 5-layer carbon nanotubes with a diameter of 124 nm.

[0055] The preparation method of the tread rubber composite material for a vehicle transporting inflammable and explosive goods is carried out according to the following steps:

[0056] Step 1: In an internal mixer, natural rubber, solution-polymerized styrene-butadiene rubber, cis-butadiene rubber and butadiene-pentadiene rubber are added at a filling factor of 0.68, and plasticized at 132° C. for 240 seconds to obtain a plasticized rubber;

[0057] Step 2: Put the plasticized rubber, reinforcing filler, carbon nanotubes, stearic acid, zinc oxide, plasticizer, coupling agent, tackifying resin, antioxidant and anti-scorch agent into an internal mixer with a filling factor of 0.69, and mix at 138° C. for 300 seconds to obtain a mixed rubber;

[0058] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

[0059] Example 3: The formula of the tread rubber composite material of the inflammable and explosive goods transport vehicle of this example is shown in Table 1, and the performance test results are shown in Table 2;

[0060] The number average molecular weight of the butadiene-vinyl rubber is 92.4w, the molar ratio of monomers butadiene to isoprene during the preparation process is 3:7, and the microstructure composition of the prepared butadiene-vinyl rubber is as follows: the molar content of 1,2-butadiene in the butadiene structural unit is 20%, the molar content of 1,4-butadiene is 80%, the molar content of 3,4-isoprene in the isoprene structural unit is 86%, and the molar content of 1,4-isoprene is 14%, which is recorded as BIR-7369.

[0061] The carbon nanotube has a diameter of 131 nm and is a 5-layer carbon nanotube.

[0062] The preparation method of the tread rubber composite material for a vehicle transporting inflammable and explosive goods is carried out according to the following steps:

[0063] Step 1: In an internal mixer, natural rubber, solution-polymerized styrene-butadiene rubber, cis-butadiene rubber and butadiene-pentadiene rubber are added at a filling factor of 0.71, and plasticized at 131° C. for 240 seconds to obtain a plasticized rubber;

[0064] Step 2: Put the plasticized rubber, reinforcing filler, carbon nanotubes, stearic acid, zinc oxide, plasticizer, coupling agent, tackifying resin, antioxidant and anti-scorch agent into an internal mixer with a filling factor of 0.69, and mix at 144° C. for 300 seconds to obtain a mixed rubber;

[0065] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

[0066] Example 4: The formula of the tread rubber composite material of the inflammable and explosive goods transport vehicle of this example is shown in Table 1, and the performance test results are shown in Table 2;

[0067] The number average molecular weight of the butadiene-vinyl rubber is 92.4w, the molar ratio of monomers butadiene to isoprene during the preparation process is 3:7, and the microstructure composition of the prepared butadiene-vinyl rubber is as follows: the molar content of 1,2-butadiene in the butadiene structural unit is 20%, the molar content of 1,4-butadiene is 80%, the molar content of 3,4-isoprene in the isoprene structural unit is 86%, and the molar content of 1,4-isoprene is 14%, which is recorded as BIR-7369.

[0068] The carbon nanotube has a diameter of 169 nm and is a 5-layer carbon nanotube.

[0069] The preparation method of the tread rubber composite material for a vehicle transporting inflammable and explosive goods is carried out according to the following steps:

[0070] Step 1: In an internal mixer, natural rubber, solution-polymerized styrene-butadiene rubber, butadiene rubber and butadiene-pentadiene rubber are added at a filling factor of 0.69, and plasticized at 131° C. for 240 seconds to obtain a plasticized rubber;

[0071] Step 2: Put the plasticized rubber, reinforcing filler, carbon nanotubes, stearic acid, zinc oxide, plasticizer, coupling agent, tackifying resin, antioxidant and anti-scorch agent, which have been parked for more than 4 hours, into an internal mixer with a filling factor of 0.72, and mix at 142° C. for 300 seconds to obtain a mixed rubber;

[0072] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

[0073] Comparative Example 1: This comparative example differs from Example 4 in that: no BIR-7369 is added, the carbon nanotubes have a diameter of 162 nm and are 5-layer carbon nanotubes, the specific formula is shown in Table 1; the performance test results are shown in Table 2; the preparation method is as follows:

[0074] Step 1: In an internal mixer, natural rubber, solution polymerized styrene-butadiene rubber and butadiene rubber are added at a filling factor of 0.67, and plasticized at 135° C. for 240 seconds to obtain plasticized rubber;

[0075] Step 2: Put the plasticized rubber, reinforcing filler, carbon nanotubes, stearic acid, zinc oxide, plasticizer, coupling agent, tackifying resin, antioxidant and anti-scorch agent, which have been parked for more than 4 hours, into an internal mixer with a filling factor of 0.71, and mix at 144° C. for 300 seconds to obtain a mixed rubber;

[0076] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

[0077] Comparative Example 2: This comparative example differs from Example 4 in that no carbon nanotubes are added, the specific formula is shown in Table 1; the performance test results are shown in Table 2; the preparation method is as follows:

[0078] Step 1: In an internal mixer, natural rubber, solution-polymerized styrene-butadiene rubber, cis-butadiene rubber and butadiene-pentadiene rubber are added at a filling factor of 0.68, and plasticized at 133° C. for 240 seconds to obtain a plasticized rubber;

[0079] Step 2: Put the plasticized rubber, reinforcing filler, stearic acid, zinc oxide, plasticizer, coupling agent, tackifying resin, antioxidant and anti-scorch agent, which have been parked for more than 4 hours, into an internal mixer with a filling factor of 0.71, and mix at 143° C. for 300 seconds to obtain a mixed rubber;

[0080] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

[0081] Comparative Example 3: This comparative example is different from Example 4 in that no butadiene-vinyl rubber BIR-7369 and carbon nanotubes are added, and the specific formula is shown in Table 1; the performance test results are shown in Table 2; and the preparation method is as follows:

[0082] Step 1: In an internal mixer, natural rubber, solution polymerized styrene-butadiene rubber and butadiene rubber are added at a filling factor of 0.71, and plasticized at 133° C. for 240 seconds to obtain plasticized rubber;

[0083] Step 2: Put the plasticized rubber, reinforcing filler, stearic acid, zinc oxide, plasticizer, coupling agent, tackifying resin, antioxidant and anti-scorch agent, which have been parked for more than 4 hours, into an internal mixer with a filling factor of 0.71, and mix at 142° C. for 300 seconds to obtain a mixed rubber;

[0084] Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle

[0085] Table 1 Formulation of rubber composite materials

[0086]

[0087]

[0088] Table 2 Rubber composite material properties

[0089] Performance parameters Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength, MPa 13.64 14.32 14.79 15.23 13.45 13.38 13.21 100% tensile stress, MPa 2.14 2.23 2.28 2.37 2.08 2.11 1.99 300% tensile stress, MPa 8.23 8.38 8.51 8.62 8.12 8.09 7.98 Elongation at break, % 458.76 465.73 478.21 489.59 463.17 457.62 449.95 Shore A Hardness 64 64 65 65 64 64 63 Tear strength, KN / m 44.7 46.1 47.3 48.5 43.5 43.8 43.1 <![CDATA[DIN wear, mm 3 / 40m]]> 0.1896 0.1874 0.1831 0.1789 0.1912 0.1908 0.1929 0℃tanδ 0.306 0.312 0.317 0.322 0.284 0.301 0.297 60℃tanδ 0.091 0.088 0.086 0.085 0.092 0.091 0.094 Surface resistance, Ω <![CDATA[3×10 6 ]]> <![CDATA[7×10 5 ]]> <![CDATA[4×10 7 ]]> <![CDATA[8×10 3 ]]> <![CDATA[8×10 9 ]]> <![CDATA[2×10 12 ]]> ∞

[0090] According to the data in Table 2, the present invention introduces iron-catalyzed butyl ethylene rubber and carbon nanotubes into the rubber formula, while ensuring the processing performance of the rubber composite material, under the same test conditions, the resistance of the tire tread rubber is reduced to 8×10 3 Ω, and at the same time, the mechanical properties of the rubber material are improved, the tensile performance is improved by about 15.32%, the tear resistance is improved by about 12.63%, the anti-skid performance of the rubber composite material is improved by about 8.32%, the rolling resistance of the rubber composite material is reduced by about 10.29%, and the wear is reduced by 7.89%, thereby improving the safety, fuel economy and durability of the tire.

[0091] This is mainly due to: 1) the abundant side groups (vinyl and propylene) in the iron-based catalytic butyl-pentyl rubber have a large spatial volume. The carbon nanotubes are dispersed in the composite material, which can effectively reduce the distance between the molecular chain and the carbon nanotubes, enhance the continuous distribution between the carbon nanotubes and the rubber matrix within the system, enhance the tunnel effect and field emission effect, and enhance the conductivity of the system; at the same time, due to the large specific surface area, thin layer, and small particle size of the carbon nanotubes, they can be evenly dispersed in the rubber to connect with each other, forming an electron migration path, increasing the compatibility with the iron-based catalytic butyl-pentyl rubber and enhancing the synergistic effect between the two. In addition, in the system, the adjacent atoms in the carbon nanotubes are connected by covalent bonds, and the delocalized π bonds in their structure allow electrons to move freely in them, increasing the electron mobility, and evenly dispersing in the rubber matrix, effectively improving the mechanical properties of the rubber composite material.

[0092] 2) The electron-donating side methyl group is connected to the double bond carbon in the 3,4-propylene group, which increases the activity of α-H and reduces the double bond dissociation energy, forming carbon anions that interact with the surface of the reinforcing filler. The dispersion effect of carbon nanotubes and reinforcing fillers in the rubber matrix is ​​improved, the agglomeration between fillers is destroyed, and the filler-filler grid is reduced. When the tire is deformed under stress, the friction between fillers is reduced, the resistance to movement between molecules is reduced, and the rolling resistance is reduced. The addition of carbon nanotubes increases the modulus of the entire system. Under the same external force, the deformation amount is reduced, thereby reducing the internal friction of the material and reducing rolling resistance.

[0093] Those skilled in the art should understand that the above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can modify or replace the technical solution of the present invention within the technical scope disclosed by the present invention without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A composite material for tread rubber of a vehicle for transporting inflammable and explosive goods, characterized in that: It is prepared from the following components by weight: 100 parts of olefin rubber; Reinforcing filler 20-90 parts; 1.5-5 parts of carbon nanotubes; Zinc oxide 1-5 parts; 0.5-5 parts of stearic acid; Plasticizer 0.5-30 parts; 0.5-15 parts of coupling agent; 0.5-10 parts of tackifying resin; Sulfur 1-20 parts; 1-5 parts of accelerator; 1-5 parts of antioxidant; Anti-scorch agent 0.1-3 parts; The olefin rubber is prepared by mixing 10-70 parts of natural rubber, 15-30 parts of butadiene rubber, 5-70 parts of styrene-butadiene rubber and 40-75 parts of butadiene-isoprene rubber by weight. The butadiene-isoprene rubber is iron-catalyzed butadiene-isoprene rubber with a number average molecular weight of 92.4 W. During the preparation process, the molar ratio of monomers butadiene to isoprene is 3:7, the molar content of 1,2-butadiene in the butadiene structural unit is 20%, the molar content of 1,4-butadiene is 80%, the molar content of 3,4-isoprene in the isoprene structural unit is 86%, the molar content of 1,4-isoprene is 14%, and the carbon nanotube has a diameter of 1-500 nm and is a 5-layer carbon nanotube.

2. The tread rubber composite material for a vehicle transporting inflammable and explosive goods according to claim 1, characterized in that: The reinforcing filler is one or both of carbon black and white carbon black.

3. The tread rubber composite material for a vehicle transporting inflammable and explosive goods according to claim 2, characterized in that: The carbon black is one or more of contact carbon black, furnace carbon black, thermal carbon black and new process carbon black.

4. The tread rubber composite material for a vehicle transporting inflammable and explosive goods according to claim 2, characterized in that: The white carbon black is one or more of fumed white carbon black and precipitated white carbon black.

5. The tread rubber composite material for a vehicle transporting inflammable and explosive goods according to claim 1, characterized in that: The plasticizer is one or more of aromatic oil, cyclohexane oil, paraffin oil, coal tar, paraffin, microcrystalline wax and naphtha, the coupling agent is one or more of silanes, phthalates, phosphates and aluminates, the tackifying resin is one or more of coumarone-indene resin, terpene resin, petroleum resin, alkylphenol-formaldehyde resin and xylene resin, and the accelerator is one or more of sulfonamides, thiazoles, thiurams, thioureas, dithiocarbamates, aldehyde amines, guanidines and xanthates.

6. The tread rubber composite material for a vehicle transporting inflammable and explosive goods according to claim 1, characterized in that: The antioxidant is one or more of quinoline, p-phenylenediamine, naphthylamine and phenol, and the anti-scorching agent is one or more of sulfur and nitrogen, organic acid and nitroso compound.

7. The method for preparing the composite material for tread of a vehicle for transporting inflammable and explosive goods according to any one of claims 1 to 6, characterized in that: Follow these steps: Step 1: Add olefin rubber into an internal mixer for plasticization to obtain plasticized rubber; Step 2: Putting the plasticized rubber that has been stored for more than 4 hours, the reinforcing filler, the carbon nanotubes, stearic acid, zinc oxide, the plasticizer, the coupling agent, the tackifying resin, the antioxidant and the anti-scorch agent into an internal mixer for mixing to obtain a mixed rubber; Step 3: Add the mixed rubber, sulfur and accelerator into the internal mixer and continue mixing to obtain the tread rubber composite material for the flammable and explosive goods transport vehicle.

8. Use of the tread rubber composite material for a vehicle transporting inflammable and explosive goods according to any one of claims 1 to 6 in preparing tires for a vehicle transporting inflammable and explosive goods.