A carbon-based water-based high-temperature resistant solder ink and its preparation method and application
By using water-based high-temperature resistant resin and carbon nanotube composite materials in aqueous carbon electronic paste, the adhesion and conductivity at high temperatures are improved, and the insufficient performance of existing aqueous carbon electronic paste under high temperature conditions is solved. , and reduce VOC emissions through solvent preparation, achieving environmentally friendly and low-carbon printed circuit board manufacturing.
Patent Information
- Application Number
- CN202310388021.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-12
AI Technical Summary
The existing aqueous carbon electronic paste has poor adhesion and conductivity under high temperature conditions, and the solvent-based electronic paste has problems of high VOC emissions and poor environmental protection.
Carbon-based water-based high-temperature resistant solder ink, including water-based high-temperature resistant resin, carbon black, graphite and carbon nanotube composite materials, improve the conductivity through three-dimensional electron transmission channels, and improve the high-temperature resistant performance of the ink through the coating of water-based high-temperature resistant resin. and adhesion, and use solvents at different boiling points to adjust the dispersion and surface tension of the ink to improve printing adaptability.
Maintain excellent adhesion and conductivity under high temperature conditions, reduce VOC emissions, simplify printing waste recycling and treatment, and realize economical, environmentally friendly, green and low-carbon printed circuit board manufacturing.
Smart Images

Figure BDA0004174780100000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic pastes, and in particular to a carbon-based water-based high-temperature-resistant solder ink and a preparation method and application thereof. Background Art
[0002] In the PCB (printed circuit board) industry, the electronic paste used in printed circuits must have good conductivity, high adhesion, good printing adaptability and stable performance.
[0003] Electronic pastes usually include metal-based electronic pastes and carbon-based electronic pastes. Metal-based electronic pastes have good conductivity, high curing temperature and long curing time, so they have the problems of high cost and high energy consumption. Carbon-based electronic pastes are widely used due to their low cost and stable performance, but the electronic carbon pastes currently used in the market are solvent-based, with high VOC emissions and poor environmental protection.
[0004] Developing water-based electronic carbon paste is an effective way to solve this problem. However, PCB boards inevitably undergo welding operations during the production process, and the adhesion and conductivity of existing water-based carbon pastes at high temperatures do not meet the requirements. Summary of the invention
[0005] In view of this, the present application provides a carbon-based water-based high-temperature resistant solder ink and a preparation method and application thereof, which has high adhesion and good conductivity under high temperature conditions.
[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions:
[0007] In a first aspect, the present application provides a carbon-based water-based high-temperature resistant solder ink, comprising the following components in mass proportions: 15-30 parts of water-based high-temperature resistant resin, 3-8 parts of dispersant, 8-15 parts of solvent, 0.5-2 parts of defoaming agent, 30-55 parts of deionized water, 5-8 parts of carbon black, 10-18 parts of graphite, and 2-4 parts of carbon nanotubes, the heat-resistant temperature of the water-based high-temperature resistant resin is greater than or equal to 250°C, and the solvent is an organic mixture with different melting points.
[0008] Preferably, the solvent is a mixture of isohexylene glycol and isopropanol.
[0009] Preferably, the mass ratio of isohexylene glycol to isopropanol is 1-3:1.
[0010] Preferably, the water-based high temperature resistant resin is obtained by reacting water-based acrylic monomers and water-based polyurethane monomers as raw materials.
[0011] Preferably, the mass ratio of the waterborne acrylic monomer to the waterborne polyurethane monomer is 20-30:8-12.
[0012] Preferably, the mass ratio of the sum of the mass of carbon black, graphite and carbon nanotubes to the mass of the water-based high temperature resistant resin is 1:1-1.4.
[0013] Preferably, the mass ratio of the sum of the mass of carbon black, graphite and carbon nanotubes to the mass of the dispersant is 3-5:1.
[0014] In a second aspect, the present application provides a method for preparing a carbon-based water-based high temperature resistant solder ink, comprising the following steps:
[0015] S1. After mixing the dispersant, solvent, defoamer and deionized water in parts by mass, carbon black, graphite and carbon nanotubes were added, and then stirred and filtered to obtain a primary carbon slurry;
[0016] S2. Grind the primary carbon slurry, add the water-based high temperature resistant resin, and stir evenly to obtain the carbon-based water-based high temperature resistant solder ink.
[0017] Preferably, in step S2, the particle size of the primary slurry after grinding is less than or equal to 5 μm.
[0018] In a third aspect, the present application provides an application of a carbon-based water-based high-temperature resistant solder ink in the preparation of a printed circuit board.
[0019] The beneficial effects of the present application are as follows: the present application uses a composite of carbon black, graphite and carbon nanotubes as conductive fillers to construct a three-dimensional electron transmission channel during the preparation of the carbon slurry, thereby improving the conductivity of the ink; the added water-based high-temperature resistant resin is used to coat the carbon material, and the resin can be evenly dispersed and coated on the surface of the carbon material, giving the ink high-temperature resistance, so that it still has excellent adhesion after high-temperature treatment, and has good conductivity, and also has the advantages of good printing adaptability, clear and continuous circuits, and no bubbles. At the same time, it reduces the VOC emissions of the ink, simplifies the recycling and treatment process of printing waste liquid, and is economical, environmentally friendly, green and low-carbon; solvents with different boiling points improve the dispersibility of the water-based high-temperature resistant resin in the system and the coating of carbon materials (carbon black, graphite and carbon nanotubes), and at the same time can adjust the surface tension of the ink, improve the wettability and leveling of the ink, and improve the printing adaptability. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0021] The present application provides a carbon-based water-based high-temperature-resistant solder ink, comprising the following components in parts by mass: 15-30 parts of water-based high-temperature-resistant resin, 3-8 parts of dispersant, 8-15 parts of solvent, 0.5-2 parts of defoaming agent, 30-55 parts of deionized water, 5-8 parts of carbon black, 10-18 parts of graphite, and 2-4 parts of carbon nanotubes. The heat-resistant temperature of the water-based high-temperature-resistant resin is greater than or equal to 250°C, and the solvent is an organic mixture with different melting points.
[0022] The carbon-based water-based high-temperature solder ink of this scheme can reduce the VOC emission of the ink while ensuring conductivity and adhesion under high temperature conditions above 250°C, simplify the recycling and treatment process of printing waste liquid, and is economical, environmentally friendly, green and low-carbon. Carbon black, graphite and carbon nanotubes are used as conductive fillers to construct a three-dimensional electron transmission channel during the preparation of carbon slurry to improve the conductivity of the ink; the added water-based high-temperature resin is used to coat the carbon material, and the resin can be evenly dispersed and coated on the surface of the carbon material, giving the ink high-temperature resistance, so that it still has excellent adhesion after high-temperature treatment, and good conductivity, and also has the advantages of good printing adaptability, clear and continuous circuits, and no bubbles. Solvents with different boiling points improve the dispersibility of water-based high-temperature resin in the system and the coating of carbon materials (carbon black, graphite and carbon nanotubes), and at the same time can adjust the surface tension of the ink, improve the wettability and leveling of the ink, and improve the printing adaptability. Among them, when the mass ratio of carbon black and graphite is 1:1.5-1.8, the conductivity of the ink is the best.
[0023] In some embodiments, the solvent is a mixture of isohexanediol and isopropanol. The boiling points of isohexanediol (boiling point is 198°C) and isopropanol (boiling point is 82.5°C) are different and the difference is large. Together with water (boiling point is 100°C), they form three solvents with different boiling points. The three solvents with different boiling points are more conducive to improving the dispersibility of water-based high temperature resistant resin in the system and the coating of carbon materials (carbon black, graphite and carbon nanotubes). At the same time, the surface tension of the ink can be adjusted, the wettability and leveling of the ink can be improved, and the printing adaptability can be improved.
[0024] In some embodiments, the mass ratio of isohexanediol to isopropanol is 1-3:1. The boiling point of isohexanediol is 198°C. If the amount added is too large, the curing time and curing temperature of the ink will increase, which will increase the cost and extend the process time. The boiling point of isopropanol is only 82.5°C. If the amount added to the system is large, the ink will dry too quickly, affecting the printing adaptability.
[0025] In some embodiments, the water-based high temperature resistant resin is obtained by reacting water-based acrylic monomer and water-based polyurethane monomer as raw materials. The specific preparation method is as follows: add acrylic monomer, emulsifier, and water to a pre-stirred reactor, stir evenly for 30 minutes, and obtain a non-stratified emulsion 1; add the remaining water, emulsifier, and polyurethane neutralizer to the reactor, heat it to 90°C, add emulsion 1 and initiator, react for 30 minutes, and obtain emulsion 2; slowly drip polyurethane monomer into emulsion 2, and the whole process is controlled within 2 hours; after keeping warm for 2 hours, adjust the pH value to about 7.5 to obtain a water-based high temperature resistant resin. The resin is a mixed emulsion of water-based acrylic monomer and water-based polyurethane monomer obtained by adding a temperature-resistant group to the molecular chain segment.
[0026] In some embodiments, the mass ratio of waterborne acrylic monomer to waterborne polyurethane monomer is 20-30:8-12. Different raw material ratios can adjust the high temperature resistance threshold of the waterborne high temperature resistant resin to adapt to the high temperature resistance requirements under different environments.
[0027] This scheme limits the amount of carbon material and water-based high-temperature resistant resin. The mass ratio of the sum of the mass of carbon black, graphite, and carbon nanotubes to the mass of the water-based high-temperature resistant resin is 1:1-1.4. From the perspective of the percolation threshold, exceeding this limited range is not conducive to the performance of the ink. If the amount of resin is small, the adhesion and temperature resistance cannot be guaranteed. If the amount of resin is too much, the resistance of the ink increases.
[0028] In some embodiments, the dispersant is one or more of BYK-ET 3033 aqueous wetting dispersant, Disponer W-18 aqueous wetting dispersant, and Sago-9710 aqueous wetting dispersant; the mass ratio of the sum of the masses of carbon black, graphite, and carbon nanotubes to the mass of the dispersant is 3-5:1. Considering the dispersion stability, if there is too little dispersant, the carbon material will not be fully dispersed and will easily agglomerate and precipitate; if there is too much dispersant, electron transmission will be hindered and conductivity will be reduced.
[0029] The defoaming agent is one or more of DefomW-0506 water-based defoaming agent, TEGO Foamex 805 water-based defoaming agent or SF-809B Biaomei silicone-fluorine defoaming agent.
[0030] The present application provides a method for preparing a carbon-based water-based high-temperature resistant solder ink, comprising the following steps:
[0031] S1. After mixing the dispersant, solvent, defoamer and deionized water in parts by mass, carbon black, graphite and carbon nanotubes were added, and then stirred and filtered to obtain a primary carbon slurry;
[0032] S2. Grind the primary carbon slurry, add the water-based high temperature resistant resin, and stir evenly to obtain the carbon-based water-based high temperature resistant solder ink.
[0033] In the preparation method of the present scheme, step S1 allows the dispersant to be fully dissolved and dispersed in water first. After the carbon material is added, the dispersant can interact with the carbon material more evenly to improve the dispersion stability of the ink. Step S2 is to add the resin after the primary carbon slurry is ground. On the one hand, it can avoid the grinding process from destroying the resin structure and thus affecting the heat resistance and adhesion of the ink. On the other hand, it is to ensure that the resin fully covers the carbon material to improve the adhesion under high temperature conditions.
[0034] Preferably, in step S2, the particle size of the primary slurry after grinding is less than or equal to 5 μm, which is conducive to the full coating of the carbon material by the resin.
[0035] The present application provides an application of a carbon-based water-based high-temperature-resistant solder ink in the preparation of a printed circuit board.
[0036] The present solution is further described below through specific embodiments.
[0037] Raw material preparation
[0038] The water-based high temperature resistant resin-1 is prepared according to the following method: 20 parts of acrylic monomer, 3 parts of emulsifier and water are added to a pre-stirred reactor, and stirred evenly for 30 minutes to obtain a non-stratified emulsion 1; the remaining water, 2 parts of emulsifier and 4 parts of polyurethane neutralizer are added to the reactor, and the emulsion 1 and 1 part of initiator are added after heating to 90°C, and the reaction is carried out for 30 minutes to obtain an emulsion 2; 12 parts of polyurethane monomer are slowly dripped into the emulsion 2, and the whole process is controlled within 2 hours; after keeping warm for 2 hours, the pH value is adjusted to about 7.5 to obtain the water-based high temperature resistant resin-1, and the heat resistant temperature of the water-based high temperature resistant resin-1 is 250°C.
[0039] The preparation method of water-based high temperature resistant resin-2 is basically the same as that of water-based high temperature resistant resin-1. The difference is that the amount of acrylic monomer used is 30 parts, the amount of polyurethane monomer used is 8 parts, and the heat resistant temperature of water-based high temperature resistant resin-2 is 280°C.
[0040] Examples 1-4
[0041] A carbon-based water-based high-temperature-resistant solder ink, the composition of which is shown in Table 1. The water-based high-temperature-resistant resin used in Example 2 is water-based high-temperature-resistant resin-2, and the water-based high-temperature-resistant resin used in Examples 1, 3, and 4 is water-based high-temperature-resistant resin-1; the mass ratio of isohexanediol to isopropanol in Example 1 is 1:1, in Example 2 it is 3:1, and in Examples 3 and 4 it is 2:1.
[0042] The preparation method of carbon-based water-based high temperature resistant solder ink is as follows:
[0043] S1. Weigh the components of the high temperature resistant solder ink by mass, place the dispersant, defoamer, deionized water and solvent in a stirring kettle and stir for 60 minutes. After mixing evenly, add carbon black, graphite and carbon nanotubes in sequence, stir until uniform after fully wetting, mix the above carbon slurry with ball milling beads at a mass ratio of 3:1, place in an electric stirrer and stir for 3 hours, then take out and filter to form a primary carbon slurry;
[0044] S2. Grind the primary carbon slurry in a sand mill to a particle size of less than 5 μm, add water-based high temperature resistant resin-1 to the ground carbon slurry, stir at a low speed until uniform, and obtain a carbon-based water-based high temperature resistant solder ink.
[0045] Table 1 Composition formulation of Examples 1-4
[0046] Example 1 Example 2 Example 3 Example 4 Water-based high temperature resistant resin 15 25 30 15 Dispersants 5 8 3 5 Solvents 14 8 15 15 Defoaming agent 0.5 2 2 2 Deionized water 39.5 30 30 55 Carbon Black 5 8 5 6 graphite 18 15 10 12 Carbon Nanotubes 2 3 4 3
[0047] Comparative Example 1
[0048] A carbon-based water-based high-temperature resistant solder ink, the other contents of which are the same as those of Example 3, except that the solvent is isohexanediol.
[0049] Comparative Example 2
[0050] A carbon-based water-based high-temperature resistant solder ink, other contents of which are the same as those of Example 2, except that carbon black and carbon nanotubes are not included.
[0051] Evaluation Test
[0052] The inks in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests, wherein the adhesion was tested according to standard GB / T36650-2018 (25°C, 250°C), the viscosity was tested according to standard GB / T14624.5-1993, the square resistance was tested according to DB13_T 5255-2020, and the surface tension was measured according to the capillary measurement method. The test results are shown in Table 2.
[0053] Table 2 Test results
[0054]
[0055] The mass ratio of carbon material to water-based high temperature resistant resin in Example 1 is 1.6:1, the mass ratio of carbon material to water-based high temperature resistant resin in Example 3 is 0.6:1, and the mass ratio of carbon material to water-based high temperature resistant resin in Examples 2 and 4 is within the range specified in this scheme. It can be seen that the adhesion in Example 1 is lower than that in Examples 2 and 4, while the resistance in Example 3 is higher than that in Examples 2 and 4, indicating that exceeding the specified range is not conducive to the performance of the ink, the amount of resin is small, the adhesion and heat resistance cannot be guaranteed, and the amount of resin is too much, and the resistance of the ink increases; and the resistance in Example 3 is significantly higher than that in Example 4, the reason is that in addition to the increase in the resistance of the ink due to the excessive amount of resin, the amount of dispersant is too much, which exceeds the specified range of this application, so the resistance is further increased, indicating that the dispersant is too much, hindering electron transmission, and reducing conductivity. In Comparative Example 1, no mixed solvent is used, and its adhesion is significantly reduced. In Comparative Example 2, no carbon black and carbon nanotube materials are used, and the square resistance of the ink is significantly increased, indicating that the formula of this scheme can significantly improve the conductivity of the ink and the adhesion at high temperature.
[0056] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A carbon-based water-based high temperature resistant solder ink, It is characterized in that The invention comprises the following components in parts by mass: 15-30 parts of water-based high temperature resistant resin, 3-8 parts of dispersant, 8-15 parts of solvent, 0.5-2 parts of defoamer, 30-55 parts of deionized water, 5-8 parts of carbon black, 10-18 parts of graphite and 2-4 parts of carbon nanotubes, wherein the heat-resistant temperature of the water-based high temperature resistant resin is greater than or equal to 250°C; the solvent is a mixture of isohexanediol and isopropanol, and the mass ratio of isohexanediol to isopropanol is 1-3:1; the water-based high temperature resistant resin is obtained by reacting acrylic acid monomer and polyurethane monomer as raw materials; the mass ratio of acrylic acid monomer to polyurethane monomer is 20-30:8-12; the mass ratio of the sum of the mass of carbon black, graphite and carbon nanotubes to the water-based high temperature resistant resin is 1:1-1.4; the mass ratio of the sum of the mass of carbon black, graphite and carbon nanotubes to the dispersant is 3-5:
1.
2. A method for preparing the carbon-based water-based high temperature resistant solder ink as claimed in claim 1, It is characterized in that The following steps are involved: S1. After mixing the dispersant, solvent, defoamer and deionized water in parts by mass, carbon black, graphite and carbon nanotubes were added, and then stirred and filtered to obtain a primary carbon slurry; S2. Grind the primary carbon slurry, add the water-based high temperature resistant resin, and stir evenly to obtain the carbon-based water-based high temperature resistant solder ink.
3. The preparation method according to claim 2, It is characterized in that In step S2, the particle size of the primary slurry after grinding is less than or equal to 5 μm.
4. A use of the carbon-based water-based high temperature resistant solder ink as claimed in claim 1 in the preparation of printed circuit boards, It is characterized in that Its application temperature is greater than or equal to 250℃.