A method for extracting lithium from salt lake
By adopting a variable-speed adsorption process in the salt lake brine adsorption stage, the brine flow rate is gradually reduced, which solves the problem of low lithium adsorption efficiency at low temperatures, enables the production of desorption solutions with high lithium content and uninterrupted production throughout the year, and improves the economics of the process. and environmental protection.
Patent Information
- Application Number
- CN202111630401.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-28
Smart Images

Figure CN116356144B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of environmental protection and resource recycling, and in particular to a method for extracting lithium from a salt lake. Background Art
[0002] Most of China's lithium resources are stored in salt lake brines, most of which are brines with a high magnesium-to-lithium ratio. Therefore, extracting lithium from brines with a high magnesium-to-lithium ratio has become the focus of China's lithium resource development. The adsorption method developed in recent years has been widely favored due to its advantages such as good selectivity for lithium ions, simple process, ability to extract lithium from salt lake brines with a high magnesium-to-lithium ratio, and low cost.
[0003] However, the current adsorption process for lithium extraction has low lithium adsorption efficiency, and there is also the problem of difficulty in producing qualified desorption liquid with high lithium content at low temperatures (such as winter). Summary of the invention
[0004] In view of this, the present application provides a method that can be used to extract lithium from salt lakes. By adopting a specific variable speed adsorption process in the brine adsorption stage, the adsorption efficiency of lithium in the brine can be greatly improved, solving the problem of difficulty in obtaining a qualified desorption liquid with a high lithium content at low temperatures, and ensuring uninterrupted production all year round.
[0005] Specifically, the present application provides a method for extracting lithium from a salt lake, comprising the following steps:
[0006] (1) passing salt lake brine through a lithium adsorbent at a variable speed so that lithium ions in the salt lake brine are adsorbed on the lithium adsorbent to obtain a lithium-rich adsorbent; wherein, during the adsorption process, the flow rate of the salt lake brine gradually decreases, and the difference between the initial flow rate and the final flow rate of the salt lake brine is 0.5-3 BV / h;
[0007] (2) cleaning the lithium-rich adsorbent;
[0008] (3) Using a lithium ion eluent to desorb lithium ions from the cleaned lithium-rich adsorbent to obtain a desorption solution.
[0009] In the method for extracting lithium from salt lakes provided in the present application, by adopting a specific flow rate change process in which the brine flow rate is gradually reduced during the adsorption stage of the salt lake brine, the adsorption efficiency of lithium in the brine can be greatly improved, especially efficient lithium adsorption at low temperatures (below zero degrees) can be achieved, and thus a desorption liquid with a lithium content of more than 500 mg / L can be obtained without affecting the production capacity; under the same adsorption time (for example, 180 minutes), under the condition that the production capacity remains unchanged, the lithium content in the desorption liquid obtained by the lithium extraction method of the present application is much higher than the desorption liquid obtained by the conventional lithium extraction method using a brine adsorption process with a fixed flow rate (generally around 400 mg / L).
[0010] In the present application, during the adsorption process, the flow rate of the salt lake brine can vary according to time, and the overall flow rate gradually decreases as the adsorption process proceeds. The difference between the initial flow rate and the final flow rate of the salt lake brine is 0.5-3BV / h, specifically 0.8BV / h, 1BV / h, 1.2BV / h, 1.5BV / h, 1.8BV / h, 2BV / h or 2.5BV / h, etc. The appropriate difference between the initial and final flow rates is conducive to improving the adsorption efficiency of lithium in the brine.
[0011] The definition of the initial flow rate and the final flow rate can be determined according to the specific brine speed change process. If the brine flow rate is continuously reduced, the initial flow rate is the brine flow rate that first passes through the lithium adsorbent when the adsorption starts, and the final flow rate is the brine flow rate that last passes through the lithium adsorbent when the adsorption is about to end. If the brine flow rate is discretely reduced in stages, that is, during the adsorption process, the brine flow rate has n different values (n is a finite value, and the flow rates can be V1, V2, ... V n ), where the first velocity segment (velocity V1) is the initial velocity of the brine, and the last velocity segment (i.e., the nth velocity segment, velocity V n ) is the final flow rate. If the total amount of brine to be adsorbed is Q (in Bv), the amount of brine passing through the adsorbent at each flow rate stage can be Q / n, wherein the flow rate of the first Q / n BV of salt lake brine passing through the lithium adsorbent can be called the initial flow rate, and the flow rate of the last Q / n BV of salt lake brine passing through the lithium adsorbent can be called the final flow rate. For example, when 6 BV of salt lake brine needs to be adsorbed, each BV of brine is passed through the lithium adsorbent at a flow rate of 2.5, 2.3, 2.1, 2.0, 1.8, and 1.6 BV / h, respectively, wherein the initial flow rate of the brine is 2.5 BV / h, the final flow rate is 1.6 BV / h, and the adsorption time of each brine is 24 min, 26 min, 28.6 min, 30 min, 33 min, and 37.5 min, respectively.
[0012] In some embodiments of the present application, the initial flow rate is 2.0-3.0BV / h, and the final flow rate is 1.2-1.8BV / h. Compared with the brine adsorption process with a fixed flow rate, the adsorption efficiency of lithium in the brine can be improved by 5%-20% by using such an initial flow rate and final flow rate of the brine. Among them, BV generally refers to the filling volume of the lithium adsorbent, and 2.0-3.0BV / h (the same below) represents that the volume of the brine flow rate is 1.5-3 times the volume of the lithium adsorbent per hour. In some embodiments, the initial flow rate can specifically be 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3.0BV / h, etc. The final flow rate can specifically be 1.2, 1.3, 1.4, 1.5, 1.6, 1.7 or 1.8BV / h, etc.
[0013] Optionally, during the adsorption process, the total amount of the salt lake brine to be adsorbed is 6-8 BV, that is, the volume of the salt lake brine to be contacted with the lithium adsorbent is 6-8 times the loading volume of the lithium adsorbent. The amount of salt lake brine to be adsorbed can vary depending on the lithium content in the salt lake brine (generally 180-300 ppm). Optionally, the total duration of the adsorption can be 2.5-4h, for example, 2.8h, 3h, 3.5h, 3.8h, etc.
[0014] Optionally, in step (1), before the salt lake brine is speed-changed to pass through the lithium adsorbent, it also includes: filtering the brine to remove impurities (especially particulate impurities) therein. Wherein, the filtration can include in sequence: high-speed centrifugal filtration and backwash filtration. High-speed centrifugal filtration is mainly used to remove large particles of precipitate. High-speed centrifugal filtration can be carried out in a centrifugal solid-liquid separator with a centrifugal speed of 15000-35000rpm. Backwash filtration is for further precision filtration to reduce the solid impurities in the salt lake brine to ensure that the filtered material does not affect the adsorption function of the lithium adsorbent, and the impurities after filtration are convenient to backwash, and there is no need to frequently replace the filter consumables. Backwash filtration can be carried out using a stainless steel filter mesh backwash filter.
[0015] In the present application, the salt lake brine is extracted with lithium by adsorption. The lithium adsorbent can be loaded in an exchange column (such as a glass column, a stainless steel column) or a carrier such as an adsorption tower. When the salt lake brine flows through a carrier loaded with a lithium adsorbent and contacts the lithium adsorbent, the lithium ions therein can be adsorbed and fixed by the lithium adsorbent, and the lithium adsorbent is also transformed into a lithium-rich adsorbent adsorbed with lithium.
[0016] In the implementation manner of the present application, the lithium adsorbent used may include an adsorbent material and a binder. Among them, the adsorbent material may be an aluminum-based adsorbent material, a manganese-based adsorbent material (such as a combination of spinel-type manganese oxide and lithium ions), a titanium-based adsorbent material (such as a metatitanate-type lithium ion sieve adsorbent), an iron-based adsorbent material, etc. In some implementation manners of the present application, the adsorbent material is an aluminum-based adsorbent material. The aluminum-based adsorbent material may be a combination of aluminum hydroxide and a lithium-containing compound (such as lithium halide, lithium sulfate, etc.). The aluminum-based adsorbent material can adsorb lithium ions from a lithium-containing solution, and after the adsorption is saturated, the lithium ions can be resolved from it into the solution after elution with water at a certain temperature. In some embodiments, the aluminum-based adsorbent material can be expressed as Li a X·mAl(OH)3·nH2O, where X can be Cl - 、SO4 2- etc.; a=1 or 2; m is 1-5, preferably 2; n is 1-5. Further, in order to make the lithium adsorption capacity of the lithium adsorbent of the present application stronger, before using it to extract lithium from salt lake, the lithium adsorbent can be properly delithiated so that the adsorbent material has more lithium vacancies. The aluminum adsorbent after delithiation can be expressed as (1-x)Li a’ X·mAl(OH)3·nH2O, 0<x<1. Among them, the aluminum-based adsorption material can be prepared by mechanochemical synthesis, immersion, acidification conversion, precipitation, etc. Taking LiCl·mAl(OH)3·nH2O as an example, it can be prepared by soaking aluminum hydroxide in LiCl solution, or by soaking aluminum hydroxide in LiOH solution and then acidifying and converting it, or by co-precipitation of AlCl3 and LiCl solution, or by grinding LiOH and aluminum hydroxide, etc.
[0017] Among them, the binder can be one or more of epoxy resin, phenolic resin, polyvinyl chloride, polyethylene, polypropylene, polystyrene, polyvinylidene fluoride, ethylene-vinyl acetate copolymer, vinylidene fluoride-trifluorochloroethylene copolymer (abbreviated as VDF-CFFE copolymer) and fluoroolefin-vinyl ether copolymer (also known as FEVE type fluorocarbon resin).
[0018] In some embodiments, the binder is at least one of vinylidene fluoride-chlorotrifluoroethylene copolymer and fluoroolefin-vinyl ether copolymer. At this time, the lithium adsorbent also includes a wetting dispersant, which can specifically include one or more of polyethylene glycol, sodium polyacrylate, polyvinyl alcohol, and formaldehyde condensate. Exemplary formaldehyde condensates can include, but are not limited to, one or more of naphthalenesulfonate formaldehyde condensate, methylnaphthalenesulfonate formaldehyde condensate, benzylnaphthalenesulfonate formaldehyde condensate, phenolsulfonate formaldehyde condensate, etc.
[0019] The use of vinylidene fluoride-chlorotrifluoroethylene copolymer and / or fluoroolefin-vinyl ether copolymer as a binder can not only make the lithium adsorbent have high structural stability, mechanical strength and good corrosion resistance, but also have a low dissolution rate and a long service life after repeated lithium absorption and de-lithium use. At the same time, the above-mentioned binder can also make the adsorbent form a surface state with suitable porosity and narrow pore size, so that the lithium adsorption efficiency of the above-mentioned lithium adsorbent is high and the effective active area of the lithium adsorbent will not be reduced to affect its adsorption speed and efficiency; the wettability of the above-mentioned wetting dispersant is also conducive to improving the adsorption efficiency and adsorption amount of lithium ions by the adsorbent. In addition, with the synergistic effect of the excellent surface smoothness and cleaning performance of these two specific binders and the wettability of the wetting dispersant, the above-mentioned lithium adsorbent is easy to clean after adsorbing lithium and the process of desorbing lithium is easier to carry out, thereby saving water in the cleaning and desorption processes, reducing the dissolution rate of the adsorbent in these processes, and lowering the desorption temperature. It is of great significance to realize industrial lithium extraction in high-energy-deficient areas such as salt lakes, and obtain qualified desorption liquid with low magnesium-to-lithium ratio and high lithium content.
[0020] Optionally, the molecular weight of the vinylidene fluoride-chlorotrifluoroethylene copolymer or the fluoroolefin-vinyl ether copolymer can be 100,000-800,000. The bonding effect of the appropriately high molecular weight binder is better, and the risk of cracking and breaking of the lithium adsorbent during use is reduced, thereby increasing its service life. Among them, in the vinylidene fluoride-chlorotrifluoroethylene copolymer, the copolymerization ratio of the monomers vinylidene fluoride and chlorotrifluoroethylene can be 1: (1-5), preferably 1: 4. Preferably, the binder is a vinylidene fluoride-chlorotrifluoroethylene copolymer, or a mixture of a vinylidene fluoride-chlorotrifluoroethylene copolymer and a fluoroolefin-vinyl ether copolymer.
[0021] Optionally, the molecular weight of the formaldehyde condensate is 4000-10000. The molecular weight of the sodium polyacrylate is 5000-10000.
[0022] In some embodiments of the present application, the wetting and dispersing agent is polyethylene glycol. Polyethylene glycol has excellent wetting and dispersibility. Optionally, the molecular weight of the polyethylene glycol is 10000-30000. Polyethylene glycol with a higher molecular weight has a lower solubility in water with the adsorbent, which prolongs the service life of the adsorbent.
[0023] In the embodiment of the present application, based on the weight of the lithium adsorbent, the content of the adsorbent material is 80-95wt%, the content of the binder is 4-17wt%, and the content of the wetting and dispersing agent is 1-5wt%. With the proper proportion of adsorbent material, binder, and wetting and dispersing agent, the overall lithium adsorbent can take into account good structural stability, adsorption effect, and desorption effect. Preferably, the content of the adsorbent material is 85-92wt%. Preferably, the content of the binder is 5-15wt%, and more preferably 6-12wt%. Preferably, the content of the wetting and dispersing agent is 1-3wt%.
[0024] In some embodiments of the present application, the mass of the binder is 8%-12.5% of the adsorbent material. The appropriate amount of binder can ensure the high structural stability and long service life (not easy to break) of the lithium adsorbent, while also weakening its effect on reducing the adsorption capacity of the obtained lithium adsorbent.
[0025] In the embodiment of the present application, the mass of the wetting dispersant is 1%-5% of the adsorbent material. At this time, the wetting dispersant can make the distribution of the adsorbent material in the lithium adsorbent particles more uniform, the skeleton more stable, and the wettability of the lithium adsorbent particles is also improved, thereby increasing the rate of adsorption / desorption of lithium. In addition, the wetting dispersant can also dissolve more slowly in the brine, so that the porosity of the adsorbent increases slowly, further improving the adsorption efficiency of the adsorbent, and will not significantly affect the dissolution rate of the adsorbent and will not significantly reduce the service life of the adsorbent.
[0026] In some embodiments of the present application, the ratio of the mass of the adsorbent material to the sum of the masses of the binder and the wetting and dispersing agent is greater than or equal to 8:1. This is more conducive to the lithium adsorbent having both good structural stability and excellent adsorption and desorption performance. Preferably, the ratio can be in the range of (8-10):1. The ratio can specifically be 8.5, 9:1, 9.5:1, etc.
[0027] In the embodiment of the present application, the lithium adsorbent may be columnar particles. The columnar lithium adsorbent particles are simple to form and have a high degree of surface smoothness, which can prevent wear or powder loss due to mutual extrusion, friction, etc. during use, thereby reducing the amount of loss. Optionally, the particle diameter of the lithium adsorbent is 1.2mm-1.8mm and the length is 1.5mm-2.5mm. Lithium adsorbents with such morphology and suitable size can make the diffusion paths of liquids and ions more suitable, and it is easy to leave certain gaps when squeezing between adsorbents to facilitate the penetration of brine, which is beneficial to the improvement of lithium ion adsorption efficiency, and makes the ion exchange between lithium ions and water easier during the desorption process, which is convenient for reducing the delithiation temperature and the amount of desorption water to ensure that the adsorbed lithium is completely desorbed.
[0028] In step (2) of the present application, the cleaning of the lithium-rich adsorbent is mainly to wash away impurities on the surface of the lithium-rich adsorbent that has been adsorbed with lithium ions. In the embodiment of the present application, the cleaning is carried out in three steps, which include: the first cleaning, the second cleaning and the third cleaning, wherein the flow rate of the first cleaning agent during the first cleaning, the flow rate of the second cleaning agent during the second cleaning, and the flow rate of the third cleaning agent during the third cleaning are in a sequentially increasing relationship (i.e., the flow rate of the first cleaning agent < the flow rate of the second cleaning agent < the flow rate of the third cleaning agent); the amount of the second cleaning agent is greater than the amount of the first cleaning agent and the amount of the third cleaning agent. Among them, the amount of the first cleaning agent and the amount of the third cleaning agent can be equal or different.
[0029] The above-mentioned cleaning process of the lithium-rich adsorbent is divided into three steps, first slow and then fast. The flow rate during the first cleaning is low, which can prevent a large amount of high-concentration brine in the carrier containing the lithium-rich adsorbent from forming a coagulation layer under an excessively fast cleaning flow rate, making it difficult to discharge impurities in the brine, greatly reducing the cleaning effect. The flow rate during the second cleaning is moderate, and the amount of cleaning agent used is large, which can ensure sufficient cleaning time to ensure that impurities such as magnesium attached to the adsorbent can be fully dissolved and removed. The flow rate during the third cleaning is fast, and the amount of cleaning agent used is lower than the amount of cleaning agent used in the second cleaning process, which can reduce the desorption of lithium adsorbed on the lithium-rich adsorbent into the cleaning agent and reduce the lithium loss in the water washing process. Therefore, the above-mentioned specific cleaning process can clean the impurities on the surface of the lithium-rich adsorbent, so that the magnesium and lithium mass of the desorption liquid obtained by subsequent desorption is relatively low, and the amount of cleaning agent used is small, and the lithium loss rate during the cleaning process (that is, the mass ratio of lithium elements dissolved in the cleaning agent to the total lithium elements adsorbed by the lithium-rich adsorbent) is within 16%, or even 15%.
[0030] Optionally, the difference between the flow rate of the cleaning agent during the third cleaning and the flow rate of the cleaning agent during the first cleaning may be 5-9 BV / h. In this case, a better cleaning effect can be achieved.
[0031] In some embodiments of the present application, the cleaning is carried out in three steps, including: the first cleaning, the flow rate of the first cleaning agent is 3-5BV / h, and the dosage is 0.5-1BV; the second cleaning, the flow rate of the second cleaning agent is 6-8BV / h, and the dosage is 1-1.5BV; the third cleaning, the flow rate of the third cleaning agent is 9-12BV / h, and the dosage is 0.5-1BV. The use of this cleaning process can better clean the impurities on the surface of the lithium-rich adsorbent, so that the magnesium-lithium mass ratio of the desorption liquid obtained by subsequent desorption is lower, such as being reduced to below 2:1, and the lithium loss rate during the cleaning process is lower, less than 15%, which is much lower than the lithium loss level of about 20% (even 25% loss rate) caused by the fixed-speed cleaning process commonly used in the industry.
[0032] Specifically, the dosage of the first cleaning agent can be 0.6, 0.7, 0.8 or 0.9 BV, etc.; the dosage of the second cleaning agent can be 1, 1.2, 1.3, 1.4, 1.5 BV, etc.; the dosage of the third cleaning agent can be 0.6, 0.7, 0.8 or 0.9 BV, etc. Further, in order to reduce the lithium loss rate during the cleaning process, in some embodiments, the total dosage of each cleaning agent during the cleaning process is controlled not to exceed 2.5 BV.
[0033] In some embodiments, the first cleaning time is 6-20 minutes, further can be 7-15 minutes (for example, 9 minutes), the second cleaning time is 7.5-15 minutes, further can be 9-13 minutes (for example, 11 minutes), and the third cleaning time is 2.5-6.6 minutes (for example, 4 minutes). In some embodiments, in step (2), the total cleaning time can be controlled within 25 minutes, further can be within 20 minutes. In this way, while achieving a better impurity cleaning purpose, the lithium loss rate can also be reduced.
[0034] In a specific embodiment, the cleaning process specifically includes:
[0035] i) using a first cleaning agent (i.e., a first cleaning agent) to perform a first cleaning on the lithium-rich adsorbent to obtain a first cleaning solution and a first adsorbent;
[0036] ii) using a second cleaning agent (i.e., a cleaning agent for the second cleaning) to perform a second cleaning on the first adsorbent to obtain a second cleaning solution and a second adsorbent;
[0037] iii) The second adsorbent is cleaned for the third time with a third cleaning agent (i.e., a cleaning agent for the third cleaning) to obtain a third cleaning solution and a third adsorbent. The third adsorbent here is the lithium-rich adsorbent after cleaning, and the desorption in the aforementioned step (3) is also performed on it.
[0038] In the present application, the first cleaning agent, the second cleaning agent, and the third cleaning agent all contain a large amount of water, and each cleaning agent can be pure water, or recycled water (containing certain inorganic metal ion impurities), and the composition of each cleaning agent can be different. In some embodiments, the first cleaning agent, the second cleaning agent, and the third cleaning agent are all pure water. At this time, the amount of pure water is large, and the loss rate of lithium in the cleaning process will be slightly large.
[0039] In other embodiments, the first cleaning agent and the second cleaning agent are recycled water; the third cleaning agent is pure water instead of recycled water, which can be deionized water, distilled water, clean groundwater, tap water, etc. The cleaning agent for the first two cleanings is recycled water containing lithium, which can inhibit the desorption of lithium during the cleaning process. The last cleaning is pure water, which uses a small amount of pure water and can ensure a cleaner cleaning effect. Optionally, each cleaning agent does not contain organic matter, and the conductivity is less than 300μs / cm, and further the conductivity is less than 200μs / cm, preferably less than 50μs / cm.
[0040] Further, the magnesium content in the first cleaning agent, the second cleaning agent, and the third cleaning agent decreases in sequence. Optionally, the magnesium content in the first cleaning agent does not exceed 50g / L, preferably does not exceed 30g / L, and more preferably does not exceed 10g / L; the magnesium content in the second cleaning agent does not exceed 5g / L, and the magnesium content in the third cleaning agent does not exceed 100mg / L. In some embodiments, the magnesium ion content in the first cleaning agent does not exceed 50g / L, and the lithium ion content does not exceed 300mg / L. Optionally, the first cleaning agent may also include other metal ions (calcium, boron, sodium or potassium) whose concentrations do not exceed 10g / L. The magnesium ion content in the second cleaning agent does not exceed 5g / L, and the lithium ion content does not exceed 250mg / L.
[0041] In some embodiments of the present application, the unqualified desorption liquid (produced in the later stage of desorption) with a lithium concentration of no more than 250 mg / L obtained in the desorption process of step (3) can be used as the cleaning agent for the second cleaning (i.e., the second cleaning agent); in addition, the residual water in the carrier (such as the adsorption column) containing the lithium adsorbent after the desorption is completed can also be discharged as the second cleaning agent. The third cleaning liquid obtained after the third cleaning or the second cleaning liquid obtained after the second cleaning can be used as the cleaning agent for the first cleaning (i.e., the first cleaning agent). The first cleaning liquid obtained after the first cleaning can be returned and mixed into the salt lake brine. In this way, in the entire cleaning process, only pure water is used in the third cleaning, and the amount of pure water used is relatively small, which has great economic and environmental benefits for the salt lake brine lithium extraction process in water-scarce areas. Exemplarily, the second cleaning liquid generally contains magnesium ions with a concentration of no more than 50 g / L, and the concentrations of other metal ions (calcium, lithium, boron, sodium or potassium) are all no more than 10 g / L; the lithium ion concentration can further be 100-200 ppm. The third cleaning solution generally contains magnesium ions at a concentration not exceeding 10 g / L, and other metal ions (such as calcium, lithium, boron, sodium or potassium, etc.) at a concentration not exceeding 0.5 g / L; further, the lithium ion concentration is lower than 300 mg / L.
[0042] In step (3) of the present application, a lithium ion eluent (also called a lithium desorbent) is used to elute the washed lithium-rich adsorbent in order to desorb the lithium ions adsorbed on the lithium-rich adsorbent, so that the lithium ions are eluted and desorbed into the eluent to obtain a desorption liquid, so that the desorption liquid can be further processed and utilized (generally converted into a lithium carbonate product); at the same time, after the lithium is desorbed from the lithium-rich adsorbent, the lithium adsorbent can be regenerated and then used to contact with salt lake brine for adsorption and lithium extraction. In the above-mentioned lithium extraction method, steps (1)-(3) are one cycle.
[0043] In the embodiment of the present application, the temperature of the lithium ion eluent (that is, the "temperature of the desorption process") can be 30-50°C. In some embodiments (such as when the lithium adsorbent containing the above-mentioned vinylidene fluoride-chlorotrifluoroethylene copolymer and / or fluoroolefin-vinyl ether copolymer as a binder is used), the temperature can be 30-40°C, for example, 28, 30, 32, 35, 38 or 40°C, and further can be 30-35°C. Among them, the lithium ion eluent can be deionized water, distilled water, clean groundwater or tap water. Of course, it is also possible to use unqualified desorption liquid (produced in the later stage of desorption) that does not meet the lithium concentration requirements and desorb them in order from high to low lithium content to obtain the maximum amount of qualified desorption liquid containing lithium.
[0044] Optionally, the flow rate of the lithium ion eluent is 1.5-2.5 BV / h, such as 1.8 BV / h, 2 BV / h, 2.2 BV / h, etc. This can ensure that the lithium ion content in the desorption solution is high and the desorption time is not too long. Optionally, the desorption time is 2.5-4h, such as 2.8h, 3h, 3.5h, 3.8h, etc.
[0045] The method for extracting lithium from salt lakes provided in this application can effectively improve the adsorption efficiency of lithium in brine by adopting a specific flow rate change process in the adsorption stage of salt lake brine, solving the problem of difficulty in obtaining qualified desorption liquid with high lithium content at low temperature (brine generally does not freeze at a minimum of minus ten degrees Celsius in winter), and can ensure uninterrupted production all year round. The process flow of the method for extracting lithium from salt lakes is simple, the lithium extraction yield is high, and it is convenient for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 A process flow chart of a method for extracting lithium from a salt lake provided in one embodiment of the present application.
[0047] Figure 2 A process flow chart of a method for extracting lithium from a salt lake provided in another embodiment of the present application. DETAILED DESCRIPTION
[0048] The technical solutions of the embodiments of the present application are described in detail below in multiple embodiments.
[0049] The composition of the salt lake brine to be used for lithium extraction in the following examples is shown in Table 1.
[0050] Table 1
[0051]
[0052] Example 1
[0053] A method for extracting lithium from salt lakes, the process flow chart is as follows Figure 1 As shown, the specific steps include:
[0054] (1) Adsorption:
[0055] The lithium adsorbent (specifically including aluminum-based adsorbent material LiCl·2Al(OH)3·nH2O and binder-polyvinylidene fluoride, the mass ratio of the two is 9:1) is loaded into the glass adsorption column, and the loading amount is 0.9dm 3 ;
[0056] The salt lake brine to be extracted with lithium is subjected to high-speed centrifugal filtration and backwash filtration in sequence, and then is passed through an adsorption column containing the above-mentioned lithium adsorbent at a variable speed, so that the lithium ions therein are adsorbed on the lithium adsorbent and the lithium adsorbent is converted into a lithium-rich adsorbent; wherein the temperature of the adsorption process is 25°C, the brine to be adsorbed is 6 BV, a total of 5400 mL, the flow rate of the first BV of brine passing through the column (i.e., the initial flow rate) is 2.5 BV / h, the adsorption time is 24 minutes, and the flow rate of the second BV of brine is The flow rate of the brine in the first stage is 2.3BV / h, and the adsorption time is 26 minutes. The flow rate of the brine in the third BV is 2.1BV / h, and the adsorption time is 28 minutes. The flow rate of the brine in the fourth BV is 2.0BV / h, and the adsorption time is 30 minutes. The flow rate of the brine in the fifth BV is 1.8BV / h, and the adsorption time is 33 minutes. The flow rate of the brine in the sixth BV (i.e., the final flow rate) is 1.3BV / h, and the adsorption time is 38 minutes. The total adsorption time of the above adsorption process is about 3 hours.
[0057] (2) Cleaning of lithium-rich adsorbent:
[0058] The adsorption column with lithium-rich adsorbent is cleaned with clean water to wash away impurities adsorbed on the surface of the lithium-rich adsorbent; the entire cleaning process is carried out in 3 steps, the total amount of cleaning agent is 2250mL (i.e., 2.5BV), the total cleaning time is 20 minutes, specifically including:
[0059] a) First cleaning: Use the third cleaning solution (composition: Li + The content is 210mg / L, Mg 2+The content is 10g / L) as the first cleaning agent to clean the lithium-rich adsorbent, wherein the dosage of the first cleaning agent is 0.6BV, the flow rate is 4.5BV / h, and the cleaning time is 8 minutes. After the cleaning is completed, the first adsorbent and the first cleaning liquid are obtained; the first cleaning liquid can be reused and mixed with salt lake brine;
[0060] b) Second cleaning: using the unqualified desorption liquid collected from the last stage of the previous cycle (composition: Li + The content is 105mg / L, Mg 2+ The first adsorbent is cleaned with a second cleaning agent having a content of 150 mg / L, wherein the volume of the second cleaning agent is 1.3 BV (i.e., 1170 mL), the flow rate is 8.5 BV / h, and the cleaning time is 9 minutes; after the cleaning is completed, a second adsorbent and a second cleaning liquid are obtained; the second cleaning liquid has a magnesium-lithium mass ratio of 206:1, and can be collected and used as brine for re-adsorption to reduce lithium loss;
[0061] c) The third cleaning: pure water is used as the third cleaning agent for this cleaning, with a volume of 0.6BV (5400mL), a flow rate of 12BV / h, and a cleaning time of 3 minutes. After the cleaning is completed, a third adsorbent and a third cleaning liquid are obtained; the third cleaning liquid can be stored in a pre-storage tank and used as the first cleaning agent for the next cycle.
[0062] (3) Desorption:
[0063] Pure water at 50 °C was used as a lithium ion eluent to elute and desorb the third adsorbent to remove the adsorbed lithium ions. The amount of water was 3.3 BV, the flow rate was 1.7 BV / h, the desorption time was 116 min, and the first 2 BV of liquid in the desorption process was collected as a qualified desorption liquid (Li + The content is greater than 500 mg / L), and the following 1.3 BV is recovered as unqualified liquid and used as cleaning agent.
[0064] Example 2
[0065] The difference between Example 2 and Example 1 is that during the adsorption process, the flow rates of the brine are 2.8 BV / h (initial flow rate), 2.6 BV / h, 2.4 BV / h, 2.1 BV / h, 1.8 BV / h, 1.5 BV / h (final flow rate) in the order of adsorption, and the adsorption times are 21.5 min, 23 min, 25 min, 28.5 min, 33 min, 40 min, respectively. The total adsorption time is 171 minutes (i.e. 2.85 h), and the other process parameters are guaranteed to be consistent with those in Example 1.
[0066] Example 3
[0067] The difference between Example 3 and Example 1 is that: during the adsorption process, the flow rates of the brine are 2BV / h (initial flow rate), 1.8BV / h, 1.6BV / h, 1.4BV / h, 1.3BV / h, 1.2BV / h (final flow rate) in the order of adsorption, and the adsorption times are 30min, 33.3min, 37.5min, 43min, 46min, 50min, respectively. The total adsorption time is about 240min, and the other process parameters are guaranteed to be consistent with Example 1.
[0068] Example 4
[0069] The difference between Example 4 and Example 1 is that the initial flow rate of the brine is 3.5 BV / h, and the final flow rate is 2.0 BV / h. Specifically, in the order of adsorption, the flow rates of the 6 BV of brine to be adsorbed are 3.5 BV / h, 3.2 BV / h, 3.0 BV / h, 2.8 BV / h, 2.5 BV / h, and 2.0 BV / h. The adsorption time of each BV of brine is 17 min, 18.75 min, 20 min, 21.4 min, 24 min, and 30 min, respectively, and the total adsorption time is about 240 min.
[0070] Example 5
[0071] The difference between Example 5 and Example 1 is that the amount of brine to be adsorbed is 7.5 BV. During the adsorption process, the flow rate of the brine increases and decreases, and is divided into 7 different flow rate sections. The reduction amplitude of adjacent flow rate sections is 0.5 BV / h, among which the initial flow rate is 5 BV / h, and the final flow rate is 2 BV / h. The adsorption time of 1.07 BV of brine is 12.9 min, 14.3 min, 16.1 min, 18.4 min, 21.4 min, 25.7 min, and 32.1 min respectively, and the total adsorption time is about 140.9 min.
[0072] Example 6
[0073] The difference between Example 6 and Example 1 is that the flow rates of the three steps of the cleaning process are 5BV / h, 8BV / h, and 12BV / h respectively, the cleaning times are 7min, 10min, and 3min respectively, and the total cleaning time is 20 minutes. The other process parameters are guaranteed to be consistent with Example 1.
[0074] Example 7
[0075] The difference between Example 7 and Example 1 is that the cleaning process adopts a constant speed cleaning process, and the three steps of cleaning are cleaned at the same flow rate of 7.5 BV / h. The amount of cleaning agent used in each cleaning is 0.8 BV, 0.9 BV and 0.8 BV respectively, and the cleaning time is 384 seconds, 432 seconds, and 384 seconds respectively. The total time of the cleaning process is 20 minutes, and the total amount of cleaning agent is 2.5 BV, which remains unchanged.
[0076] Example 8
[0077] The difference between Example 8 and Example 1 is that the cleaning process adopts a constant speed cleaning process, the three steps of cleaning are cleaned at the same flow rate of 7.5 BV / h, the amount of cleaning agent used in each cleaning is 0.83 BV, and the cleaning time of each cleaning is 6.64 min. The total time of the cleaning process is 20 min, and the total amount of cleaning agent used is 2.5 BV, which remains unchanged.
[0078] Example 9
[0079] The difference between Example 9 and Example 1 is that the cleaning process adopts a constant speed cleaning process, the three steps of cleaning are cleaned at the same flow rate of 5BV / h, the amount of cleaning agent used in each cleaning is 0.83BV, and the cleaning time of each cleaning is 10 minutes. The total amount of cleaning agent used is 2.5BV, and the total time of the cleaning process is changed to 30 minutes.
[0080] Example 10
[0081] A method for extracting lithium from salt lakes, the process flow chart is as follows Figure 2 As shown, the difference between Example 10 and Example 1 is that during the cleaning process, the cleaning agent used in each cleaning process is pure water (unlike Example 1 in which the 1st and 2nd cleaning processes both use recycled water).
[0082] Embodiment 11
[0083] The difference between Example 11 and Example 1 is that the lithium adsorbent used is different, the desorption temperature is 30°C, and the other process parameters are the same. Specifically, the lithium adsorbent used in Example 11 includes the same adsorbent material as in Example 1, but its binder is a vinylidene fluoride-chlorotrifluoroethylene copolymer with a molecular weight of about 20,000, and also includes polyethylene glycol with a molecular weight of 10,000 as a wetting dispersant, and the mass ratio of the adsorbent material, the binder and the polyethylene glycol is 9:0.9:0.1.
[0084] Example 12
[0085] The difference between Example 12 and Example 11 is that in the method for extracting lithium from salt lakes, the binder in the lithium adsorbent used is FEVE type fluorocarbon resin.
[0086] Example 13
[0087] The difference between Example 13 and Example 11 is that in the method for extracting lithium from salt lakes, the binder in the lithium adsorbent used is a VDF-CFFE copolymer and a FEVE type fluorocarbon resin in a mass ratio of 1:1.
[0088] Embodiment 14
[0089] The difference between Example 14 and Example 11 is that the mass ratio of the adsorbent material, the binder, and the polyethylene glycol is 9.5:0.4:0.1.
[0090] Embodiment 15
[0091] The lithium adsorbent of Example 15 is different from that of Example 11 in that the molecular weight of the binder (VDF-CFFE copolymer) used is 200,000.
[0092] Example 16
[0093] The lithium adsorbent of Example 16 is different from that of Example 11 in that the molecular weight of the binder (VDF-CFFE copolymer) used is 600,000.
[0094] Embodiment 17
[0095] The lithium adsorbent of Example 17 is different from that of Example 11 in that the wetting and dispersing agent used is sodium polyacrylate with a molecular weight of 6,000.
[0096] In order to highlight the beneficial effects of the embodiments of the present application, the following comparative examples are provided.
[0097] Comparative Example 1
[0098] The difference between Comparative Example 1 and Example 1 is that the adsorption process adopts a constant-rate adsorption process, and the salt lake brine passes through the lithium adsorbent at a flow rate of 2.5 BV / h, and the adsorption time is still 3 hours.
[0099] Comparative Example 2
[0100] The difference between Comparative Example 2 and Example 1 is that: the adsorption process of step (1) adopts a constant-speed adsorption process, and the salt lake brine passes through the lithium adsorbent at a flow rate of 2.5BV / h, and the adsorption time is still 3 hours; the cleaning process of step (2) adopts a constant-speed cleaning process, and the three steps of cleaning are cleaned at the same flow rate of 7.5BV / h, and the amount of cleaning agent used in each cleaning is 0.83BV, and the cleaning time of each cleaning is 6.64min. The total time of the cleaning process is 20min, and the total amount of cleaning agent used is 2.5BV, which remains unchanged.
[0101] In order to provide strong support for the effects of the embodiments of the present application, the amount of lithium adsorption and the adsorption yield during the adsorption process of each embodiment and comparative method, the lithium loss rate during the cleaning process, the lithium content in the desorption solution and the magnesium-lithium ratio were determined. Among them, the amount of lithium adsorption is expressed by the mass ratio of the lithium element adsorbed by the adsorbent (that is, the mass difference between the lithium element in the brine after adsorption and the lithium element in the brine before adsorption) and the mass of the adsorbent, and the adsorption yield is expressed by the ratio of the mass of lithium element adsorbed by the lithium adsorbent to the mass of lithium element in the original brine. The lithium loss rate during the cleaning process is the ratio of the mass of lithium element in the cleaning solution obtained after the cleaning is completed (if there are multiple steps of cleaning, this refers to the cleaning solution obtained by the last cleaning) to the total amount of lithium adsorbed by the lithium-rich adsorbent.
[0102] The above results are summarized in Table 2 below.
[0103] Table 2 Summary of results of various embodiments and comparative examples
[0104]
[0105]
[0106] Generally, when the same adsorbent is used for lithium extraction at the same temperature, the longer the total adsorption time, the higher the adsorption efficiency. It can be seen from Table 2 that when the adsorbent is the same and the total adsorption time is the same, the adsorption efficiency of the variable speed adsorption process (Example 1) is much higher than the adsorption rate efficiency of the fixed speed adsorption process (Comparative Example 1-2). The adsorption time of Examples 2-5 is different from that of Example 1, but when the total adsorption time is short, the adsorption efficiency of Examples 2, 4, and 5 is quite high. In addition, the use of variable speed variables and a cleaning process from slow to fast can effectively reduce the lithium loss rate during the cleaning process (Examples 1 and 6); while the constant speed cleaning process (Examples 7-9), the lithium loss rate will be slightly higher, and the magnesium-lithium ratio in the obtained desorption solution will be slightly higher (the comparison between Comparative Example 2 and Comparative Example 1 is similar); in addition, the lithium loss rate of the whole process using pure water for cleaning (Example 10) is higher than the lithium loss rate when the recycled water and pure water are used for cleaning together (Example 1).
[0107] In addition, by comparing Examples 11-14 with Example 1, it can be seen that when at least one of vinylidene fluoride-chlorotrifluoroethylene copolymer and fluoroolefin-vinyl ether copolymer is used as a binder and an adsorbent containing a wetting dispersant, the desorption temperature can be lower, and the lithium ion concentration of the lithium desorption solution is substantially equivalent to that of Example 1. When the lithium ion concentration of the lithium desorption solution is equivalent, the lower the desorption temperature of the embodiment, the more energy can be saved. For salt lake areas with scarce hydropower energy, the amount of hydropower is of great significance to production costs and production capacity, especially tap water, pure water, etc., which often cost more than 3-5 times that of other areas. In addition, the difference between Examples 15-16 and Example 11 is that the molecular weight of the binder VDF-CFFE copolymer is different. The molecular weight of the binder in Examples 15-16 is in the range of 100,000-800,000. When other conditions are the same, it has a better desorption effect than Example 11 with a binder molecular weight of 20,000. The wetting and dispersing agents of Example 17 and Example 11 are different. The desorption effect of Example 17 using polyethylene glycol as the wetting and dispersing agent is slightly better than that of Example 17 using sodium polyacrylate as the wetting and dispersing agent.
[0108] In general, the lithium extraction method of the embodiment of the present application adopts a specific variable speed adsorption process, which has a high adsorption efficiency for lithium in brine, helps to achieve efficient lithium adsorption at low temperatures, and thus can ensure that a reasonable lithium desorption solution is obtained.
[0109] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A method for extracting lithium from a salt lake, characterized in that: The following steps are involved: (1) passing salt lake brine through a lithium adsorbent at a variable speed so that lithium ions in the salt lake brine are adsorbed on the lithium adsorbent to obtain a lithium-rich adsorbent; wherein the total amount of the salt lake brine to be adsorbed is 6-8 BV, the total duration of the adsorption process is 2.5-4 h, and during the adsorption process, the flow rate of the salt lake brine gradually decreases, and the difference between the initial flow rate and the final flow rate of the salt lake brine is 0.5-3 BV / h, the initial flow rate is 2.0-3.0 BV / h, and the final flow rate is 1.2-1.8 BV / h; (2) cleaning the lithium-rich adsorbent; (3) Using a lithium ion eluent to desorb lithium ions from the cleaned lithium-rich adsorbent to obtain a desorption solution.
2. The method for extracting lithium from salt lake according to claim 1, characterized in that: The cleaning includes: a first cleaning, a second cleaning and a third cleaning in sequence, and the flow rate of the first cleaning agent during the first cleaning, the flow rate of the second cleaning agent during the second cleaning, and the flow rate of the third cleaning agent during the third cleaning are in a sequentially increasing relationship; the amount of the second cleaning agent is greater than the amount of the first cleaning agent and the amount of the third cleaning agent.
3. The method for extracting lithium from salt lake according to claim 2, characterized in that: During the first cleaning, the flow rate of the first cleaning agent is 3-5 BV / h and the dosage is 0.5-1 BV; During the second cleaning, the flow rate of the second cleaning agent is 6-8 BV / h, and the dosage is 1-1.5 BV; During the third cleaning, the flow rate of the third cleaning agent is 9-12 BV / h, and the dosage is 0.5-1 BV.
4. The method for extracting lithium from salt lake according to claim 2, characterized in that: The first cleaning agent includes an aqueous solution containing magnesium ions at a concentration not exceeding 50 g / L and lithium ions at a concentration not exceeding 300 mg / L; the second cleaning agent includes an aqueous solution containing magnesium ions at a concentration not exceeding 5 g / L and lithium ions at a concentration not exceeding 250 mg / L; the third cleaning agent is pure water.
5. The method for extracting lithium from salt lake according to claim 1, characterized in that: During the lithium desorption process, the lithium ion eluent is water at a temperature of 30-50°C.
6. The method for extracting lithium from salt lake according to any one of claims 1 to 5, characterized in that: The lithium adsorbent includes an adsorbent material, a binder and a wetting and dispersing agent, wherein the binder includes at least one of vinylidene fluoride-chlorotrifluoroethylene copolymer and fluoroolefin-vinyl ether copolymer, and the wetting and dispersing agent includes one or more of polyethylene glycol, sodium polyacrylate, polyvinyl alcohol, and formaldehyde condensate.
7. The method for extracting lithium from salt lake according to claim 6, characterized in that: Based on the weight of the lithium adsorbent, the content of the adsorbent material is 80-95wt%, the content of the binder is 4-17wt%, and the content of the wetting and dispersing agent is 1-5wt%.
8. The method for extracting lithium from salt lake according to claim 6, characterized in that: The ratio of the mass of the adsorption material to the sum of the masses of the binder and the wetting and dispersing agent is greater than or equal to 8:
1.
9. The lithium adsorbent according to claim 6, characterized in that The mass of the binder is 8%-12.5% of the mass of the adsorption material.
10. The lithium adsorbent according to claim 6, characterized in that The molecular weight of the vinylidene fluoride-chlorotrifluoroethylene copolymer or the fluoroolefin-vinyl ether copolymer is 100,000-800,000.
Citation Information
Patent Citations
Method for extracting lithium from salt lake brine by adsorption method
CN101928828A
Continuous ion exchange device and method for extracting lithium from salt lake brine