Cobalt and nickel recovery method
By adjusting the pH of the acidic solution in the lithium-ion battery waste, the cobalt, nickel and aluminum form hydroxides, and the aluminum is separated under high pH, which solves the problems of cobalt and nickel loss and high processing costs in the existing technology. Efficient aluminum separation and cobalt and nickel recovery are achieved.
Patent Information
- Application Number
- CN202180069923.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-11
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-08-11
AI Technical Summary
In the existing technology, when recovering valuable metals such as cobalt and nickel from lithium-ion battery waste, adjusting the pH to separate aluminum in the form of hydroxide precipitation causes cobalt and nickel to also form hydroxides at the same time, causing process losses. And when using organic solvents to extract aluminum, there are problems such as increased processing costs and complicated operations.
Add alkali to an acidic solution containing cobalt and nickel, adjust the pH to 5 to 7, so that aluminum, cobalt and nickel form hydroxide together, and mix it with an alkali solution through solid-liquid separation, and perform aluminum leaching at a pH of 8 or above. The cobalt and nickel hydroxides are recovered and subsequently returned to the acidic solution to increase the cobalt and nickel concentration.
It achieves efficient and selective separation of aluminum from acidic solutions containing aluminum, avoids the loss of cobalt and nickel, improves the recovery rate of cobalt and nickel, reduces the separation load of aluminum, and reduces processing costs.
Smart Images

Figure CN116368249B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for efficiently separating aluminum from a solution containing cobalt and nickel and recovering cobalt and nickel. More specifically, the present invention relates to a method for efficiently separating cobalt and nickel from aluminum, which are valuable substances, from waste lithium-ion batteries (referred to as waste LIBs) and the like and recovering them. Background Art
[0002] As methods for recovering valuable metals such as cobalt and nickel from waste LIB, the methods of Patent Document 1 and Patent Document 2 are known. (I) The method of Patent Document 1 discloses the following method: dissolving the waste LIB crushed material with an acid to leach out valuable metals such as cobalt and nickel, neutralizing the leachate to precipitate aluminum, extracting cobalt and nickel from the leachate from which aluminum has been removed by solid-liquid separation into an organic solvent and separating them from phosphorus and fluorine in the residual liquid, and recovering cobalt and nickel by back-extracting them from the organic solvent. (II) Patent Document 2 discloses the following method: adding hydrogen peroxide to the acid in which the waste LIB crushed material has been impregnated to leach out cobalt, nickel, etc., and on the other hand, separating manganese in the form of residue, extracting and separating aluminum from the recovered leached liquid with an organic solvent, and recovering cobalt, nickel, etc. from the extracted liquid.
[0003] Patent Document 1: Japanese Patent Application Publication No. 2016-113672
[0004] Patent Document 2: Japanese Patent Application Publication No. 2016-186118
[0005] As described in Patent Document 1, in the method of separating aluminum in the form of hydroxide precipitation by adjusting pH, cobalt and nickel also form hydroxides at the same time, thus causing process losses. Furthermore, if the hydroxide is dissolved with acid and returned to the leachate before the hydroxide is formed to recover the above process losses, a part of the aluminum hydroxide is also dissolved at the same time, so that the aluminum hydroxide will return to the leachate, and the separation of aluminum is insufficient, so there is a problem of increased load for removing aluminum in the next process. On the other hand, in the extraction and separation of aluminum using organic solvents, since organic solvents such as PC-88A are used, there are problems such as increased processing costs and complicated operations. Summary of the invention
[0006] The present invention solves the existing problems in the above-mentioned recovery methods, etc., and improves the method of separating aluminum in the form of hydroxide precipitation, providing a recovery method that can selectively and efficiently separate aluminum from hydroxides containing cobalt and nickel that have been precipitated together with aluminum, thereby improving the recovery rate of cobalt and nickel.
[0007] The present invention is a method for recovering cobalt and nickel that solves the above-mentioned problems by the following configuration.
[0008] [1] A method for recovering cobalt and nickel, characterized in that, for an acidic solution containing cobalt, nickel and aluminum, an alkali is added to the acidic solution to adjust the pH to 5 to 7 so that aluminum forms hydroxides together with cobalt and nickel, the hydroxides recovered by solid-liquid separation are mixed with an alkali solution, the aluminum contained in the hydroxides is leached at a pH of 8 or above, and solid-liquid separation is performed, thereby recovering cobalt hydroxide and nickel hydroxide from which aluminum is separated.
[0009] [2] A method for recovering cobalt and nickel according to [1] above, wherein sodium hydroxide having a concentration of less than 1 mol / L is added to a sulfuric acid solution having a concentration of 1.5 to 2 mol / L containing cobalt and nickel and also containing aluminum, so that the pH of the solution is adjusted to 5 to 7 to generate hydroxides, the hydroxides recovered by solid-liquid separation are mixed with a sodium hydroxide solution having a concentration of 4 to 6 mol / L, the aluminum contained in the hydroxides is leached at a pH of 8 or above and a liquid temperature of 50 to 80°C, and then solid-liquid separation is performed to remove the aluminum, thereby recovering cobalt hydroxide and nickel hydroxide.
[0010] [3] A method for recovering cobalt and nickel according to [1] or [2] above, wherein the cobalt hydroxide and nickel hydroxide recovered by removing aluminum are returned to the acidic solution at the beginning of the treatment to increase the concentration of cobalt and nickel in the solution.
[0011] [4] A method for recovering cobalt and nickel according to any one of [1] to [3] above, wherein the acidic solution containing cobalt, nickel and aluminum is a liquid obtained by leaching a crushed positive electrode active material extracted from lithium ion battery waste with sulfuric acid.
[0012] According to the method of the present invention, aluminum can be efficiently and selectively separated from an acidic solution containing aluminum while containing cobalt and nickel, thereby avoiding the loss of cobalt and nickel and improving the recovery rate of cobalt and nickel. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a processing step diagram of Example 2. DETAILED DESCRIPTION
[0014] Next, a mode for carrying out the present invention will be described with reference to the drawings.
[0015] 〔Specific description〕
[0016] A method according to one embodiment of the present invention is a method for recovering cobalt and nickel, characterized in that, for an acidic solution containing cobalt, nickel and aluminum at the same time, an alkali is added to the acidic solution, the pH is adjusted to 5 to 7 so that aluminum forms hydroxides together with cobalt and nickel, the hydroxides recovered by solid-liquid separation are mixed with an alkaline solution, the aluminum contained in the hydroxides is leached at a pH of 8 or above and solid-liquid separation is performed, thereby recovering cobalt hydroxide and nickel hydroxide from which aluminum is separated.
[0017] The acidic solution containing cobalt, nickel and aluminum used in the recovery method of the present invention is, for example, a liquid obtained by leaching the positive electrode active material taken out from lithium ion battery waste with sulfuric acid. The positive electrode active material of the lithium ion battery contains lithium and also contains nickel, cobalt, manganese, etc., and a laminated material such as aluminum foil is provided inside the battery. Aluminum of the laminated material is attached to the crushed positive electrode active material taken out by crushing the lithium ion battery waste, and copper of the conducting material coexists. The leachate obtained by leaching the crushed positive electrode active material with sulfuric acid or the like contains nickel, cobalt, lithium and also aluminum and copper. Lithium is recovered from the leachate, and nickel and cobalt are further recovered.
[0018] The recovery method of the present invention can be used as a method for recovering nickel and cobalt from a crushed positive electrode active material, which is taken out from lithium ion battery waste. Specifically, for example, sulfuric acid to which hydrogen peroxide is added is used to leach the crushed positive electrode active material of lithium ion battery waste. Sodium hydrosulfide (NaHS aqueous solution) is added to the leachate to form copper sulfide precipitate from the copper in the liquid, the copper sulfide precipitate is filtered to remove the copper, sodium hydroxide (NaOH) is added to the filtrate to make the pH 2 to 4, sodium hypochlorite (NaClO aqueous solution) is added to form manganese in the liquid into manganese oxide precipitate, and solid-liquid separation is performed to remove the manganese oxide precipitate. The recovery method of the present invention can use the leachate from which copper and manganese have been removed. In addition, the recovery method of the present invention can use the leachate obtained by leaching the crushed positive electrode active material with sulfuric acid.
[0019] The acidic solution containing cobalt and nickel and aluminum used in the recovery method of the present invention is, for example, an acidic solution (sulfuric acid leaching solution (sulfuric acid solution)) obtained by leaching the positive electrode active material crushed material with sulfuric acid having a concentration of 1.5 to 2 mol / L. The recovery method of the present invention includes a step (de-Al step) of selectively removing aluminum from such an acidic solution containing cobalt and nickel and also aluminum to recover cobalt and nickel.
[0020] The above-mentioned Al removal step includes: a step of forming a hydroxide precipitate (hereinafter referred to as Al hydroxide) containing aluminum and a part of cobalt and nickel (hereinafter referred to as Al hydroxide) [Al precipitation step]; a step of leaching aluminum from the Al hydroxide [Al leaching step]; and a step of performing solid-liquid separation to separate and recover the leaching residue (Co, Ni hydroxide) from the aluminum leachate [separation and recovery step].
[0021] If an alkali is added to the above-mentioned acidic solution and the pH is adjusted to 5-7, aluminum forms hydroxide and precipitates. And, at the same time, in this pH range, a part of the cobalt and nickel in the liquid also forms hydroxide and coprecipitates with aluminum, forming a hydroxide (hereinafter referred to as Al hydroxide) containing aluminum and a part of cobalt and nickel [Al precipitation process]. Regarding the alkali added to the above-mentioned acidic solution, for example, sodium hydroxide with a concentration of less than 1 mol / L is used. When the pH of the solution is less than 5, aluminum hydroxide is not fully formed. If the pH of the solution exceeds 7, the solubility of aluminum becomes strong and remains in the liquid, so it is not preferred. The pH of the above-mentioned acidic solution is adjusted to 5-7 to form the above-mentioned Al hydroxide. A part of cobalt and nickel coprecipitates and is contained in the Al hydroxide. On the other hand, unprecipitated cobalt and nickel are dissolved in the liquid.
[0022] The Al hydroxide is recovered by solid-liquid separation and mixed with an alkaline solution, and the mixed solution is set to a pH of 8 or more, preferably 8 or more and 14 or less, and more preferably 8 or more and 12.5 or less, so that the aluminum of the Al hydroxide is leached (Al leaching step). As for the alkaline solution, for example, a sodium hydroxide solution with a concentration of 4 to 6 mol / L is used so that the pH becomes 8 or more when the Al hydroxide is mixed. Aluminum forms hydroxide at a pH below pH 7, but forms a complex [Al(OH4)(H2O)2]- at a pH above pH 8, so aluminum is leached from the Al hydroxide in a sodium hydroxide mixed solution above pH 8. The liquid temperature for leaching aluminum is preferably 50°C to 80°C. When the liquid temperature is less than 50°C, the aluminum leaching effect decreases.
[0023] On the other hand, since the cobalt and nickel contained in the Al hydroxide remain in the form of hydroxide at a pH of 8 or higher, solid-liquid separation is performed to recover the leaching residue (Co, Ni hydroxide), and the Co, Ni hydroxide contained in the leaching residue is separated from the aluminum contained in the filtrate (separation and recovery step).
[0024] In the above-mentioned Al removal step, aluminum is separated from cobalt and nickel, and cobalt and nickel coprecipitated with Al hydroxide are recovered, thereby avoiding the loss of cobalt and nickel.
[0025] By returning the recovered leaching residue (Co, Ni hydroxide) to the sulfuric acid leachate (acidic solution) at the beginning of the treatment (at least before the addition of alkali, more specifically, before the removal of copper), a sulfuric acid leachate with a higher concentration of cobalt and nickel than the sulfuric acid leachate before the return can be obtained, and by using the sulfuric acid leachate, the recovery rate of cobalt and nickel can be improved. In addition, since aluminum is not contained in the above-mentioned leaching residue (Co, Ni hydroxide), even if the leaching residue (Co, Ni hydroxide) is returned to the sulfuric acid leachate (acidic solution) at the beginning of the treatment, the aluminum concentration of the sulfuric acid leachate (acidic solution) will not increase, and the recovery treatment of cobalt and nickel can be performed without accumulating aluminum.
[0026] The “recovery rate” in the present embodiment refers to the ratio of the content of cobalt and nickel contained in the leaching residue recovered after Al leaching to the content of cobalt and nickel contained in the positive electrode active material before leaching with sulfuric acid.
[0027] Example
[0028] Next, examples of the present invention will be described in detail together with comparative examples.
[0029] The following is an example of the present invention. The aluminum removal rate is calculated by the following formula [1], and the elution rate of cobalt or nickel is calculated by the following formula [2].
[0030] Aluminum removal rate = A1 / A2 × 100 (%) [1]
[0031] [In the above formula [1], A1 is the aluminum content in the leachate obtained in the aluminum leaching step, and A2 is the aluminum content in the precipitate obtained in the Al (aluminum) precipitation step]
[0032] Cobalt or nickel elution rate = C1 / C2×100(%)[2]
[0033] [In the above formula [2], C1 is the content of cobalt or nickel in the leachate obtained in the aluminum leaching step, and C2 is the content of cobalt or nickel in the precipitate obtained in the Al precipitation step]
[0034] [Example 1]
[0035] For the liquid obtained by leaching 14.5g of positive electrode active material taken out from the waste LIB with 100mL of sulfuric acid with a concentration of 2mol / L, a sodium hydroxide solution with a concentration of 25% was added to make the pH of the leachate 5.5, and the generated hydroxide precipitate was suction filtered and solid-liquid separation was performed to recover the hydroxide precipitate (Al precipitation process). The cobalt content in the hydroxide precipitate was 9.1% by weight, the nickel content was 12.7% by weight, and the aluminum content was 25.1% by weight. 20g of the hydroxide precipitate was mixed with 200mL of sodium hydroxide solution with a concentration of 4mol / L to prepare a sodium hydroxide mixed solution with a pH of more than 8. The mixed solution was stirred at 80°C for two hours to leach aluminum (aluminum leaching process). The sodium hydroxide mixed solution was suction filtered again and solid-liquid separation was performed to recover the leached residue (separation and recovery process). As a result of analyzing the filtrate after the separation process by ICP-AES, the aluminum concentration was 2.9g / L, and no cobalt and nickel were detected. On the other hand, the composition analysis of the leached residue after the separation process by XRF showed that the cobalt content was 30.7% by weight, the nickel content was 45.8% by weight, and the aluminum content was 3.5% by weight. According to this result, the removal rate of aluminum contained in the leached residue after the separation process was 68.9% (sample No. A1). It was confirmed that the cobalt and nickel contained in the leached residue could be easily leached with sulfuric acid at a concentration of 2 mol / L.
[0036] The same treatment was performed by changing the concentration and amount of the sodium hydroxide solution in the aluminum leaching process and the liquid temperature during leaching. The results are shown in Table 1. As shown in Table 1, the concentration of the sodium hydroxide solution in the aluminum leaching process is preferably 4 to 6 mol / L, and the liquid temperature is preferably 50°C to 80°C (Sample No. A1 to A9). When the concentration of the sodium hydroxide solution is less than 2 mol / L or the liquid temperature is less than 50°C, the removal rate of aluminum contained in the leaching residue after the separation process is reduced (Sample No. A10 to A19).
[0037] [Table 1]
[0038]
[0039] (Note) De-Al residue is the leaching residue after the separation process, and De-Al leachate is the leachate after the separation process.
[0040] [Comparative Example 1]
[0041] Aluminum was leached in the same manner as in Example 1 except that sulfuric acid was used instead of the sodium hydroxide solution in the aluminum leaching step. The results are shown in Table 2 (Comparative Example: Sample No. B1, B2). As shown in Table 2, cobalt and nickel were largely leached together with aluminum during leaching with sulfuric acid, so aluminum could not be selectively leached and separated.
[0042] [Table 2]
[0043]
[0044] [Example 2]
[0045] according to Figure 1 The processing step shown processes the pulverized positive electrode active material taken out from the waste LIB.
[0046] The contents of cobalt, nickel, manganese, lithium, aluminum, etc. contained in the positive electrode active material (hereinafter referred to as the valuable metal content) are shown in Table 3. The positive electrode active material pulverized material was leached using sulfuric acid to which hydrogen peroxide was added (sulfuric acid leaching step). The valuable metal content in the sulfuric acid leaching solution (pH 0.2) is shown in Table 3. Sodium hydrosulfide (NaHS aqueous solution) was added to the sulfuric acid leaching solution to form copper sulfide precipitation in the liquid, and the copper sulfide precipitation was filtered to remove copper (Cu removal step). The valuable metal content in the Cu removal filtrate and the filtration residue (Cu-containing residue) is shown in Table 3. Sodium hydroxide (NaOH) was added to the Cu removal filtrate to make the pH 3.5, sodium hypochlorite (NaClO aqueous solution) was added to form manganese oxide precipitation in the liquid, and the manganese oxide precipitation was removed by filtration, thereby recovering the Mn removal filtrate (Mn removal step). Table 3 shows the valuable metal contents in the Mn-removed filtrate and the filtration residue (Mn-containing residue).
[0047] 25% sodium hydroxide solution was added to the Mn removal filtrate to adjust the pH to 5.5, and the resulting hydroxide precipitate was filtered and recovered [Al precipitation process]. 4 mol / L sodium hydroxide solution was mixed into the hydroxide precipitate to adjust the pH to above 8, and stirred at 80°C for two hours to leach aluminum. Next, the filtrate was filtered to recover the filtration residue (Co, Ni residue), which was separated from the filtrate (Al leaching solution) [Al leaching process, separation and recovery process]. The valuable metal contents in the filtration residue and the filtrate are shown in Table 3.
[0048] [Table 3]
[0049]
[0050] [Example 3]
[0051] In Example 2, after the treatment of returning the filtration residue (containing Co and Ni residue) recovered in the separation and recovery step to the sulfuric acid leaching solution at the start of the treatment was repeated 10 times, the filtrate (containing Co and Ni filtrate) obtained by solid-liquid separation of aluminum hydroxide precipitated in the Al precipitation step was used, and the concentration of the filtrate was adjusted, and cobalt and nickel were extracted and recovered using a solvent (2-ethylhexyl phosphonic acid mono-2-ethylhexyl ester, a solvent obtained by mixing 20 volume % of PC-88A (trade name) and 80 volume % of kerosene). The recovery rate of cobalt was 93.3%, and the recovery rate of nickel was 94.4%.
[0052] On the other hand, the filtrate (containing Co and Ni filtrate) obtained by solid-liquid separation of aluminum hydroxide precipitated in the Al precipitation step was used to recover cobalt and nickel by solvent extraction in the same manner as above, without returning the filtration residue (containing Co and Ni residue) recovered in the separation and recovery step to the sulfuric acid leaching solution at the start of the treatment. The recovery rate of cobalt was 59.3%, and the recovery rate of nickel was 64.4%, and the loss of cobalt and nickel was large.
Claims
1. A method for recovering cobalt and nickel, which is a method for recovering cobalt and nickel coprecipitated with aluminum hydroxide, characterized in that: For an acidic solution containing cobalt and nickel and also containing aluminum, an alkali is added to the acidic solution to adjust the pH to 5 to 7 so that aluminum forms hydroxide together with a part of the cobalt and nickel in the acidic solution, and after obtaining aluminum hydroxide contained by coprecipitation of the above part of cobalt and nickel, a sodium hydroxide solution with a concentration of 4 to 6 mol / L is mixed with the above aluminum hydroxide recovered by solid-liquid separation, and the liquid temperature is adjusted to 50 to 80°C and stirred, so that aluminum can form a complex [Al(OH4)(H2O)2] at a pH of pH 8 or above. - , so that the aluminum contained in the above-mentioned aluminum hydroxide is leached and solid-liquid separation is performed, thereby recovering and separating the cobalt hydroxide and nickel hydroxide of the aluminum.
2. The method for recovering cobalt and nickel according to claim 1, wherein: Sodium hydroxide having a concentration of less than 1 mol / L is added to a sulfuric acid solution having a concentration of 1.5 to 2 mol / L, which is the acidic solution containing cobalt, nickel and aluminum, so that the pH of the solution is adjusted to 5 to 7 to generate the aluminum hydroxide. The aluminum hydroxide recovered by solid-liquid separation is mixed with the sodium hydroxide solution to leach the aluminum contained in the aluminum hydroxide. Then, solid-liquid separation is performed to remove the aluminum, thereby recovering the cobalt hydroxide and the nickel hydroxide.
3. The method for recovering cobalt and nickel according to claim 1 or 2, wherein: The cobalt hydroxide and the nickel hydroxide recovered by removing aluminum are returned to the acid solution at the start of the treatment to increase the concentrations of cobalt and nickel in the acid solution.
4. The method for recovering cobalt and nickel according to any one of claims 1 to 3, wherein: The acidic solution containing cobalt, nickel and aluminum is a liquid obtained by leaching a pulverized positive electrode active material extracted from lithium ion battery waste with sulfuric acid.