A positive electrode material precursor and its preparation method and application

By sintering and treating composite metal oxides of nickel, cobalt, manganese and aluminum under an oxygen-containing atmosphere, a positive electrode material with low cation mixing rate was prepared, which solved the problem of difficult removal of impurity ions in the prior art and improved the performance of the battery and productivity.

CN116375106BActive Publication Date: 2024-11-15NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
0 Cites 0 Cited by

Patent Information

Application Number
CN202310345963.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-11-15
Estimated Expiration
2043-03-31

Smart Images

  • Figure CN116375106B_ABST
    Figure CN116375106B_ABST
Patent Text Reader

Abstract

The present invention provides a positive electrode material precursor and a preparation method and application thereof. The positive electrode material precursor comprises a compound shown in Formula 1; Ni a Co b Mn c Al d O n Formula 1; wherein 0<a≤0.98, 0≤b≤0.98, 0≤c≤0.98, 0≤d≤0.2, 0.5≤n≤1.5, and at least two of b, c and d are not zero at the same time; the mass fraction of nickel oxide in the positive electrode precursor is W NixOy , 50%*a*M NixOy / M 总 ≤W NixOy <100%*a*M NixOy / M 总 ; The mass fraction of elemental Ni in the cathode material precursor is W Ni , 0<W Ni ≤50%*a*M Ni / M 总 The special composition of the cathode material precursor is conducive to the preparation of cathode materials with low cation mixing rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a pole piece material, in particular to a positive electrode material precursor and a preparation method and application thereof, belonging to the technical field of secondary batteries. Background Art

[0002] Nickel-cobalt-manganese (NCM) ternary cathode material is a material that combines the properties of lithium cobalt oxide, lithium nickel oxide and lithium manganese oxide. It has the characteristics of high specific capacity, long cycle life, low toxicity and low cost. It is currently the most widely used cathode material.

[0003] At present, ternary cathode materials are mainly prepared by coprecipitation-high temperature solid phase method, which specifically includes: preparing a mixed system containing ternary cathode precursors by coprecipitation method, and then repeatedly washing the mixed system to remove impurity ions (such as Na + 、SO 4 2- and Cl - ), a ternary positive electrode precursor is obtained, and then the ternary positive electrode precursor is mixed with a lithium source and sintered to obtain a ternary positive electrode material. Since the removal of impurity ions requires repeated washing of the mixed system, not only the operation steps are complicated, but also the impurity removal is not thorough, so that the positive electrode material precursor also includes impurity ions. When the positive electrode material precursor including impurity ions is used to prepare the positive electrode material, it is easy to cause cation mixing, so that the cation mixing rate of the positive electrode material is high. Summary of the invention

[0004] The invention provides a positive electrode material precursor, the special composition of which is conducive to preparing a positive electrode material with a low cation mixing rate.

[0005] The present invention provides a method for preparing a positive electrode material precursor. The method has a simple preparation process and low preparation cost, and can prepare the positive electrode material precursor.

[0006] The present invention provides a positive electrode material, which is prepared by the positive electrode material precursor mentioned above and thus has a lower cation mixing rate.

[0007] The present invention provides a battery, comprising the positive electrode material, and thus having excellent discharge capacity and cycle performance.

[0008] The present invention provides a positive electrode material precursor, wherein the positive electrode material precursor comprises a compound shown in Formula 1;

[0009] Ni a Co b Mn c Al d O n Formula 1;

[0010] Wherein, 0<a≤0.98, 0≤b≤0.98, 0≤c≤0.98, 0≤d≤0.2, 0.5≤n≤1.5, and b, c and d are not zero at the same time;

[0011] In the X-ray diffraction spectrum, the positive electrode material precursor has a diffraction peak of nickel oxide and a diffraction peak of elemental Ni, and the mass fraction of nickel oxide in the positive electrode material precursor is W NixOy , 50%*a*M NixOy / M 总 ≤W NixOy <100%*a*M NixOy / M 总 ; The mass fraction of elemental Ni in the positive electrode material precursor is W Ni , 0<W Ni ≤50%*a*M Ni / M 总 ;

[0012] M NixOy is the molar mass of NixOy, M Ni is the molar mass of Ni, M 总 is the molar mass of the cathode material precursor.

[0013] The positive electrode material precursor as described above, wherein the intensity I(012) of the 012 diffraction peak of nickel oxide and the intensity I(101) of the 101 diffraction peak of nickel oxide satisfy: I(012) / I(101)=1.0-2.0; and,

[0014] The intensity I(012) of the 012 diffraction peak of nickel oxide and the intensity I(background) of the background satisfy: I(012) / I(background)≤25.

[0015] The positive electrode material precursor as described above, wherein b>0, the positive electrode material precursor has a diffraction peak of single substance Co, and the mass fraction of single substance Co in the positive electrode material precursor is W Co , 0<W Co ≤50%*b*M Co / M 总 , M Co is the molar mass of Co.

[0016] The positive electrode material precursor as described above, wherein when b>0, the positive electrode material precursor has a diffraction peak of cobalt oxide, and the mass fraction of cobalt oxide in the positive electrode precursor is W CoxOy , 50%*b*M CoxOy / M 总 ≤W CoxOy <100%*b*M CoxOy / M 总, M CoxOy is the molar mass of CoxOy.

[0017] The positive electrode material precursor as described above, wherein c>0, has a diffraction peak of manganese oxide.

[0018] The positive electrode material precursor as described above, wherein d>0, has a diffraction peak of aluminum oxide.

[0019] The positive electrode material precursor as described above, wherein the Dv50 of the positive electrode material precursor is 3-8 μm.

[0020] The present invention provides a method for preparing the positive electrode material precursor as described above, which comprises: sintering a raw material system in a reaction container under an oxygen-containing atmosphere to obtain the positive electrode material precursor;

[0021] Wherein, the raw material system includes at least two of a nickel source, a cobalt source, a manganese source and an aluminum source;

[0022] The flow rate of the oxygen-containing atmosphere is 5-20 L / min; the volume fraction of oxygen in the oxygen-containing atmosphere is 21%-100%;

[0023] The volume of the raw material system accounts for 5-10% of the volume of the reaction container.

[0024] In the method for preparing the positive electrode material precursor as described above, the temperature of the sintering treatment is 250-700°C.

[0025] In the method for preparing the positive electrode material precursor as described above, the sintering treatment time is 1-12 hours.

[0026] The present invention provides a positive electrode material, wherein the positive electrode material is prepared by the positive electrode material precursor as described above.

[0027] The positive electrode material as described above, wherein an X-ray diffraction test is performed on the positive electrode material, and the ratio of the unit cell c-axis length to the a-axis length of the positive electrode material is c' / a'>4.93, and the cation mixing rate is <0.03.

[0028] The present invention provides a battery, comprising the positive electrode material as described above.

[0029] The battery as described above, wherein the battery is charged and discharged in a voltage window of 2.8V-4.25V, and the first discharge capacity at a rate of 0.2C is greater than 180.0mAh / g; after 50 cycles at a rate of 1C, the capacity retention rate is greater than 93%.

[0030] The cathode material precursor of the present invention has a special composition, and when used for preparing the cathode material, it can reduce the cation mixing rate of the cathode material.

[0031] The preparation method of the positive electrode material precursor of the present invention obtains the above-mentioned positive electrode material precursor by sintering the raw material system under specific conditions. The preparation method has a simple preparation process, uses less raw materials, has low production cost, and is suitable for wide promotion and application.

[0032] The positive electrode material of the present invention is prepared by the positive electrode material precursor mentioned above, and therefore has a lower cation mixing rate.

[0033] The battery of the present invention includes the above-mentioned positive electrode material and thus has excellent discharge capacity and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 is the XRD diagram of the cathode material precursor in Example 1 of the present invention;

[0036] Figure 2 is the XRD pattern of the cathode material precursor in Example 6 of the present invention;

[0037] Figure 3 This is the XRD diagram of the positive electrode material precursor in Comparative Example 1 of the present invention;

[0038] Figure 4 XRD diagram of the positive electrode material obtained from the positive electrode material precursor in Example 1 of the present invention;

[0039] Figure 5 XRD diagram of the positive electrode material obtained from the positive electrode material precursor in Example 6 of the present invention;

[0040] Figure 6 This is the XRD diagram of the positive electrode material obtained from the positive electrode material precursor in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] A first aspect of the present invention provides a positive electrode material precursor, the positive electrode material precursor comprising a compound shown in Formula 1;

[0043] Ni a Co b Mn c Al d O n Formula 1;

[0044] Wherein, 0<a≤0.98, 0≤b≤0.98, 0≤c≤0.98, 0≤d≤0.2, 0.5≤n≤1.5, and b, c and d are not zero at the same time;

[0045] In the X-ray diffraction spectrum, the cathode material precursor has diffraction peaks of nickel oxide and elemental nickel, and the mass fraction of nickel oxide in the cathode material precursor is W. NixOy , 50%*a*M NixOy / M 总 ≤W NixOy <100%*a*M NixOy / M 总 ; The mass fraction of elemental Ni in the cathode material precursor is W Ni , 0<W Ni ≤50%*a*M Ni / M 总 ;

[0046] M NixOy is the molar mass of NixOy, M Ni is the molar mass of Ni, M 总 is the molar mass of the cathode material precursor.

[0047] The compound in Formula 1 of the present invention is a composite metal oxide comprising at least two metal elements. For example, the compound in Formula 1 can be a composite metal oxide comprising nickel and cobalt, or a composite metal oxide comprising nickel, cobalt, manganese and aluminum.

[0048] The cathode material precursor of the present invention also has characteristic peaks of nickel oxide and characteristic peaks of elemental Ni in the X-ray diffraction spectrum, so it is inferred that the cathode material precursor of the present invention contains nickel oxide and elemental Ni. It can be understood that part of the Ni element in the present invention exists in the form of nickel oxide, and part exists in the form of elemental Ni.

[0049] The inventors have studied the content of nickel oxide in the positive electrode material precursor. NixOy And the content of elemental Ni W Ni After analysis, it was found that 50%*a*M NixOy / M 总 ≤W NixOy <100%*a*M NixOy / M 总 ; The mass fraction of elemental Ni in the cathode material precursor is W Ni , 0<W Ni ≤50%*a*M Ni / M 总 .

[0050] The present invention does not limit Ni x O y The specific molecular formula of can be used as long as the valence can be balanced. For example, Ni x O y It can be NiO and / or Ni 2 O 3 .

[0051] The positive electrode material precursor of the present invention includes a specific content of elemental Ni and nickel oxide. When calcined with a lithium source to prepare a positive electrode material, the positive electrode material precursor of the present invention can fully react with the lithium source to reduce the mixing of lithium elements and metal elements (especially lithium-nickel mixing), thereby improving the capacity and cycle performance of the positive electrode material; at the same time, a certain content of elemental Ni can increase the looseness of the positive electrode material precursor seed, which is more conducive to the calcination of the positive electrode material precursor and the lithium source, thereby forming a positive electrode material with excellent performance.

[0052] In the present invention, in the XRD spectrum, the positions of 2θ of 43°-45°, 50°-52° and 75°-77° have characteristic peaks of elemental nickel (the three peaks are respectively from strong to weak). In the XRD spectrum, the position of 2θ of 42°-44° has the 012 characteristic peak of nickel oxide, and the position of 2θ of 36°-38° has the 101 characteristic peak of nickel oxide.

[0053] In some embodiments of the present invention, when the intensity I(012) of the 012 characteristic peak of nickel oxide and the intensity I(101) of the 101 characteristic peak of nickel oxide satisfy: I(012) / I(101)=1.0-2.0; and,

[0054] When the intensity I(012) of the 012 characteristic peak of nickel oxide and the intensity I(background) of the background satisfy: I(012) / I(background)≤25, the degree of crystallization of the positive electrode material precursor is high, and the positive electrode material precursor is used to prepare a positive electrode material with a low cation mixing rate.

[0055] In the present invention, I (background) refers to the background intensity (target baseline and noise) of XRD test.

[0056] Furthermore, I(012) / I(101)=1-1.8, the higher the degree of crystallization of the positive electrode material precursor, the more helpful it is to obtain a positive electrode material with a low cation mixing rate, I(012) / I(background)=1-20, the higher the degree of crystallization of the positive electrode material precursor, the more helpful it is to obtain a positive electrode material with a low cation mixing rate.

[0057] In some embodiments of the present invention, b>0, the cathode material precursor has a diffraction peak of single substance Co, and the mass fraction of single substance Co in the cathode material precursor is W Co , 0<W Co ≤50%*b*M Co / M 总 , M Co is the molar mass of Co.

[0058] In the present invention, part of the Co element exists in the form of cobalt oxide, and part exists in the form of Co element. In the XRD spectrum, 2θ has characteristic peaks of elemental cobalt at 43°-45°, 50°-52° and 74°-76° (three strong peaks from strong to weak, respectively). It can be understood that when the compound of Formula 1 has a Co element, the positive electrode material precursor can also have a specific content of Co element. Similar to the technical effect of elemental Ni with a specific content, when the positive electrode material precursor has a specific content of elemental Co, a positive electrode material with better comprehensive performance can be obtained.

[0059] In some embodiments of the present invention, b>0, the cathode material precursor has a diffraction peak of cobalt oxide, and the mass fraction of cobalt oxide in the cathode precursor is W CoxOy , 50%*b*M CoxOy / M 总 ≤W CoxOy <100%*b*M CoxOy / M 总 , M CoxOy is the molar mass of CoxOy.

[0060] In the present invention, in the XRD spectrum, the positions of 2θ of 41°-43°, 35°-37° and 63°-65° have characteristic peaks of cobalt oxide (the three peaks are respectively from strong to weak). It can be understood that the compound shown in Formula 1 contains the Co element, and the XRD diffraction spectrum of the positive electrode material precursor also has characteristic peaks of cobalt oxide. It can be inferred that the positive electrode material precursor may also contain a specific content of cobalt oxide. The present invention does not limit Co x O y The specific molecular formula of can be used as long as the valence can be balanced. For example, Co x O y It can be CoO and / or Co 2 O 3 .

[0061] In some embodiments of the present invention, c>0, the cathode material precursor has a diffraction peak of manganese oxide; and / or,

[0062] d>0, the cathode material precursor has a diffraction peak of aluminum oxide.

[0063] In the present invention, in the XRD spectrum, the positions of 2θ of 18°-20°, 44°-46° and 36°-38° have characteristic peaks of manganese oxide (the three strongest peaks are from strong to weak); the positions of 2θ of 44°-46°, 65°-67° and 36°-38° have characteristic peaks of aluminum oxide (the three strongest peaks are from strong to weak).

[0064] It can be understood that the compound shown in Formula 1 contains the Mn element, and the XRD diffraction spectrum of the positive electrode material precursor also has a characteristic peak of manganese oxide. It can be inferred that the positive electrode material precursor may also contain a specific content of manganese oxide (when the content of the Mn element in the positive electrode precursor is extremely small, it will be difficult to observe the characteristic peak of manganese oxide in the XRD spectrum, and other detection methods can be used for detection); and / or,

[0065] The compound shown in Formula 1 contains Al element, and the XRD diffraction spectrum of the positive electrode material precursor also has characteristic peaks of aluminum oxide. It can be inferred that the positive electrode material precursor may also contain a specific content of manganese oxide. The positive electrode material precursor may also contain a specific content of aluminum oxide.

[0066] The positive electrode material precursor of the present invention is a loose fine particle, and its appearance can be black, brown, yellow or reddish brown. The larger the particle size of the positive electrode material precursor, the higher the degree of crystallization of the positive electrode material precursor. The present invention can further promote the reaction of the positive electrode material precursor with the lithium source and improve the comprehensive performance of the positive electrode material by specifically selecting the particle size of the positive electrode material precursor.

[0067] In some embodiments of the present invention, when the Dv50 of the positive electrode material precursor is 3-8μm, a positive electrode material with a suitable particle size can be obtained at a lower calcination temperature. The lower calcination temperature not only helps to save energy consumption and reduce production costs, but also helps to reduce the volatilization of lithium sources, reduce excessive mixing of lithium elements and metal elements (especially lithium-nickel mixing), and improve the comprehensive performance of the positive electrode material.

[0068] The second aspect of the present invention provides a method for preparing the positive electrode material precursor, which comprises: sintering the raw material system in a reaction container under an oxygen-containing atmosphere to obtain the positive electrode material precursor;

[0069] Wherein, the raw material system includes at least a nickel source, and the raw material system also includes at least one of a cobalt source, a manganese source and an aluminum source;

[0070] The flow rate of the oxygen-containing atmosphere is 5-20 L / min; the volume fraction of oxygen in the oxygen-containing atmosphere is 21%-100%;

[0071] The volume of the raw material system accounts for 5-10% of the volume of the reaction container.

[0072] Specifically, the preparation method of the positive electrode material precursor of the present invention may include: sintering a specific volume of a raw material system in an oxygen-containing atmosphere with an oxygen volume fraction of 21-100%, and in a reaction vessel of a specific volume. During the sintering process, a portion of the nickel source in the raw material system will be oxidized to form nickel oxide, and a portion will be reduced to form elemental Ni, while the cobalt source, manganese source and aluminum source will be oxidized, thereby obtaining the above-mentioned positive electrode material precursor of the present invention.

[0073] The present invention does not impose any particular limitation on the oxygen-containing atmosphere, as long as the volume fraction of oxygen in the oxygen-containing atmosphere is 21-100%. In some embodiments, the oxygen-containing atmosphere can be air or oxygen.

[0074] In the present invention, since the reduction temperatures of manganese oxide and aluminum oxide are about 1100° C. respectively, they are usually not easily reduced. Therefore, when the compound shown in Formula 1 contains Mn, there is no single substance Mn in the positive electrode material precursor, and when the compound shown in Formula 1 contains Al, there is no single substance Al in the positive electrode material precursor. Nickel oxide and cobalt oxide are easily reduced. Therefore, when the compound shown in Formula 1 contains Co, the positive electrode material precursor may include single substance Co.

[0075] In the present invention, the metal source can be any compound containing the metal commonly used in the art, for example, the metal source can be selected from at least one of oxides, chlorides, sulfates, organic acid salts and nitrates containing the metal. Exemplarily, the nickel source can be selected from at least one of oxides, chlorides, sulfates, organic acid salts and nitrates containing the nickel element.

[0076] In the present invention, at least two of the nickel source, manganese source, cobalt source and aluminum source can be ball-milled and mixed to obtain a uniformly dispersed raw material system with uniform particle size, thereby promoting the sintering process and improving the comprehensive performance of the positive electrode material. The present invention does not particularly limit the specific method of ball milling and mixing, and any ball milling and mixing method commonly used in the art can be selected. In some embodiments, a planetary ball mill can be used for ball milling and mixing.

[0077] The method for preparing a positive electrode material precursor of the present invention can prepare the positive electrode material precursor mentioned above. When the obtained positive electrode material precursor is used to prepare a positive electrode material, the lithium-nickel mixing of the positive electrode material can be reduced, and the comprehensive performance of the positive electrode material can be improved. Compared with the method for preparing a positive electrode material precursor by coprecipitation, the method for preparing a positive electrode material precursor of the present invention does not require the addition of a precipitant and a complexing agent, and does not require washing and filtering, has simple raw materials, a simple preparation process, can significantly save production costs, and has excellent economic benefits.

[0078] The present invention does not specifically limit the specific method of sintering treatment, and the sintering treatment can be carried out by using the sintering method commonly used in the art. In the present invention, the specific process of sintering treatment can be further selected to improve the crystallization degree of the raw material system, thereby improving the comprehensive performance of the positive electrode material.

[0079] In some embodiments of the present invention, the sintering temperature is 250-700° C.; and / or,

[0080] When the sintering time is 1-12 hours, the crystallization degree of the raw material system can be improved while saving energy, thereby improving the comprehensive performance of the positive electrode material.

[0081] A third aspect of the present invention provides a positive electrode material, which is prepared by the positive electrode material precursor mentioned above.

[0082] In the present invention, the positive electrode material precursor can be calcined with a lithium source to obtain a positive electrode material; or the positive electrode material precursor can be prepared using the preparation method of the positive electrode material precursor, and the positive electrode material precursor can be calcined with a lithium source to obtain a positive electrode material.

[0083] In the present invention, when the positive electrode material precursor containing a metal element is calcined with a lithium source, the metal element will first be oxidized into an oxide and then react with the lithium source. The present invention uses a positive electrode material precursor containing a specific content of a metal element and a lithium source for calcination, which can not only make the positive electrode material precursor fully react with the lithium source, reduce the mixing of lithium elements and metal elements (especially lithium nickel mixing), so as to improve the capacity and cycle performance of the positive electrode material; and a certain content of elemental Ni can increase the looseness of the positive electrode material precursor seed, which is more conducive to the calcination of the positive electrode material precursor and the lithium source, thereby forming a positive electrode material with excellent performance.

[0084] In some embodiments, the ratio of the total molar content of the metal elements in the positive electrode material precursor to the molar content of the lithium element in the lithium source may be 1:(1-1.5);

[0085] The temperature of the calcination treatment can be 650-1000°C;

[0086] The calcination treatment may be performed in an oxygen-containing atmosphere.

[0087] The present invention does not impose any particular limitation on the lithium source, and it may be any lithium-containing compound commonly used in the art.

[0088] In some embodiments of the present invention, an X-ray diffraction test is performed on the positive electrode material, and the ratio of the c-axis length to the a-axis length of the unit cell of the positive electrode material is c' / a'>4.93, and the cation mixing rate is <0.03.

[0089] A fourth aspect of the present invention provides a battery comprising the above-mentioned positive electrode material.

[0090] In practical applications, the positive electrode material can be prepared into a positive electrode sheet, and the positive electrode sheet can be used to prepare a battery. Since the battery of the present invention includes the positive electrode material, it has excellent discharge capacity and cycle performance.

[0091] In some embodiments of the present invention, the battery is charged and discharged in a voltage window of 2.8V-4.25V, and the first discharge capacity at a rate of 0.2C is greater than 180.0mAh / g; after 50 cycles at a rate of 1C, the capacity retention rate is greater than 93%.

[0092] The technical solution of the present invention will be further explained below in conjunction with specific embodiments.

[0093] Example 1

[0094] The positive electrode material precursor of this embodiment is prepared by a method comprising the following steps:

[0095] Adding a nickel source, a cobalt source and a manganese source into a planetary ball mill, performing ball milling mixing to obtain a mixed system, placing the mixed system into a sagger, and placing the mixed system into an atmosphere furnace for sintering treatment to obtain a positive electrode material precursor;

[0096] The nickel source is nickel citrate, the cobalt source is cobalt citrate, and the manganese source is manganese citrate; in the mixed system, the molar ratio of nickel element, cobalt element and manganese element is 1:1:1;

[0097] The sintering temperature was 550°C and the sintering time was 6 h. The flow rate of the oxygen-containing atmosphere in the atmosphere furnace was 10 Lpm.

[0098] The volume of the raw material system accounts for 8.5% of the volume of the atmosphere furnace.

[0099] The cathode material precursor was subjected to XRD test, using a copper target as an excitation source, a test angle of 2θ = 10°-90°, and a scanning speed of 1° / min to obtain an XRD spectrum. Figure 1 is the XRD diagram of the cathode material precursor in Example 1 of the present invention, according to Figure 1 Compare the corresponding single substance spectra, and the type of single substance can be determined by the position of the three strong peaks corresponding to the standard PDF card. Use the refinement software to perform quantitative calculation of the phase and calculate the proportion of the single substance in the precursor, so as to obtain the mass fraction of nickel and cobalt in the cathode material precursor;

[0100] The particle size of the cathode material precursor was measured using a Malvern laser particle size analyzer. The test results are shown in Table 1.

[0101] Example 2-22

[0102] The preparation method of the positive electrode material precursor of Example 2-22 is basically the same as that of Example 1, except that the process parameters are different. The process parameters are shown in Table 1;

[0103] Figure 2 This is the XRD diagram of the positive electrode material precursor in Example 6 of the present invention.

[0104] Comparative Example 1

[0105] The positive electrode material precursor of this comparative example is prepared by a method comprising the following steps:

[0106] 1) simultaneously feeding a mixed salt solution including nickel sulfate, cobalt sulfate and manganese sulfate, a sodium hydroxide aqueous solution and an ammonia aqueous solution into a first reaction kettle containing a base liquid through a metering pump at a uniform speed to carry out a first reaction, and stopping feeding when the material in the first reaction kettle reaches full, to obtain a slurry containing positive electrode material precursor seed crystals;

[0107] Wherein, in the mixed salt solution, the molar ratio of nickel element, manganese element and cobalt element is 8:1:1, the molar content of the metal element is 2 mol / L, and the flow rate of the solution is 350 L / h;

[0108] In the sodium hydroxide aqueous solution, the mass percentage of sodium hydroxide is 30%;

[0109] In the ammonia solution, the mass percentage of ammonia is 18%;

[0110] In the base solution, the concentration of free ammonia is 4 g / L and the concentration of sodium sulfate is 1.7 mol / L;

[0111] In the first reaction, the temperature was 44°C, the pH was 11, and the stirring speed was 200 rpm;

[0112] 2) filtering and washing the slurry obtained in step 1) to obtain precursor seed crystals, transferring the precursor seed crystals to a second reactor, adjusting the pH of the slurry in the second reactor to 11, and adjusting the concentration of free ammonia in the slurry in the second reactor to 9 g / L;

[0113] The mixed salt solution, sodium hydroxide aqueous solution and ammonia aqueous solution having the same concentration as in step 1) are simultaneously pumped into the second reaction kettle at a uniform speed through a metering pump to carry out a second reaction. When the material in the second reaction kettle reaches a target particle size, the feeding is stopped to obtain a slurry containing a positive electrode material precursor;

[0114] The slurry containing the positive electrode material precursor is filtered, washed, dried, batch mixed, sieved, impurity-removed and packaged to obtain a positive electrode material precursor having a molar ratio of nickel, cobalt and manganese elements of 8:1:1;

[0115] In the second reaction, the reaction temperature was 50°C, the stirring speed was 150 rpm, and the pumping speed of the mixed salt solution was 280 L / h;

[0116] Figure 3 This is the XRD diagram of the positive electrode material precursor in Comparative Example 1 of the present invention.

[0117] Comparative Example 2

[0118] The preparation method of the positive electrode material precursor of this comparative example is basically the same as that of Example 1, except that;

[0119] The flow rate of the oxygen-containing atmosphere in the atmosphere furnace is 30 Lpm, and other parameters are shown in Table 1.

[0120] Test example

[0121] 1. Cathode materials

[0122] The positive electrode material is prepared by using the positive electrode material precursor in each embodiment and comparative example, specifically comprising:

[0123] The cathode material precursor and lithium hydroxide monohydrate are mixed in a high-speed mixer to obtain a mixture, the mixture is placed in a box furnace in an oxygen atmosphere for calcination, then naturally cooled to room temperature, crushed and sieved to obtain the cathode material;

[0124] Wherein, in the mixture, the ratio of the total molar content of the metal elements in the positive electrode material precursor to the molar content of the lithium element in the lithium hydroxide monohydrate is 1:1.01;

[0125] The calcination temperature is 800°C and the time is 16 hours.

[0126] The positive electrode material was subjected to XRD test and the XRD refinement results were analyzed. The results are shown in Table 1;

[0127] Figure 4 XRD diagram of the positive electrode material obtained from the positive electrode material precursor in Example 1 of the present invention; Figure 5 XRD diagram of the positive electrode material obtained from the positive electrode material precursor in Example 6 of the present invention; Figure 6 This is the XRD diagram of the positive electrode material obtained from the positive electrode material precursor in Comparative Example 1 of the present invention.

[0128] 2. Battery

[0129] The positive electrode materials prepared in part 1 are used to prepare button-type half-cells respectively. The button-type half-cells are prepared by a method comprising the following steps:

[0130] The positive electrode material, conductive carbon black SP (particle size 40 nm) and PVDF (molecular weight 900,000) were dissolved in n-methyl-1,2-pyrrolidone solvent (NMP) at a mass ratio of 90:5:5 and placed in a dry room (dew point -45°C, room size 15m 2 ) to obtain a uniform positive electrode slurry, which was coated on the surface of an aluminum foil (the thickness of the aluminum foil was 12 μm and the purity was 99.5%), and cut into a flat plate with a diameter of 12 mm to form a mass load of 8.5 ± 0.15 mg / cm 2 The positive electrode;

[0131] A 2032-type button-type half-cell was assembled in an argon-filled glove box (water and oxygen contents were both less than 0.1 ppm) using a 11 mm diameter lithium metal disc (0.3 mm thickness, 99.9% purity) as the negative electrode and an electrolyte;

[0132] The electrolyte includes LiPF 6 , ethyl carbonate and diethylene carbonate, among which LiPF 6 The concentration of 1M, the volume ratio of ethyl carbonate to diethylene carbonate is 1:1, and the H 2O content <10ppm.

[0133] 3. Battery comprehensive performance test

[0134] The following tests were performed on the batteries obtained from the two parts, and the test results are shown in Table 1;

[0135] 1) Cycle performance test

[0136] The battery was charged at 1C and discharged at 1C. The battery was charged and discharged in cycles at a cut-off current of 0.05C and an ambient temperature of 25℃±2℃. The voltage range was 2.5V-4.25V. The capacity retention rate of the battery was calculated after 50 cycles.

[0137] The capacity retention rate is the ratio of the discharge capacity in the 50th week to the discharge capacity in the first week.

[0138] 2) Discharge capacity

[0139] The battery test is carried out at 0.2C charge and discharge to test the gram capacity, and the test voltage range is 2.5V-4.25V.

[0140] It can be seen from the embodiments and comparative examples that the positive electrode material prepared using the positive electrode material precursor of the present invention has a lower cation mixing rate, and the obtained battery has more excellent cycle performance and capacity, and the preparation method of the positive electrode material precursor of the present invention is simple and suitable for wide promotion and application.

[0141] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

[0142]

[0143]

[0144]

Claims

1. A cathode material precursor, characterized in that: The positive electrode material precursor includes a compound shown in Formula 1; Ni a Co b Mn c Al d O n Formula 1; Among them, 0<a≤0.98, 0<b≤0.98, 0≤c≤0.98, 0≤d≤0.2, 0.5≤n≤1.5; In the X-ray diffraction spectrum, the positive electrode material precursor has a diffraction peak of nickel oxide and a diffraction peak of elemental Ni, and the mass fraction of nickel oxide in the positive electrode material precursor is W NixOy , 50%*a*M NixOy / M 总 ≤W NixOy <100%*a*M NixOy / M 总 ; The mass fraction of elemental Ni in the positive electrode material precursor is W Ni , 0<W Ni ≤50%*a*M Ni / M 总 ; M NixOy For you x O y The molar mass, M Ni is the molar mass of Ni, M 总 is the molar mass of the cathode material precursor; b>0, the positive electrode material precursor has a diffraction peak of single substance Co, and the mass fraction of single substance Co in the positive electrode material precursor is W Co , 0<W Co ≤50%*b*M Co / M 总 , M Co is the molar mass of Co.

2. The cathode material precursor according to claim 1, characterized in that: The intensity I(012) of the 012 diffraction peak of nickel oxide and the intensity I(101) of the 101 diffraction peak of nickel oxide satisfy: I(012) / I(101)=1.0-2.0; and, The intensity I(012) of the 012 diffraction peak of nickel oxide and the intensity I(background) of the background satisfy: I(012) / I(background)≤25.

3. The cathode material precursor according to any one of claims 1 to 2, characterized in that: When b>0, the positive electrode material precursor has a diffraction peak of cobalt oxide, and the mass fraction of cobalt oxide in the positive electrode material precursor is W CoxOy , 50%*b*M CoxOy / M 总 ≤W CoxOy <100%*b*M CoxOy / M 总 , M CoxOy For Co x O y The molar mass of .

4. The cathode material precursor according to any one of claims 1 to 2, characterized in that: c>0, the positive electrode material precursor has a diffraction peak of manganese oxide.

5. The cathode material precursor according to claim 3, characterized in that: c>0, the positive electrode material precursor has a diffraction peak of manganese oxide.

6. The cathode material precursor according to any one of claims 1 to 2 and 5, characterized in that: d>0, the positive electrode material precursor has a diffraction peak of aluminum oxide.

7. The cathode material precursor according to claim 3, characterized in that: d>0, the positive electrode material precursor has a diffraction peak of aluminum oxide.

8. The cathode material precursor according to claim 4, characterized in that: d>0, the positive electrode material precursor has a diffraction peak of aluminum oxide.

9. The cathode material precursor according to any one of claims 1-2, 5, 7, and 8, characterized in that: The Dv50 of the positive electrode material precursor is 3-8 μm.

10. The cathode material precursor according to claim 3, characterized in that: The Dv50 of the positive electrode material precursor is 3-8 μm.

11. The cathode material precursor according to claim 4, characterized in that: The Dv50 of the positive electrode material precursor is 3-8 μm.

12. The cathode material precursor according to claim 6, characterized in that: The Dv50 of the positive electrode material precursor is 3-8 μm.

13. A method for preparing a cathode material precursor according to any one of claims 1 to 12, characterized in that: include: Under an oxygen-containing atmosphere, sintering the raw material system in a reaction container to obtain the positive electrode material precursor; Wherein, the raw material system includes at least a nickel source and a cobalt source, and the raw material system also includes at least one of a manganese source and an aluminum source; The flow rate of the oxygen-containing atmosphere is 5-20 L / min, and the volume fraction of oxygen in the oxygen-containing atmosphere is 21%-100%; The volume of the raw material system accounts for 5-10% of the volume of the reaction container.

14. The method for preparing a cathode material precursor according to claim 13, characterized in that: The sintering temperature is 250-700°C; and / or, The sintering time is 1-12 hours.

15. A positive electrode material, characterized in that: The positive electrode material is prepared by the positive electrode material precursor according to any one of claims 1 to 12.

16. The positive electrode material according to claim 15, characterized in that The positive electrode material is subjected to an X-ray diffraction test, and the ratio of the c-axis length to the a-axis length of the unit cell of the positive electrode material is c' / a'>4.93, and the cation mixing rate is <0.

03.

17. A battery, characterized in that: Comprising the positive electrode material according to claim 15 or 16.

18. The battery according to claim 17, characterized in that The battery is charged and discharged in a voltage window of 2.8V-4.25V, and the first discharge capacity is greater than 180.0mAh / g at a rate of 0.2C; after 50 cycles at a rate of 1C, the capacity retention rate is greater than 93%.