A kind of water-based organic pigment and preparation method thereof

By forming a core-shell structure with inorganic nanomaterials and organic pigment powder, and combining superdispersant and non-ionic dispersant, the problem of poor dispersion of aqueous organic pigments in water is solved, and more stable dispersion and better The color performance is suitable for industrial production.

CN116376316BActive Publication Date: 2024-12-03HANGZHOU YINGSHANHUA PIGMENT CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310170628.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-12-03
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

The dispersion of water-based organic pigments in water is poor, which affects their coloring effect and stability.

Method used

Inorganic nanomaterials are used to form a core-shell structure with organic pigment powder, combined with superdispersant and non-ionic dispersant, and the particle size is refined through surface treatment and grinding to improve the dispersion stability and color performance of the pigment.

Benefits of technology

It significantly improves the dispersion stability and color performance of aqueous organic pigments, reduces particle agglomeration, enhances the light resistance and fluidity of the pigments, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application discloses a water-based organic pigment and a preparation method thereof, comprising the following components by weight: 46-62 parts of modified organic pigment powder, 3-6 parts of dispersant, 1-2 parts of wetting agent, 1-2 parts of auxiliary agent and 74-128 parts of water; the modified organic pigment powder is obtained by forming a core-shell structure with organic pigment powder and inorganic nanomaterials. Compared with conventional pigments, the water-based organic pigment prepared in the present application has a smaller and more uniform particle size, is not prone to agglomeration, and has better storage performance and tinting power.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of pigments, and in particular to a water-based organic pigment and a preparation method thereof. Background Art

[0002] Organic pigments are insoluble organic substances that are added to substrates in a highly dispersed state to color the substrates. They are widely used in coatings, printing masterbatches and other fields. Among them, water-based organic pigments are organic pigments that use water as a dispersion medium, and have environmental advantages such as low pollution and low toxicity.

[0003] However, due to the low surface polarity and weak hydrophilicity of water-based organic pigments, it is not easy to maintain uniform and stable dispersion in water, which will affect the coloring effect of water-based organic pigments. Summary of the invention

[0004] In order to solve the problem that water-based organic pigments have poor dispersibility in water, the present application provides a water-based organic pigment and a preparation method thereof.

[0005] In a first aspect, a water-based organic pigment comprises the following components in parts by weight: 46-62 parts of modified organic pigment powder, 3-6 parts of dispersant, 1-2 parts of wetting agent, 1-2 parts of auxiliary agent and 74-128 parts of water; the modified organic pigment powder is obtained by forming a core-shell structure with inorganic nanomaterials and organic pigment powder.

[0006] Typically but not limiting, the organic pigment powder is one of an azo pigment or a phthalocyanine pigment, and the azo pigment may be particularly preferably a benzimidazolone pigment; the auxiliary agent is a combination of one or more of an adsorption promoter, an antioxidant and a defoamer; and the particle size of the inorganic nanomaterial is 8-18 nm.

[0007] By adopting the above technical scheme, the organic pigment powder forms a core-shell structure with the inorganic nanomaterial, and the inorganic nanomaterial is used as the nucleation center, and the organic pigment powder is wrapped to form particles with a core-shell structure. Compared with the unmodified organic pigment powder, the particles have a smaller and more uniform particle size, thereby improving the color performance of the pigment; at the same time, the amount of charge on the surface of the particles will also be reduced, reducing the agglomeration effect between the particles caused by electrostatic effects, and improving the storage stability and coloring effect of the water-based organic pigment; when the inorganic nanomaterial is used as the nucleation center and the organic pigment powder is used as the shell, desorption is not easy to occur between the inorganic nanomaterial and the organic pigment powder, thereby improving the stability of the pigment.

[0008] Preferably, the inorganic nanomaterial is nano silicon dioxide or nano titanium dioxide.

[0009] By adopting the above technical solution, when the above materials are selected as inorganic nanomaterials, the particle size distribution of the modified organic pigment powder is narrower, and the agglomeration effect is further limited; and the silicon element can reduce the surface energy of the particle surface, improve the fluidity and wettability of the modified organic pigment powder, further improve the dispersibility of the modified organic pigment powder, and improve the storage stability of the particle size of the modified organic pigment powder. Nano-titanium dioxide and nano-silicon dioxide can also provide a certain ultraviolet shielding function and improve the light resistance of the pigment.

[0010] Preferably, the modified organic pigment powder comprises the following components in parts by weight: 8-16 parts of organic pigment powder, 4-8 parts of inorganic nanomaterials, and 12-24 parts of polysiloxane.

[0011] Typically, but not limiting, the polysiloxane is dimethylhydroxy silicone oil or polyether-modified silicone oil.

[0012] By adopting the above technical solution, the surface of the inorganic nanomaterial is modified by using polysiloxane, and active groups and hydrophobic groups are introduced into the surface of the inorganic nanomaterial, so as to improve the binding ability of the inorganic nanomaterial and the organic pigment powder, so that the particle size distribution of the modified organic pigment is narrower and the stability is higher. In addition, the surface polarity of the modified organic pigment is improved, the hydrophilicity of the modified organic pigment is increased, the particle aggregation caused by the strong hydrophobicity of the organic pigment is reduced, and the dispersion stability is improved.

[0013] Preferably, the preparation method of the modified organic pigment powder is prepared by the following steps:

[0014] Surface treatment of inorganic nanomaterials: Mixing inorganic nanomaterials with polysiloxane and drying to obtain modified inorganic nanomaterials;

[0015] Modification of organic pigment powder: Mix the organic pigment powder and the modified inorganic nanomaterial, grind at 5-10°C for 1-3h to obtain modified organic pigment powder.

[0016] The parameters of the modified organic pigment preparation method are adjusted, and the organic pigment powder and the modified inorganic nanomaterial are ground at low temperature to reduce the particle agglomeration caused by the temperature increase, and the particle size distribution of the obtained particles is further controlled to improve the color performance and storage stability of the water-based organic pigment.

[0017] Preferably, the preparation method of the modified organic pigment is prepared by the following steps:

[0018] Surface treatment of inorganic nanomaterials: Mixing inorganic nanomaterials with polysiloxane and drying to obtain modified inorganic nanomaterials;

[0019] Modification of organic pigment powder: Mix the organic pigment powder and the modified inorganic nanomaterial, grind at 5-10°C for 1-3h, dry for 15-25min, and then grind at 5-10°C for 10-20min to obtain a modified organic pigment.

[0020] Typically, but not limiting, drying is performed using hot air drying at 50-70°C.

[0021] By adopting the above technical solution, secondary grinding is performed after drying, so that the particles are ground while being kept dry, the grinding effect is improved, and the particle size of the particles is reduced. In addition, the secondary grinding method improves the grinding effect and improves the uniformity of the particle size.

[0022] Preferably, the dispersant is prepared by compounding a super dispersant and a non-ionic dispersant, and the weight ratio of the super dispersant to the non-ionic dispersant is 1:(1-2).

[0023] By adopting the above technical solution, the super dispersant has two parts with different functions. The first part has good compatibility with the pigment, can combine with the pigment, and adhere to the surface of the pigment; the second part has good compatibility with water, can stretch in water, and make the pigment particles repel each other through electrostatic repulsion or entropy repulsion, thereby improving the dispersibility and storage stability of water-based organic pigments. Among them, after the super dispersant is adsorbed on the surface of the particles, it can provide a certain electrostatic repulsion and steric hindrance to maintain the stability between the particles, so only a small amount of addition is needed to achieve a good dispersion effect; and the non-ionic dispersant has good stability and is not easily disturbed by other ions in the water, which can improve the dispersion stability. Therefore, by compounding the super dispersant and the non-ionic dispersant and optimizing the weight ratio of the two, a compatibility effect is formed, which significantly improves the dispersibility and dispersion stability of the pigment particles.

[0024] Preferably, the raw materials of the ionic dispersant include the following components in parts by weight: 4-12 parts of methacrylic acid, 30-46 parts of dimethylaminoethyl methacrylate, 54-70 parts of hydroxyethyl methacrylate, 8-16 parts of polycarboxylic acid, 1.6-2.0 parts of initiator, and 4.5-5 parts of chain transfer agent.

[0025] Typically but not limiting, the initiator is selected from azobisisobutyronitrile and ammonium persulfate; the chain transfer agent is selected from thioglycolic acid and mercaptopropionic acid.

[0026] By adopting the above technical scheme, dimethylaminoethyl methacrylate is selected as the monomer of the anchoring part, and the polymer after polymerization has a large number of tertiary amino groups as anchoring groups, and the polymer can be firmly adsorbed on the surface of the pigment in a tail-shaped adsorption manner to form a thick molecular layer, thereby improving the dispersion stability. Hydroxyethyl methacrylate is selected as the polymerization monomer, which can provide a large number of hydroxyl groups and improve the water solubility of the polymer. Polycarboxylic acid and methacrylic acid are also selected as polymerization monomers, which can adjust the chain length and molecular weight of the polymer, and introduce multiple carboxyl functional groups. Since there are a large number of hydroxyl active groups on the surface of the modified organic pigment, a large number of chemical bonds can be formed between the dispersant and the modified organic pigment, thereby improving the adsorption stability. A large number of carboxyl groups can also improve the fluidity of the pigment and the dispersion state during coloring, thereby improving the color performance of the pigment.

[0027] Preferably, the polycarboxylic acid is itaconic acid.

[0028] By adopting the above technical scheme, the chain length of itaconic acid is shorter and the molecular weight is smaller. While providing multiple carboxyl groups, it will not have a significant impact on the molecular chain length of the polymer, so that the polymer after polymerization will not have a reduced dispersion effect due to the problems of excessive molecular weight and excessive molecular weight. In addition, multiple carboxyl groups are randomly introduced into the molecular chain, the polymer is adsorbed on the particles, the electrostatic repulsion between the particles is increased, and the dispersion stability is improved.

[0029] Preferably, the preparation method of the ionic dispersant is prepared by the following steps:

[0030] Methacrylic acid, dimethylaminoethyl methacrylate, hydroxyethyl methacrylate, itaconic acid and ethyl acetate are mixed, and then the temperature is adjusted to 70-84° C., an initiator and a chain transfer agent are added, reacted for 4-7 hours, and filtered to obtain an ionic dispersant.

[0031] By adopting the above technical solution, when the molecular weight of the polymer is too long and the chain length is too long, the polymers may cause entanglement, causing the viscosity of the system to increase, affecting the color performance of the pigment; at the same time, the bridging reaction of the polymer will be greatly improved, causing bridging between particles, causing the particle size of the pigment particles to increase and the dispersibility to decrease. However, when the molecular weight of the polymer is too small and the chain length is too short, it is difficult for the dispersant to form a thick molecular layer after it adheres to the surface of the pigment particles, and the steric hindrance dispersion effect decreases, causing the pigment particles to easily agglomerate. Therefore, the process parameters of the polymerization are optimized, so that the ionic dispersant has a better dispersion effect and better color performance.

[0032] In a second aspect, a method for preparing a water-based organic pigment is provided, which is prepared by the following steps: taking a modified organic pigment powder, a dispersant, a wetting agent and water, mixing, grinding for 1-2 hours, taking out, adding an auxiliary agent and mixing to obtain a water-based organic pigment.

[0033] By adopting the above technical solution, the modified organic pigment powder, dispersant, wetting agent and water are mixed and ground to further even out the particle size, reduce the agglomeration caused by the mixing of the modified organic pigment powders, and improve the dispersibility of the pigment particles. After grinding, the additive is added to promote the adhesion of the wetting agent and dispersant on the surface of the modified organic pigment powder, further improving the coloring performance and storage stability of the pigment.

[0034] In summary, this application has the following beneficial effects:

[0035] 1. Organic pigment powder is modified by inorganic nanomaterials to form a core-shell structure with inorganic nanomaterials as the core and organic pigment powder as the shell, which further refines the particle size distribution of the pigment particles and improves the storage stability and dispersion stability of the pigment powder.

[0036] 2. A super dispersant with significant dispersibility and improved pigment color performance is prepared by using methacrylic acid, dimethylaminoethyl methacrylate, hydroxyethyl methacrylate and itaconic acid, and a super dispersant and a nonionic dispersant are compounded to have good dispersibility when the amount of dispersant is small. The dispersant used in this application has a stronger adsorption force with the modified organic pigment, and the thickness of the surface molecular layer formed is moderate, so that the particles of the modified organic pigment have stronger electrostatic shielding and steric hindrance effects, so that the water-based organic pigment has a narrower particle size distribution, storage stability and color performance. DETAILED DESCRIPTION

[0037] The raw materials used in the examples and preparation examples are all commercially available and described in detail. The present application is further described in detail below in conjunction with the examples.

[0038] A modified organic pigment powder

[0039] Preparation Example 1-1, a modified organic pigment powder, is prepared by the following preparation method:

[0040] Surface treatment of inorganic nanomaterials: 6 g of nano-silicon dioxide and 18 g of polyether-modified silicone oil were mixed and stirred for 2 h, and the nano-silicon dioxide was taken out and dried to obtain modified inorganic nanomaterials;

[0041] Modification of organic pigment powder: Pigment Red 254# and modified inorganic nanomaterials were mixed, ground at 8°C for 2h, dried at 60°C with hot air for 20min, and then ground at 8°C for 15min to obtain modified organic pigment powder. The particle size of the inorganic nanomaterial was 13nm.

[0042] Preparation Example 1-2, a modified organic pigment powder, is prepared by the following preparation method:

[0043] Surface treatment of inorganic nanomaterials: 8 g of nano-silicon dioxide and 12 g of polyether-modified silicone oil were mixed and stirred for 3 h, and the nano-silicon dioxide was taken out and dried to obtain modified inorganic nanomaterials;

[0044] Modification of organic pigment powder: Pigment Red 254# and modified inorganic nanomaterials were mixed, ground at 5°C for 3 hours, dried at 70°C with hot air for 20 minutes, and then ground at 5°C for 20 minutes to obtain modified organic pigment powder. The particle size of the inorganic nanomaterial was 18nm.

[0045] Preparation Example 1-3, a modified organic pigment powder, is prepared by the following preparation method:

[0046] Surface treatment of inorganic nanomaterials: 4 g of nano-silicon dioxide and 24 g of polyether-modified silicone oil were mixed and stirred for 1 h, and the nano-silicon dioxide was taken out and dried to obtain modified inorganic nanomaterials;

[0047] Modification of organic pigment powder: Pigment Red 254# and modified inorganic nanomaterials were mixed, ground at 10°C for 1 hour, dried at 50°C with hot air for 20 minutes, and then ground at 10°C for 10 minutes to obtain modified organic pigment powder. The particle size of the inorganic nanomaterial was 8 nm.

[0048] Preparation Example 1-4, a modified organic pigment powder, is prepared by the following preparation method:

[0049] Surface treatment of inorganic nanomaterials: 6 g of nano titanium dioxide and 18 g of dimethylhydroxy silicone oil were mixed and stirred for 2 h, and the nano titanium dioxide was taken out and dried to obtain modified inorganic nanomaterials;

[0050] Modification of organic pigment powder: Pigment Red 254# and modified inorganic nanomaterials were mixed, ground at 8°C for 2h, dried with hot air at 60°C for 20min, and then ground at 8°C for 15min to obtain modified organic pigment powder.

[0051] Preparation Example 1-5, a modified organic pigment powder, is different from Preparation Example 1-1 in that Pigment Red 254# is replaced by an equal amount of Pigment Orange 73#.

[0052] Preparation Example 1-6, a modified organic pigment powder, is different from Preparation Example 1-1 in that Pigment Red 254# is replaced by an equal amount of CI Pigment Green 7.

[0053] Preparation Example 1-7, a modified organic pigment powder, is prepared by the following method:

[0054] Surface treatment of inorganic nanomaterials: 6 g of nano-silicon dioxide and 18 g of polyether-modified silicone oil were mixed and stirred for 2 h, and the nano-silicon dioxide was taken out and dried to obtain modified inorganic nanomaterials;

[0055] Modification of organic pigment powder: Pigment Red 254# and modified inorganic nanomaterials were mixed and ground at 8°C for 2h to obtain modified organic pigment powder.

[0056] Preparation Example 1-8, a modified organic pigment powder, is prepared by the following method:

[0057] Surface treatment of inorganic nanomaterials: 6 g of nano-silicon dioxide and 18 g of polyether-modified silicone oil were mixed and stirred for 2 h, and the nano-silicon dioxide was taken out and dried to obtain modified inorganic nanomaterials;

[0058] Modification of organic pigment powder: Pigment Red 254# and modified inorganic nanomaterials were mixed and ground at 10°C for 1 hour to obtain modified organic pigment powder.

[0059] Preparation Example 1-9, a modified organic pigment powder, is prepared by the following method:

[0060] Surface treatment of inorganic nanomaterials: 6 g of nano-silicon dioxide and 18 g of polyether-modified silicone oil were mixed and stirred for 2 h, and the nano-silicon dioxide was taken out and dried to obtain modified inorganic nanomaterials;

[0061] Modification of organic pigment powder: Pigment Red 254# and modified inorganic nanomaterials were mixed and ground at 5°C for 3 hours to obtain modified organic pigment powder.

[0062] Preparation Example 1-10, a modified organic pigment powder, is prepared by the following method:

[0063] Modification of organic pigment powder: Pigment Red 254# and 6 g of nano-silicon dioxide were mixed, ground at 8°C for 2 h, dried with hot air at 60°C for 20 min, and then ground at 8°C for 15 min to obtain modified organic pigment powder.

[0064] Preparation Example 1-11, a modified organic pigment powder, is different from Preparation Example 1-1 in that the nano-silicon dioxide is replaced by an equal amount of sepiolite powder.

[0065] Preparation of hyperdispersants

[0066] Preparation Example 2-1, a hyperdispersant, is prepared by the following method:

[0067] Take 8 g of methacrylic acid, 38 g of dimethylaminoethyl methacrylate, 62 g of hydroxyethyl methacrylate, 12 g of itaconic acid and 200 mL of ethyl acetate, then adjust the temperature to 77°C, add 1.8 g of azobisisobutyronitrile and 4.8 g of thioglycolic acid, react for 5.5 hours, and filter to obtain a hyperdispersant.

[0068] Preparation Example 2-2, a hyperdispersant, is prepared by the following method:

[0069] Take 12g of methacrylic acid, 46g of dimethylaminoethyl methacrylate, 54g of hydroxyethyl methacrylate, 8g of itaconic acid and 200mL of ethyl acetate, then adjust the temperature to 84°C, add 2g of azobisisobutyronitrile and 4.5g of thioglycolic acid, react for 4h, and filter to obtain a hyperdispersant.

[0070] Preparation Example 2-3, a hyperdispersant, is prepared by the following method:

[0071] Take 4 g of methacrylic acid, 30 g of dimethylaminoethyl methacrylate, 70 g of hydroxyethyl methacrylate, 16 g of itaconic acid and 200 mL of ethyl acetate, then adjust the temperature to 70°C, add 1.6 g of azobisisobutyronitrile and 5 g of thioglycolic acid, react for 7 hours, and filter to obtain a super dispersant.

[0072] Preparation Example 2-4, a hyperdispersant, is prepared by the following method:

[0073] Take 5 g of methacrylic acid, 54 g of dimethylaminoethyl methacrylate, 46 g of hydroxyethyl methacrylate, 5 g of itaconic acid and 200 mL of ethyl acetate, then adjust the temperature to 77°C, add 1.8 g of azobisisobutyronitrile and 4.8 g of thioglycolic acid, react for 5.5 hours, and filter to obtain a hyperdispersant.

[0074] Preparation Example 2-5, a hyperdispersant, differs from Preparation Example 2-1 in that itaconic acid is replaced by an equal amount of methacrylic acid. Example

[0075] Embodiment 1, a water-based organic pigment, is prepared by the following preparation method:

[0076] Take 52g of modified organic pigment powder and soak it in 1L of isopropanol for 8h, filter it and wash it with deionized water, dry it and mix it with 4.5g of dispersant, 1.5g of silicone polyether nonionic surfactant and 101g of water, grind it for 1.5h and take it out, add 1.5g of adhesion promoter and mix it, adjust the pH to 7.5 to obtain a water-based organic pigment.

[0077] The modified organic pigment powder is derived from Preparation Example 1-1. The dispersant is prepared by compounding 1 part of a super dispersant and 1.5 parts of a nonionic dispersant, and the super dispersant is derived from Preparation Example 2-1.

[0078] Embodiment 2, a water-based organic pigment, is prepared by the following preparation method:

[0079] Take 62g of modified organic pigment powder and soak it in 1L of isopropanol for 10h, filter it and wash it with deionized water, dry it and mix it with 6g of dispersant, 1g of silicone polyether nonionic surfactant and 128g of water, grind it for 2h and take it out, add 2g of adhesion promoter and mix it, adjust the pH to 7, and obtain a water-based organic pigment.

[0080] The modified organic pigment powder is derived from Preparation Example 1-2. The dispersant is prepared by compounding 1 part of a super dispersant and 2 parts of a non-ionic dispersant, and the super dispersant is derived from Preparation Example 2-2.

[0081] Embodiment 3, a water-based organic pigment, is prepared by the following preparation method:

[0082] Take 46g of modified organic pigment powder and soak it in 1L of isopropanol for 6h, filter it and wash it with deionized water, dry it and mix it with 3g of dispersant, 2g of silicone polyether nonionic surfactant and 74g of water, grind it for 2h and take it out, add 1g of adhesion promoter and mix it, adjust the pH to 8, and obtain a water-based organic pigment.

[0083] The modified organic pigment powder is derived from Preparation Examples 1-3. The dispersant is prepared by compounding 1 part of a super dispersant and 1 part of a non-ionic dispersant, and the super dispersant is derived from Preparation Examples 2-3.

[0084] Example 4 is a water-based organic pigment, which is different from Example 1 in that the modified organic pigment powder is derived from Preparation Examples 1-4.

[0085] Example 5, a water-based organic pigment, is different from Example 1 in that the modified organic pigment powder is derived from Preparation Example 1-5.

[0086] Example 6, a water-based organic pigment, is different from Example 1 in that the modified organic pigment powder is derived from Preparation Example 1-6.

[0087] Example 7, a water-based organic pigment, is different from Example 1 in that the modified organic pigment powder is derived from Preparation Example 1-7.

[0088] Example 8, a water-based organic pigment, is different from Example 1 in that the modified organic pigment powder is derived from Preparation Example 1-8.

[0089] Example 9, a water-based organic pigment, is different from Example 1 in that the modified organic pigment powder is derived from Preparation Example 1-9.

[0090] Example 10, a water-based organic pigment, is different from Example 1 in that the modified organic pigment powder is derived from Preparation Examples 1-10.

[0091] Example 11 is a water-based organic pigment, which is different from Example 1 in that the hyperdispersant is derived from Preparation Example 2-4.

[0092] Example 12, a water-based organic pigment, is different from Example 1 in that the hyperdispersant is derived from Preparation Example 2-5.

[0093] Example 13, a water-based organic pigment, is different from Example 1 in that the hyperdispersant is replaced by an equal amount of non-ionic dispersant.

[0094] Embodiment 14, a water-based organic pigment, is prepared by the following method:

[0095] 52 g of modified organic pigment powder was mixed with 4.5 g of dispersant, 1.5 g of silicone polyether nonionic surfactant and 101 g of water, and the mixture was taken out after grinding for 1.5 h. 1.5 g of adhesion promoter was added and mixed, and the pH was adjusted to 7.5 to obtain a water-based organic pigment (the modified organic pigment powder was not soaked or washed).

[0096] The modified organic pigment powder is derived from Preparation Example 1-1. The dispersant is prepared by compounding 1 part of a super dispersant and 1.5 parts of a nonionic dispersant, and the super dispersant is derived from Preparation Example 2-1.

[0097] Comparative Example

[0098] Comparative Example 1 is a water-based organic pigment, which differs from Example 1 in that the modified organic pigment powder is replaced by an equal amount of organic pigment powder (the organic pigment powder is not modified).

[0099] Comparative Example 2 is a water-based organic pigment, which differs from Example 1 in that the adhesion promoter is replaced by an equal amount of an organosilicon polyether nonionic surfactant.

[0100] Comparative Example 3 is a water-based organic pigment, which differs from Example 1 in that the dispersant is replaced by an equal amount of deionized water.

[0101] Comparative Example 4, a hybrid organic pigment, was prepared by the following method:

[0102] 1. Take 7.8g of Pigment Red 254#, 5g of inorganic salt and 87.7g of water and mix them to obtain an organic pigment aqueous dispersion A, wherein the inorganic salt is a mixture of sodium chloride, sodium nitrate and sodium carbonate, and the mass ratio of the three salts is 1:1:0.8;

[0103] 2. Centrifuge the organic pigment liquid A at a rate of 1500 rpm, remove the supernatant, and then add clean water to disperse it again. Repeat several times until the conductivity of the organic pigment aqueous dispersion is 200-300 μS / m, and then dilute it with water to a solid content of 20%-40% and a conductivity of 80-140 μS / m to obtain an organic pigment dispersion B containing salt;

[0104] 3. Mix the polymerization monomer and the aqueous phase containing emulsifier and initiator evenly, and then stir

[0105] 45 min to obtain monomer primary emulsion C, which consists of 10 g MMA, 5 g BA, 3 g GMA, 2 g DMAPMA, 0.15 g SDS, 0.3 g APS and 10 g SDBP;

[0106] 4. Take 1000 g of organic pigment dispersion B with a solid content of 29 and mix it with the aqueous phase containing only SDBP, and then use a high-speed shear dispersing emulsifier to form a uniform and stable mixed solution D. After heating the uniform and stable mixed solution D to a reaction temperature of 70-75°C, start dripping the monomer primary emulsion C. The dripping time is 45 minutes and the reaction time is 6.5 hours to obtain a hybrid pigment aqueous dispersion E. The mass ratio of ionic surfactant to non-ionic surfactant in the surfactant is 1:1;

[0107] 5. The hybrid pigment aqueous dispersion E is centrifuged and washed 5 times, dried, and finally ground to obtain a hybrid organic pigment.

[0108] Comparative Example 4 is a water-based organic pigment, which is different from Example 1 in that the modified organic pigment powder is derived from Preparation Examples 1-11.

[0109] Performance testing

[0110] The performance tests were conducted on the organic pigments of Examples 1-14 and Comparative Examples 1-4. Each test was conducted 6 times in parallel and the average value was taken. The results are shown in Table 1.

[0111] Experiment 1: Particle size test: The particle size was measured using a nano-laser particle size analyzer (Nano-90 nano-laser particle size analyzer (Malvern Instruments Ltd., UK), and the average particle size of the pigment obtained was recorded as P0.

[0112] Experiment 2: Dispersion stability test: The hybrid pigment was subjected to ultrasonic treatment (in an ultrasonic cell crusher, power 150W, ultrasound for 1h) and light treatment (using an 800W xenon lamp in a photochemical reactor, irradiation for 24h), and then the particle size test was performed again. The average particle size of the hybrid pigment after ultrasonic treatment was recorded as P1, and the average particle size of the hybrid pigment after light treatment was recorded as P2.

[0113] Test 3: Tinting strength determination: Take 0.1g sample, 1g titanium dioxide and 1mL varnish, grind on a flat grinder 3 times, 100 turns each time, to make an ink sample; take 0.1g black standard, 1g titanium dioxide and 1mL varnish and follow the same steps to make an ink standard. Scrape the ground ink and measure the tinting strength using a colorimeter.

[0114] Table 1: Test results of Examples 1-14, Comparative Examples 1-4 and blank standard samples

[0115]

[0116] It can be seen from Examples 1-6, blank standard samples and Table 1 that the particle size of the organic pigment prepared by the technical solution of the present application does not change much after ultrasonic treatment or light treatment, the dispersion stability of the pigment is good, and the tinting power is good. The reason is that the pigment particles of the present application are ground together with the pigment powder using nano-titanium dioxide or nano-silicon dioxide to form a core-shell structure with inorganic nanomaterials as the nucleation center, which reduces the particle size of the pigment powder; the hyperdispersant with a small molecular weight is adsorbed on its surface, so that the organic pigment has a small particle size and good dispersion stability. Different types of pigments have different chemical structures and chemical groups, so the effect of the pigment particle size on the tinting power will change with the change of the pigment type.

[0117] It can be seen from Example 1, Examples 7-9 and Table 1 that optimizing the preparation method of the modified organic pigment powder can improve the dispersion stability of the water-based organic pigment. The reason is that the secondary grinding can further refine the particle size of the modified organic pigment powder and make the distribution of the particle size more uniform. In the subsequent adsorption process with the hyperdispersant, a more uniform molecular layer is formed, thereby improving the dispersion stability.

[0118] In conjunction with Example 1, Example 10 and Table 1, it can be seen that after the inorganic nano material is surface modified, the modified organic pigment has better performance. The reason is that the polarity of the inorganic nano material and the organic pigment powder is too different, and the inorganic nano material itself is easy to agglomerate. Therefore, if the surface modification is not carried out, in the process of forming the core-shell structure, the inorganic nano material and the organic pigment powder themselves agglomerate, causing the pigment particle size to further become larger, and the agglomerated inorganic nano material will also be free in the water to affect the dispersion of the pigment. In the subsequent dispersant adsorption process, it will affect the thickness of the dispersant adsorbed on its surface, thereby affecting the dispersion stability.

[0119] It can be seen from Example 1, Examples 11-12 and Table 1 that optimizing the preparation of the hyperdispersant can improve the dispersion stability of the water-based organic pigment.

[0120] It can be seen from Example 1, Example 13, Comparative Example 3 and Table 1 that when no dispersant is selected or the dispersant does not adopt the compounding scheme of the present application, the dispersion stability of the water-based organic pigment is reduced, especially when no dispersant is used, after ultrasonic or light treatment, the particle size is greatly improved, which is not conducive to the storage and use of the water-based organic pigment. The reason is that although the pigment particle size adopts a core-shell structure to refine the water-based organic pigment, the attraction between the particles is increased, and the agglomeration phenomenon will be further enhanced. Instead of using a compound of a super dispersant and a non-ionic dispersant, only a non-ionic dispersant is used. The adsorption force of the non-ionic dispersant on the water-based pigment particles is relatively low, and it is difficult to form a stable electrostatic shielding layer between the particles, thereby affecting the dispersion of the particles.

[0121] Combining Example 1, Example 14 and Table 1, it can be seen that soaking and washing the modified organic pigment powder can improve the subsequent adsorption of the pigment particles with the dispersant. The reason is that the modified organic pigment powder itself has many inorganic salts and organic impurities, which will affect the adsorption of the dispersant and thus affect the thickness of the formed molecular layer.

[0122] In combination with Example 1, Comparative Examples 1-4 and Table 1, it can be seen that the water-based organic pigment prepared by the technical solution of the present application has a smaller particle size and stronger coloring property than other methods, and the raw materials used are simple, the steps are fewer, and it is more suitable for large-scale industrial production.

[0123] From Example 1, Comparative Example 5 and Table 1, it can be seen that if sepiolite is used to modify the organic pigment powder, the color performance and dispersion stability of the water-based organic pigment will be greatly reduced. The reason is that sepiolite cannot form a core-shell structure with the organic pigment powder with sepiolite as the core, and can only form a simple wrapping on the outer layer of the organic pigment powder. Therefore, the particle size of the particles is greatly increased, causing the coloring power of the pigment to decrease, and affecting the subsequent adsorption of the pigment and the dispersant, resulting in a decrease in dispersion stability.

[0124] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A water-based organic pigment, It is characterized in that The invention comprises the following components in parts by weight: 46-62 parts of modified organic pigment powder, 3-6 parts of dispersant, 1-2 parts of wetting agent, 1-2 parts of auxiliary agent and 74-128 parts of water; the modified organic pigment powder is obtained by forming a core-shell structure with inorganic nanomaterials and organic pigment powder; The inorganic nano material is one of nano silicon dioxide and nano titanium dioxide; The modified organic pigment powder comprises the following components by weight: 8-16 parts of organic pigment powder, 4-8 parts of inorganic nanomaterials, and 12-24 parts of polysiloxane; The modified organic pigment powder is prepared by the following steps: Surface treatment of inorganic nanomaterials: Mixing inorganic nanomaterials with polysiloxane and drying to obtain modified inorganic nanomaterials; Modification of organic pigment powder: Mix the organic pigment powder and the modified inorganic nanomaterial, grind at 5-10°C for 1-3h, dry for 15-25min, and grind at 5-10°C for 10-20min to obtain a modified organic pigment; The dispersant is prepared by compounding a super dispersant and a non-ionic dispersant, wherein the weight ratio of the super dispersant to the non-ionic dispersant is 1:(1-2); the raw materials of the super dispersant, in parts by weight, include the following components: 4-12 parts of methacrylic acid, 30-46 parts of dimethylaminoethyl methacrylate, 54-70 parts of hydroxyethyl methacrylate, 8-16 parts of polycarboxylic acid, 1.6-2.0 parts of initiator, and 4.5-5 parts of chain transfer agent; The polysiloxane is dimethylhydroxy silicone oil or polyether modified silicone oil.

2. A water-based organic pigment according to claim 1, It is characterized in that The polycarboxylic acid is itaconic acid.

3. A water-based organic pigment according to claim 2, It is characterized in that The preparation method of the hyperdispersant is prepared by the following steps: Methacrylic acid, dimethylaminoethyl methacrylate, hydroxyethyl methacrylate, itaconic acid and ethyl acetate are mixed, and then the temperature is adjusted to 70-84° C., an initiator and a chain transfer agent are added, reacted for 4-7 hours, and filtered to obtain a super dispersant.

4. A method for preparing a water-based organic pigment according to any one of claims 1 to 3, It is characterized in that Prepared by the following steps: The modified organic pigment powder, dispersant, wetting agent and water are mixed, ground for 1-2 hours, taken out, and auxiliary agents are added to obtain water-based organic pigment.