A low-cost, low-strength, high-toughness steel and a manufacturing method thereof
Through specific chemical composition and process flow, the problem of producing low-strength and high-tough steel in the existing technology is solved, and the efficient compliance of 235MPa grade yield strength and -60℃ low-temperature impact toughness value is achieved. It is suitable for marine engineering purposes. Reduces production costs and improves market competitiveness.
Patent Information
- Application Number
- CN202310157493.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-04
- Filing Date
- 2023-02-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-23
AI Technical Summary
It is difficult to produce low-strength, high-tough steels that meet marine engineering uses at low cost, especially steels with toughness grades F or above, and the addition of precious alloys increases production costs and affects market competitiveness.
Chemical components are C: 0.05-0.08%, Si: 0.10-0.30%, Mn: 0.80-1.00%, P: ≤0.010%, S: ≤0.0030%, Ti: 0.008-0.020%, N: 0.0030-0.0060% , Al: 0.020-0.050%, Ca: 0.0005-0.0030%, low-cost low-strength high-tough steel, and through molten iron pretreatment, converter smelting, LF refining, RH vacuum treatment, Ca treatment, continuous casting, hydrogenation treatment, heating Rolling and heat treatment process form proeutophenyl ferrite + needle-shaped ferrite structure, and then transform into sheet-like and block-like proeutophenyl ferrite and fine cementite particle structure with diffuse distribution.
It has achieved low-cost, low-strength, high-tough steel with a yield strength of 235MPa and low-temperature impact toughness value of -60℃ ≥297J, which reduces production costs and improves market competitiveness. It is suitable for manufacturing special gas ships, equipment bases and other purposes.
Smart Images

Figure CN116377339B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a low-strength and high-toughness steel for ships and marine engineering. Background Art
[0002] At present, the main steel grades for marine engineering are still mainly toughness grades D and E, and yield strength grades of 355MPa and above. With the development of new routes in the deep sea and the Arctic Ocean and the increasing demand for various gas resources, the main marine steel grades have a trend towards higher strength grades such as 400MPa steel and F and above low-temperature toughness steels with higher low-temperature toughness requirements. Steel companies and scientific research institutions are also competing to research and develop high-strength and high-toughness steels. However, there is little attention to low-strength and high-toughness steels of F and above toughness grades used in the manufacture of special gas ships, equipment bases, and foundation implementation parts. The steel for this type of use does not require high strength, but high toughness. The yield strength can meet the requirements above 235MPa, and the tensile strength can meet the requirements of 400-520MPa, while the low-temperature toughness must meet the requirements of impact temperature ≤-60℃. For 235MPa grade steel with ferrite pearlite structure, it is difficult to further improve the toughness level after reaching E grade. The reason is that in the composition design, steel of this strength level is usually mainly low C, low Mn, and appropriate amount of micro-alloy elements such as Nb, V, and Ti are added as needed. Generally, no precious alloys such as Ni, Cu, and Mo are added. In order to ensure that its strength does not exceed the standard, the ferrite in the steel is relatively coarse and the toughness is low, which makes it difficult to meet the toughness requirements of F grade and above. Since most of the welding and assembly of steel materials by marine engineering, shipbuilding and other enterprises are carried out in the open air, affected by the weather, the working time throughout the year is short, and the overall equipment cost is high. The market competition is stimulated, and strict requirements are placed on the supply and delivery time of the whole order in procurement. Usually, an order for several thousand tons of steel plates for ships or marine engineering will involve dozens of steel grades, multiple thicknesses, and hundreds of specifications and sizes. Although the proportion of steel with low strength and high toughness F and above toughness grade requirements is not large in the order of the whole ship or the whole project, it significantly increases the difficulty of production scheduling for the whole order, affects the delivery time and increases the manufacturing cost.
[0003] Patent Publication No. CN102703807A discloses a marine engineering steel with an impact absorption energy of ≥100J at -80℃ and a production method. Although this method obtains excellent low-temperature toughness, the addition of rare earth element Ce exceeds the requirements of ship classification specifications, and it is currently difficult to carry out actual delivery and realize industrial transformation. Patent Publication No. CN103695769A obtains an FH40 steel plate with an impact energy of 180-240J at -60℃ by adding a large amount of precious metals such as Nb, V, Ni, etc., and through LF+VD+hot rolling+quenching and tempering treatment. Patent Publication No. CN109266958A obtains a ≤50mm series of shipbuilding and marine engineering steels by adding precious metals such as Ni and Nb and controlling the TMCP method. However, the addition of precious alloys such as Ni and Nb significantly increases costs. At present, for the main market steel grades such as D and E, most steel companies have cancelled the addition of precious alloys such as Ni to achieve the purpose of cost reduction. The conversion of F-grade steel billets obtained by the above technology into D and E steels will result in excessively high production costs for D and E steels.
[0004] In order to solve the shortcomings of existing technologies, low-cost design is carried out for steel with low specific gravity, thickness of 6-50mm, low strength, and toughness grade F and above in the whole ship order, and D, E and other ancillary products are obtained on the basis of meeting the requirements of low strength and high toughness. The waste materials brought by smelting continuous casting and rolling are saved, and the market competitiveness is improved. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a low-cost, low-strength, high-toughness steel and its preparation method for the above-mentioned prior art. The yield strength of the product is 235MPa, and the low-temperature impact test temperature is ≤-60°C, which meets the toughness requirements of F grade and above, and the production thickness range is 6-50mm. This product is mainly to meet the market demand for low strength but high toughness, and can be used to manufacture special gas ships, equipment bases, foundation parts, etc.
[0006] The technical solution adopted by the present invention to solve the above problems is: a low-cost, low-strength and high-toughness steel, the chemical composition of which is calculated by weight percentage: C: 0.05-0.08%, Si: 0.10-0.30%, Mn: 0.80-1.00%, P: ≤0.010%, S: ≤0.0030%, Ti: 0.008-0.020%, N: 0.0030-0.0060%, Al: 0.020-0.050%, Ca: 0.0005-0.0030%, and the remainder is Fe and unavoidable impurity elements.
[0007] The reasons for limiting the steel composition in the present invention are as follows:
[0008] C: Reducing the carbon content in the steel plate can improve the low-temperature impact performance and low-temperature strain aging performance of the steel, and improve the welding cold crack sensitivity of the steel plate. However, if the carbon content is too low, the hardenability of the steel will be weakened when the Mn content is also low, which is not conducive to the strength of the steel plate with low compression ratio, especially the thickness of 50mm, etc. to reach the standard. Therefore, the carbon content is controlled to 0.05-0.08%.
[0009] Si: Mainly used for deoxidation. Although its addition amount should be determined according to different smelting methods, to obtain good steel plate performance, it must be above 0.10%. However, too much Si will seriously damage the welding performance of the steel plate, affect the impact toughness of the heat-affected zone, and the dephosphorization effect of the steel plate, so its upper limit is set at 0.30%.
[0010] Mn: It has the effect of delaying the transformation of austenite to ferrite in the steel, which is beneficial to improving the strength and low temperature toughness of the steel. The present invention must ensure that the tensile strength of the 235MPa grade steel plate does not exceed the upper limit and reduce the cost, so the manganese content is as low as possible. The manganese content is specified to be added in the range of 0.80-1.00%.
[0011] P: Although it can improve corrosion resistance, it will reduce low-temperature toughness and hinder weldability, which is inappropriate for structural steel. The present invention stipulates that it is controlled below 0.010%.
[0012] S: The formation of MnS inclusions will also lead to center segregation, which has a significant adverse effect on low-temperature impact toughness. The present invention stipulates that its content is controlled below 0.0030%.
[0013] Ti: Used to fix nitrogen in steel. Under appropriate conditions, titanium and nitrogen form titanium nitride, which prevents the austenite grains from coarsening during the heating, rolling, and especially welding of steel billets at high temperatures up to 1350°C, improves the low-temperature toughness of the base material and the heat-affected zone of welding, and improves welding performance. When titanium is less than 0.008%, the effect is poor; when it exceeds 0.020%, the excess titanium will precipitate with other elements, deteriorating the toughness of the steel.
[0014] Ca: used to spheroidize strip inclusions MnS, improve the metallurgical quality of the steel plate, and improve the toughness of the steel plate. The amount of Ca added is controlled within 0.0005 to 0.0030%.
[0015] N: is an important element in the present invention. Different from the previous control by harmful elements, the nitrogen content in the steel plate is to be guaranteed to be certain. When the ratio of Ti and N atoms in the steel is 1:1, the weight ratio of Ti and N is 3.42. TiN particles are the finest and dispersed, and the refining effect on high-temperature austenite grains is the strongest. Not only can excellent toughness be obtained, but also according to the amount of Ti added and the oxygen content in the steel, as well as other nitrogen-fixing elements, the N content in the present invention is controlled to be 0.0030-0.0060%.
[0016] Al: It is an excellent deoxidizer for steel and an effective grain refinement element, which improves the strength and toughness of steel. When the addition amount is greater than 0.050%, large composite oxide inclusions are easily formed, and nodules are easily formed at the water outlet of the crystallizer. Therefore, the present invention stipulates that the aluminum content should be within the range of 0.020-0.050%.
[0017] Another object of the present invention is to provide a method for preparing the above-mentioned low-cost, low-strength and high-toughness steel, the specific process is as follows:
[0018] Smelting process: Use molten iron pretreatment, converter smelting, then LF refining furnace refining, and RH vacuum treatment.
[0019] Ca treatment process: Usually Q235 grade steel is not treated with Ca. In order to meet the requirements of low temperature toughness, the present invention performs Ca treatment after vacuum treatment of molten steel. Preferably, the amount of Ca added is controlled within 0.0005-0.0030%. After Ca treatment, the total level of inclusions A, B, C, and D is controlled to be ≤2.5. Ca treatment is performed to improve the internal quality of the continuous casting billet and thus improve the toughness of the steel plate.
[0020] Continuous casting process: In order to control the internal looseness and segregation of the steel plate, low superheat casting, argon protection casting throughout the process, and dynamic soft pressure control are carried out. The casting temperature is controlled at 10-25℃ above the liquidus temperature to ensure that the center segregation of the ingot is not higher than C1.0 level.
[0021] Hydrogen expansion treatment process: After the ingot is off the production line, it is cooled for more than 48 hours before hydrogen expansion treatment.
[0022] Heating rolling process: The compression ratio of the continuous casting billet to the finished product thickness is ≥3. The billet is placed in a heating furnace to fully austenitize and recrystallize the steel, thereby ensuring the homogenization of the austenite to ensure the uniformity of the composition and performance of the final product. The preferred heating temperature is 1220-1250°C and the heating time is 8-15min / cm. After the billet is removed from the furnace, it needs to be descaled by high-pressure water. The water pressure of each descaling pass is preferably ≥18MPa. Then, rough rolling + finishing rolling is carried out in two stages. The starting rolling temperature of rough rolling is between 1050 and 1100°C. After rough rolling, the reduction rate of the three single passes is ≥15%, and the temperature thickness is ≥2.0H, where H is the finished product thickness. Then, finishing rolling is carried out to roll the finished product thickness. After rolling, accelerated cooling is carried out to improve the operating efficiency of the production line. The production thickness of the steel plate is affected by the rolling process, and the final microstructure after rolling is slightly different. In order to eliminate this influence, this application determines the waiting thickness, finishing rolling start temperature, post-rolling cooling rate and final cooling temperature according to the finished product thickness. The specific settings are as follows:
[0023]
[0024] Optionally, quenching heat treatment process: the steel plate is subjected to offline quenching treatment after rolling. Preferably, the quenching temperature is 900±10°C, and the time in the furnace is 30 to 100 minutes. To ensure the uniformity of the steel plate, the temperature control accuracy is ±10°C.
[0025] Optionally, tempering heat treatment process: After quenching, the steel plate is preferably tempered at 660±10°C. The furnace holding time is 30 to 175 minutes, giving enough time for the carbon in the quenched martensite to fully diffuse and obtain ferrite. In the subsequent long-term holding process, the ferrite lamellae grow in a manner that is conducive to growth to form flaky or blocky ferrite, and the supersaturated carbon of the original martensite precipitates to form cementite particles dispersed in the matrix, so as to achieve the best match of low strength and high toughness of the steel plate and achieve the purpose of engineering applicability of the steel plate.
[0026] The rolled structure of the present invention is proeutectoid ferrite + acicular ferrite structure, and the structure after heat treatment is flaky and blocky proeutectoid ferrite and fine cementite particles dispersed around the ferrite. The average grain size of the ferrite is between 5-8 μm.
[0027] After sampling and testing according to the national standard GB / T 2975 2018, the steel plate finished product of the present invention has specific transverse tensile properties: yield strength 245-299MPa, tensile strength 436-449MPa, elongation ≥29%, and the standard impact specimen of the steel plate measures longitudinal impact toughness values of ≥297J at -60°C and -80°C. It is much higher than the impact value of the rolled state in the embodiment and the comparative example. The rolled state in the embodiment and the comparative example are only suitable for producing steel grades with lower toughness grades E. The steel plate has no delamination or crack defects, and the flaw detection results meet the requirements of En10160S3 E4 level. There are no bubbles, scars, cracks, tearing, folding, inclusions, and pressed iron oxide scale on the surface of the steel plate. It has a stable production process and is easy to mass produce.
[0028] The present invention uses a low-cost composition design method and a special quenching and tempering process to obtain a low-cost, low-strength, high-toughness steel. Compared with the prior art, it has the following advantages:
[0029] The present invention adopts low C and low Mn, and the grain refining elements are only Al+Ti, without adding precious alloys such as Ni, Nb, and V, thereby greatly saving alloy costs.
[0030] The present invention obtains a mixed structure of lamellar ferrite, massive proeutectoid ferrite and dispersed carbide particles through a heat treatment method. The structure has low strength and excellent low-temperature toughness, and is significantly superior to the ferrite pearlite steel structure of traditional 235MPa grade steel.
[0031] The present invention adopts two-stage controlled rolling and controlled cooling to ensure that the single-pass reduction rate of the three passes after rough rolling is ≥15%, and sets different steel plate water cooling systems according to different plate thicknesses to fully optimize the structure and achieve good low-temperature impact toughness.
[0032] The present invention adopts quenching and tempering heat treatment, and can also avoid problems such as uneven stress and thin steel plate surface flatness caused by TMCP rolling.
[0033] The present invention can also obtain grade D and grade E steel without heat treatment, satisfying the production of multiple steel grades with one component. The remaining billets can be directly rolled without increasing the cost of other steel grades, thereby reducing the number of castings and improving production efficiency.
[0034] The method of the present invention can be extended and applied to other high-strength steel plates, such as steel for offshore shipbuilding, steel for high-rise buildings, steel for bridges, steel for engineering machinery, steel for pressure vessels, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is the rolled metallographic structure of Example 2 of the present invention without quenching and tempering, and is composed of proeutectoid ferrite + acicular ferrite structure.
[0036] Figure 2 It is the metallographic structure of Example 2 of the present invention, which is composed of lamellar and blocky proeutectoid ferrite and dispersed fine cementite particles.
[0037] Figure 3 The metallographic structure of Example 3 of the present invention is composed of lamellar and blocky proeutectoid ferrite and dispersed fine cementite particles. Compared with the metallographic structure of Example 2, part of the lamellar proeutectoid ferrite in Example 3 maintains an orientation relationship of growing inward along the original austenite grains.
[0038] Figure 4 It is the metallographic structure of the ordinary low-carbon Q235 grade steel in the comparative example of the present invention, and is composed of proeutectoid ferrite and pearlite. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0040] The present invention will be further described below in conjunction with the embodiments.
[0041] The production process of low-cost, low-strength and high-toughness steel is: converter or electric furnace steelmaking -> LF refining -> RH vacuum degassing -> Ca treatment -> continuous casting -> ingot dehydrogenation treatment -> heating -> rolling -> cooling -> quenching -> tempering.
[0042] The production method of low-cost, low-strength and high-toughness steel of embodiments 1-4 of the present invention comprises the following steps:
[0043] (1) Smelting: The molten iron is pretreated and smelted in a 150-ton converter, then sent to a LF furnace for refining and RH vacuum degassing.
[0044] (2) Ca treatment process: Ca treatment is performed after vacuum treatment of molten steel. The amount of Ca added is controlled within 0.0005-0.003%. After Ca treatment, the total level of inclusions of A, B, C, and D is controlled to be 2.0. The smelting composition of the embodiment is shown in Table 1.
[0045] (3) Continuous casting: The molten steel is cast into continuous casting billets with a thickness of more than 150 mm. The casting temperature is controlled at 10 to 25°C above the liquidus. Dynamic soft reduction is implemented during the casting process. The continuous casting process parameters are shown in Table 2.
[0046] (4) Ingot hydrogenation treatment: The continuous casting slab is subjected to slow cooling and hydrogenation. The ingot cooling temperature and slow cooling time are shown in Table 2.
[0047] (5) Heating rolling process: The 150 mm continuous casting billet is rolled to the target thickness specification of the embodiment, and the compression ratio of the continuous casting billet to the finished product thickness is ≥3, and the billet is put into a walking beam heating furnace. After the billet is removed from the furnace, it needs to be descaled by high-pressure water, and the water pressure of each descaling pass is ≥18 MPa, followed by two-stage controlled rolling of rough rolling + finishing rolling. The relevant process parameters are shown in Table 3.
[0048] (6) The embodiment was subjected to tempering treatment. The relevant tempering treatment process parameters are shown in Table 4.
[0049] (7) The heat-treated steel sheets were subjected to room temperature transverse stretching and -60°C and -80°C longitudinal impact tests. In addition to the above tests, the rolled steel sheets of Example 2 and the comparative example were also subjected to -40°C longitudinal impact tests. The mechanical properties are shown in Table 5.
[0050] Figure 1-Figure 4 The metallographic structures of Example 2 in the rolled state, Example 2, Example 3 and the comparative example are shown. The metallographic structure of the comparative example is equiaxed proeutectoid ferrite and pearlite structure. In comparison, the structure of the example of the present invention is significantly better than the metallographic structure of the comparative example in both the rolled state and the heat-treated state. The rolled state structure of Example 2 of the present invention is a two-phase structure of proeutectoid ferrite + acicular ferrite, which is an ideal structure for TMCP rolling. The structure composed of lamellar and blocky proeutectoid ferrite and dispersed fine cementite after heat treatment in the example is more excellent. The proeutectoid ferrite, which accounts for nearly 90% of the volume fraction, ensures the low strength of the steel. Because the cementite is dispersed, it has a pinning effect on the ferrite. During the tempering process, the ferrite grains are not overly coarse, thereby ensuring the good high toughness of the steel and achieving a good match of low strength and high toughness.
[0051] Table 1 Chemical composition of the examples (wt, %)
[0052]
[0053] Table 2 Continuous casting process control
[0054]
[0055]
[0056] Table 3 Rolling process control
[0057]
[0058] Table 4 Quenching and tempering heat treatment process control
[0059]
[0060] Table 5: Tensile and impact properties of the examples
[0061]
[0062] Note: The impact specimen size is 10mm×10mm×55mm standard specimen. When the steel material is insufficient to prepare the standard specimen, a small-sized specimen of 7.5mm×10mm×55mm is used as in Example 1. The impact absorption energy conversion ratio between the small-sized specimen in the example and the standard specimen is 5 / 6.
Claims
1. A low-cost, low-strength, high-toughness steel, characterized by: The chemical composition is calculated by weight percentage as follows: C: 0.05-0.08%, Si: 0.10-0.30%, Mn: 0.80-1.00%, P: ≤0.010%, S: ≤0.0030%, Ti: 0.008-0.020%, N: 0.0030-0.0060%, Al: 0.020-0.050%, Ca: 0.0005-0.0030%, and the balance is Fe and unavoidable impurity elements; The method for manufacturing the steel comprises: Molten steel smelting: including molten iron pretreatment, primary smelting, LF furnace refining and vacuum degassing; Ca treatment process: Ca treatment is carried out after vacuum degassing of molten steel. After Ca treatment, the total level of inclusions of A, B, C, and D is controlled to be ≤2.5; Continuous casting process: Casting molten steel into continuous casting billets with a thickness of more than 150 mm; Hydrogen expansion treatment process: After the continuous casting billet comes off the line, it is subjected to hydrogen expansion treatment by cold stacking; Heating rolling process: the compression ratio of continuous casting billet to finished product thickness is ≥3, the billet is heated in a heating furnace to fully austenitize and recrystallize the steel, the billet is descaled by high-pressure water after leaving the furnace, and then rough rolling + finishing rolling is carried out in two stages: rough rolling start temperature: 1050 ~ 1100 ℃, three passes after rough rolling reduction rate ≥ 15%, waiting thickness ≥ 2.0H, H is the finished product thickness, according to the finished product thickness H to determine the waiting thickness, finishing rolling start temperature, cooling speed after rolling and final cooling temperature: 6 mm≤H≤15mm, the waiting thickness is (2.5~3)H, the finishing rolling temperature is 880~940℃, the cooling rate is 3~5℃ / s, and the final cooling temperature is 600~640℃; 15mm<H≤50mm, the waiting thickness is (2~2.5)H, the finishing rolling temperature is 850~900℃, the cooling rate is 6~10℃ / s, and the final cooling temperature is 580~620℃, thereby obtaining the rolled structure of proeutectoid ferrite + acicular ferrite; Quenching and tempering heat treatment process: quenching temperature 900±10℃, furnace time 30~100min, tempering temperature 660±10℃, furnace holding time 30~175min, so that the carbon in the quenched martensite can be fully diffused to obtain ferrite, and in the subsequent holding process, the ferrite lamellae grow in a manner that is conducive to growth to form flaky or blocky ferrite, and the supersaturated carbon of the original martensite precipitates to form cementite particles dispersed in the matrix.
2. The low-cost, low-strength, high-toughness steel according to claim 1, characterized in that: The structure is lamellar and / or massive proeutectoid ferrite and fine cementite particles dispersed around the ferrite, and the average grain size of the ferrite is between 5-8μm.
3. The low-cost, low-strength, high-toughness steel according to claim 1, characterized in that: Transverse tensile properties: yield strength 245~299MPa, tensile strength 436~449MPa, elongation ≥29%, standard impact specimen measured -60℃, -80℃ longitudinal impact toughness value ≥297J.
4. The low-cost, low-strength, high-toughness steel according to claim 1, characterized in that: The amount of Ca added in the Ca treatment process is controlled within 0.0005 to 0.0030%.
5. The low-cost, low-strength, high-toughness steel according to claim 1, characterized in that: The entire continuous casting process uses argon protection pouring and dynamic light pressure control. The casting temperature is controlled at 10 to 25°C above the liquidus temperature to ensure that the center segregation of the ingot is no higher than C1.0 level.
6. The low-cost, low-strength, high-toughness steel according to claim 1, characterized in that: In the heating rolling process, the continuous casting billet is heated to 1220-1250°C in a reheating furnace, and the heating time is 8-15 min / cm.