Color process inkjet ink

By rationally proportioning organic solvents and binder resins in inkjet inks and adding wax to form micro-clusters, the problems of inkjet printing bleeding, beading, feathering, and bleed-through on difficult-to-penetrate and non-penetrating recording media are solved, achieving high stability and excellent printing results.

CN116390996BActive Publication Date: 2024-10-01아티엔스가부시키가이샤 +1
View PDF 24 Cites 0 Cited by

Patent Information

Application Number
CN202180069781.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-04
Filing Date
2021-10-18
Publication Date
2024-10-01
Estimated Expiration
2041-10-18

AI Technical Summary

Technical Problem

Existing inkjet printing technology is prone to image quality degradation problems such as bleeding, beading, feathering, and show-through on poorly penetrable or non-penetrating recording media. Furthermore, its ejection stability is insufficient, making it difficult to maintain excellent printing results on various recording media.

Method used

By rationally proportioning specific organic solvents and binder resins in inkjet inks and adding wax, the drying properties and viscosity of the inks are controlled, forming micro-clusters to improve ink flowability and uniformity, suppress bleeding, beading, and bleed-through, while also improving ejection stability.

Benefits of technology

It achieves excellent printing results on various recording media without bleeding, beading, feathering, or bleed-through, and improves ejection stability, especially exhibiting good wetting spread and anti-blocking properties on non-permeable recording media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004173202410000401
    Figure BDA0004173202410000401
  • Figure BDA0004173202410000411
    Figure BDA0004173202410000411
  • Figure BDA0004173202410000421
    Figure BDA0004173202410000421
Patent Text Reader

Abstract

One embodiment of the present invention relates to a color printing inkjet ink, which contains water, pigment, organic solvent, binder resin and wax, wherein the organic solvent includes an organic solvent having a boiling point of less than 190°C at 1 atmosphere, and the organic solvent having a boiling point of less than 190°C at 1 atmosphere includes a diol solvent and / or a glycol monoalkyl ether solvent, and when the amount of the organic solvent having a boiling point of more than 150°C at 1 atmosphere relative to the total amount of ink is set to S, and the content of the binder resin relative to the total amount of ink is set to R, the S / R value is less than 3.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to color process inkjet inks. Background Art

[0002] Inkjet printing is a method of ejecting tiny droplets of ink from a very fine nozzle located in an inkjet head onto a recording medium and causing them to land to form images and / or text (hereinafter, recording media with images and / or text recorded are collectively referred to as "printed materials"). Compared with other printing methods, inkjet printing is superior in terms of the size and cost of the printing device, the running cost during printing, and the ease of full colorization, and has become significantly popular. In addition, with the significant improvement in the performance of inkjet heads in recent years, it is expected that inkjet printing will be expanded to the industrial printing market that previously used offset printing.

[0003] In the industrial printing market, in addition to highly permeable recording media (liquid-absorbing recording media) such as premium paper, plain paper, and copy paper, printing is also required on poorly permeable recording media (low-liquid-absorbing recording media) such as coated paper and art paper.

[0004] However, the ink used in the inkjet printing method (inkjet ink) has a much lower viscosity than the ink used in the offset printing method. Therefore, when printing a color image on a poorly permeable recording medium, for example, a phenomenon called bleeding (mixed color bleeding) occurs in which different colors are mixed, and a phenomenon called beading occurs in which the light and dark colors in a single color appear to beaded, resulting in a decrease in image quality. In addition, when printing on a highly permeable recording medium, a phenomenon called feathering occurs in which the ink irregularly bleeds along the fibers of the recording medium, and a phenomenon called see-through occurs in which the ink penetrates to the back of the paper, resulting in a significant decrease in image quality. Various studies have been conducted to date to solve the above problems (Patent Documents 1 to 4).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2012-136573

[0008] Patent Document 2: Japanese Patent Application Publication No. 2009-280671

[0009] Patent Document 3: Japanese Patent Application Publication No. 2018-203802

[0010] Patent Document 4: Japanese Patent Application Publication No. 2012-1611 Summary of the invention

[0011] Problems to be solved by the invention

[0012] For example, in Patent Document 1, in order to suppress bleeding and beading, an ink containing a glycol ether-based sparingly water-soluble solvent, an acetylene glycol-based surfactant, and an amino alcohol is disclosed. According to Patent Document 1, the sparingly water-soluble solvent improves the wettability and permeability to the hydrophobically coated recording medium, thereby suppressing beading. However, since the sparingly water-soluble solvent has excessively high wettability and permeability to the recording medium, when printing on a high-permeability recording medium such as high-quality paper, there is the following problem: the ink flows and penetrates along the cellulose fibers constituting the recording medium, and feathering and print-through occur around the printed portion of the text and / or fine lines.

[0013] Patent document 2 discloses a method in which the ink is made thermosensitive by adding a gelling agent, and a temperature difference is set between the temperature of the inkjet head and the temperature of the recording medium, so that the ink has a low viscosity when ejected from the inkjet head and a high viscosity when landing on the recording medium, thereby preventing bleeding, beading, feathering and print-through. However, in this method, the inkjet head needs to be kept at a high temperature. For example, in the embodiment of patent document 2, the temperature of the inkjet head is set to 70°C. If the temperature of the inkjet head is not constant, the possibility of deterioration of the ejection stability is high. In addition, since the viscosity of the ink is relatively high, there is a concern that the inkjet ejection stability during high-speed printing is poor. Furthermore, since the time from the ink landing on the recording medium to the solidification and drying is very short, it may not be possible to fully prevent bleeding, beading, feathering and print-through during high-speed printing. In addition, the ink described in patent document 2 also has the problem that the printed matter has poor abrasion resistance to poorly permeable recording media.

[0014] It should be noted that the applicant previously proposed in Patent Document 3 an ink using a fixing resin having a specific structure and acid value in order to suppress bleeding (mixed color bleeding). In the ink, the fixing resin functions as a surfactant, thereby suppressing the fusion of adjacent ink droplets and bleeding. However, when the ink is used, due to the surface activity effect of the fixing resin, the permeability of the ink to high-permeability recording media such as high-quality paper becomes too high, and feathering and print-through may occur.

[0015] As described above, there is no inkjet ink that can produce printed materials with excellent scratch resistance and excellent ejection stability on both highly permeable recording media and poorly permeable recording media.

[0016] In recent years, there has been a demand for producing printed materials with excellent image quality not only for highly permeable recording media and poorly permeable recording media, but also for recording media that are completely impermeable to ink (impermeable recording media). Polyvinyl chloride sheets used in the billboard market, polyethylene terephthalate (PET) films, polypropylene films, polyethylene films, etc. used in the flexible packaging printing market are representative examples of impermeable recording media, and in order to promote the development of inkjet printing, it can be said that these recording media must be addressed.

[0017] However, even when printing on an impermeable recording medium, the above-mentioned beading may occur, resulting in a decrease in image quality. In addition, depending on the impermeable recording medium used and the printing conditions, the applied ink may not be fully wetted and spread on the impermeable recording medium, resulting in whitening in spots or stripes (reflection, white stripes), and when the printed material is rolled up, part of the printed layer may adhere to the non-printing surface (back side) of the impermeable recording medium (blocking).

[0018] As a method for solving the above-mentioned problems, for example, Patent Document 4 discloses an ink using two water-soluble resins with different weight-average molecular weights and acid values. In the above-mentioned Patent Document 4, by using water-soluble resins with relatively close weight-average molecular weights and acid values, the water-soluble resins in the ink are homogenized, and the viscosity of the ink caused by intermolecular interactions increases, which can prevent beading (liquid deviation) on non-permeable recording media, and can achieve improved ejection stability and abrasion resistance. However, as mentioned above, the viscosity of the ink recorded in Patent Document 4 is high, so the wetting and expansion on the non-permeable recording medium is insufficient, and the possibility of whitening and white stripes is high. In addition, when performing high-speed printing, there is a concern about the deterioration of ejection stability caused by the high viscosity.

[0019] Some embodiments of the present invention are made to solve the above-mentioned problems, and the purpose is to provide a color printing inkjet ink that can obtain printed products without image defects such as bleeding, beading, feathering and print-through for various recording media, and has excellent ejection stability. In addition, some embodiments of the present invention have the purpose of providing a color printing inkjet ink that can obtain printed products without beading even when printing on non-permeable recording media, has excellent wetting and spreading properties, and has good blocking resistance.

[0020] Methods for solving problems

[0021] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved by controlling the amount of a specific organic solvent and the amount of a binder resin to be within specific ranges and using a wax in combination, thereby completing the present invention.

[0022] That is, an embodiment of the present invention relates to a color process inkjet ink comprising water, a pigment, an organic solvent, a binder resin and a wax.

[0023] The organic solvent includes an organic solvent having a boiling point of 190° C. or less at 1 atmosphere pressure,

[0024] The organic solvent having a boiling point of 190° C. or less under 1 atmosphere pressure comprises a divalent alcohol solvent and / or a glycol monoalkyl ether solvent, and

[0025] When the amount of the organic solvent having a boiling point of 150° C. or higher at 1 atmosphere relative to the total amount of ink is S and the content of the binder resin relative to the total amount of ink is R, the value of S / R is 3.0 or less.

[0026] In another embodiment of the present invention, the color process inkjet ink is characterized in that the organic solvent having a boiling point of 190° C. or less at 1 atmosphere pressure includes a divalent alcohol solvent and a glycol monoalkyl ether solvent.

[0027] In addition, another embodiment of the present invention relates to the above-mentioned color printing inkjet ink, wherein the organic solvent having a boiling point of less than 190°C under 1 atmosphere of pressure contains two or more organic solvents, and among the above-mentioned two or more organic solvents, the difference between the boiling points of the organic solvent with the highest boiling point and the organic solvent with the lowest boiling point is 10 to 100°C.

[0028] In addition, another embodiment of the present invention relates to the above-mentioned color printing inkjet ink, which is used in a printing device having an ink circulation mechanism configured to communicate with an inkjet head.

[0029] Moreover, another embodiment of the present invention relates to the above-mentioned color process inkjet ink, wherein the above-mentioned wax includes a polyolefin wax having a melting point of 80 to 180°C.

[0030] In addition, another embodiment of the present invention relates to the above-mentioned color printing inkjet ink, wherein the amount of organic solvent having a boiling point exceeding 190° C. at 1 atmosphere is less than 1 mass % relative to the total amount of ink, and the S / R value is greater than 2.3 and less than 3.0.

[0031] Effects of the Invention

[0032] According to some embodiments of the present invention, a color printing inkjet ink can be provided for various recording media, which can produce printed materials without image defects such as bleeding, beading, feathering and print-through, and has excellent ejection stability. In addition, according to some embodiments of the present invention, in addition to the above content, a color printing inkjet ink can be provided, which can produce printed materials without beading even when printing on non-permeable recording media, has excellent wetting and spreading properties, and has good blocking resistance. DETAILED DESCRIPTION

[0033] Hereinafter, a preferred embodiment is listed to describe a color printing inkjet ink (hereinafter also referred to as "color ink" or "ink") as an embodiment of the present invention. It should be noted that in this specification, "aqueous medium" refers to a medium composed of a liquid containing at least water.

[0034] Generally, by lowering the boiling point of the organic solvent contained in the ink, the drying property of the ink is increased, and bleeding on the poorly permeable recording medium can be suppressed. For example, by using an organic solvent with a boiling point of 190°C or less under 1 atmosphere, the ink will not dry poorly on the recording medium, and even when printing on a poorly permeable recording medium, bleeding caused by the merging of ink droplets can be suppressed. On the other hand, beading caused by a single-color ink may be deteriorated by the above-mentioned method. The reason for this is believed to be that the drying property of the ink is too high, resulting in deviations in the drying behavior within the ink droplets.

[0035] In addition, by reducing the amount of organic solvent in the ink relative to the amount of binder resin in the ink, the degree of increase in viscosity accompanying the drying of the ink can be increased, and feathering and print-through on high-permeability recording media can be suppressed. In addition, since it is also possible to suppress the merging of ink droplets of different colors, it is believed that bleeding can also be further improved. However, since the above-mentioned deviation in drying behavior becomes more severe, it is possible to further deteriorate beading.

[0036] In addition, the above practices will accelerate the drying of the ink on the inkjet head and increase the viscosity, which may lead to deterioration of the ejection stability. Therefore, it is difficult to improve beading and ejection stability only by selecting an organic solvent with a suitable boiling point and adjusting the mixing amount of the organic solvent and the binder resin.

[0037] Therefore, the present inventors conducted intensive research and found that by using wax in addition to the above method, it is possible to suppress bleeding, feathering and print-through while preventing beading and deterioration of ejection stability. The reason why beading and deterioration of ejection stability can be prevented by adding wax is not yet clear, but the following reasons may be considered, for example.

[0038] As will be described in detail later, the wax and binder resin contained in the ink are of different resin types. Therefore, it is believed that the wax and binder resin are not completely homogenized in the ink, but form microscopic clusters respectively. On the other hand, when the ink applied to the recording medium dries, convection occurs inside the ink droplets. At this time, as the clusters involved in the convection flow, other components in the ink also flow, resulting in the suppression of component deviations inside the ink droplets, the drying behavior is homogenized, and beading is improved.

[0039] In addition, as described above, in the present invention, the amount of organic solvent is small relative to the amount of binder resin, and the viscosity of the ink in the middle of drying is high, so it is easy to generate flow inside the ink as a whole during convection. As a result, it is possible to achieve further suppression of deviation of components in the ink, uniformity of drying behavior, and further improvement of beading. In addition, when printing on an impermeable recording medium, it is believed that the flow inside the ink as a whole promotes the flow of the ink droplets, thereby improving the wetting and spreading properties.

[0040] It should be noted that, when the gas-liquid interface exists only in a part of the ink, as in the ink existing in the inkjet head, it is considered that the above-mentioned convection functions to prevent local drying and viscosity increase, thereby suppressing the deterioration of discharge stability.

[0041] In addition, it can also be considered that the above-mentioned clusters further improve beading by preventing the pigments inside the drying ink from getting close to each other, and further, the wax clusters hinder the network that can be formed between the clusters of the binder resin, thereby suppressing the increase in the microscopic viscosity of the ink and improving the ejection stability.

[0042] In addition, when printing on a highly permeable recording medium, the wax fills the gaps in the highly permeable recording medium, thereby further improving print-through. Furthermore, when printing on an impermeable recording medium, the wax can also be expected to improve the blocking resistance.

[0043] As described above, in order to simultaneously solve all the problems of the present invention, it can be said that the above-mentioned ink configuration is indispensable.

[0044] Next, each component contained in the color process inkjet ink which is an embodiment of the present invention will be described below.

[0045] <Organic Solvents>

[0046] The ink of an embodiment of the present invention contains an organic solvent having a boiling point of 190°C or less at 1 atmosphere, and the organic solvent having a boiling point of 190°C or less at 1 atmosphere contains a dihydric alcohol solvent and / or a glycol monoalkyl ether solvent. In the ink of an embodiment of the present invention, when the amount of the organic solvent having a boiling point of 150°C or more at 1 atmosphere relative to the total amount of the ink is set as S, and the content of the above-mentioned binder resin relative to the total amount of the ink is set as R, the S / R value is 3.0 or less. The above-mentioned S / R value is preferably 0.8 or more and 3.0 or less, more preferably 1.0 or more and 2.9 or less, and particularly preferably 1.2 or more and 2.8 or less. If it is within this range, not only the above-mentioned effect can be obtained, but also, for example, when a pigment dispersion resin described later is used, the compatibility of the binder resin and the pigment dispersion resin is improved, thereby improving the ejection stability from the inkjet head.

[0047] It should be noted that, in a certain embodiment, the S / R value is preferably 2.3 or more and 3.0 or less, more preferably 2.6 or more and 3.0 or less, and particularly preferably 2.8 or more and 3.0 or less. When the S / R value is within the above range, when printing on an impermeable recording medium, a printed material without beading, excellent wetting and spreading properties, and good blocking resistance can be obtained.

[0048] It should be noted that the "organic solvent" in the present specification refers to an organic compound used to dissolve and / or disperse a substance, and is liquid under the conditions of 25° C. and 1 atmosphere.

[0049] As the above-mentioned organic solvent, a water-soluble organic solvent is preferably used. It should be noted that "water-soluble organic solvent" refers to an organic solvent whose solubility in water is 5g / 100gH2O or more under the conditions of 25°C and 1 atmosphere. As the water-soluble organic solvent, for example, a monohydric alcohol solvent, a dihydric alcohol solvent, an alkylene glycol monoalkyl ether solvent, an alkylene glycol dialkyl ether solvent, etc. can be preferably used.

[0050] <Boiling Point of Organic Solvent>

[0051] As described above, the ink according to the embodiment of the present invention contains an organic solvent having a boiling point of 190° C. or less at 1 atmosphere. The boiling point at 1 atmosphere can be measured using a thermal analysis device such as DSC (differential scanning calorimetry).

[0052] As an organic solvent having a boiling point of 190°C or less at 1 atmosphere pressure,

[0053] The monohydric alcohol solvent includes ethanol (boiling point 78°C), 1-propanol (boiling point 97°C), isopropanol (boiling point 82°C), 1-butanol (boiling point 117°C), 2-butanol (boiling point 100°C), isobutanol (boiling point 108°C), 1-pentanol (boiling point 137.8°C), 3-methyl-1-butanol (boiling point 132°C), 3-methyl-2-butanol (boiling point 112°C), 2-methyl-2-butanol (boiling point 102°C), 3-pentanol (boiling point 115.6°C), n-hexanol (boiling point 157°C), 2-methyl-1-pentanol (boiling point 148°C), 2-ethylbutanol (boiling point 1 47℃), n-heptanol (boiling point 175.8℃), 2-heptanol (boiling point 160℃), 3-heptanol (boiling point 156℃), 2-octanol (boiling point 179℃), 2-ethylhexanol (boiling point 185℃), cyclohexanol (boiling point 161℃), 2-methylcyclohexanol (boiling point 174℃), glycidol (boiling point 167℃), furfuryl alcohol (boiling point 170℃), tetrahydrofurfuryl alcohol (boiling point 178℃), 3-methoxy-1-butanol (boiling point 158℃), 3-methoxy-3-methyl-1-butanol (boiling point 174℃), 2-(2-methoxymethoxy)ethanol (boiling point 168℃), etc.

[0054] Examples of diol solvents (glycol solvents) include propylene glycol (boiling point 188° C.) and 2,3-butanediol (boiling point 182° C.).

[0055] Examples of the alkylene glycol monoalkyl ether solvents include ethylene glycol monomethyl ether (boiling point 124°C), ethylene glycol monoethyl ether (boiling point 135°C), ethylene glycol monobutyl ether (boiling point 171°C), ethylene glycol monoisobutyl ether (boiling point 161°C), ethylene glycol monoisopropyl ether (boiling point 142°C), ethylene glycol monoallyl ether (boiling point 159°C), propylene glycol monomethyl ether (boiling point 121°C), propylene glycol monoethyl ether (boiling point 160°C), propylene glycol monopropyl ether (boiling point 150°C), propylene glycol mono-n-butyl ether (boiling point 170°C), and dipropylene glycol monomethyl ether (boiling point 187°C).

[0056] Examples of the alkylene glycol dialkyl ether solvents include ethylene glycol dimethyl ether (boiling point 85°C), diethylene glycol dimethyl ether (boiling point 162°C), diethylene glycol methyl ethyl ether (boiling point 176°C), diethylene glycol diethyl ether (boiling point 189°C), and diethylene glycol dimethyl ether (boiling point 171°C).

[0057] Examples of the alkylene glycol dialkyl ether acetate solvent include ethylene glycol monoethyl ether acetate (boiling point 156° C.), propylene glycol monoethyl ether acetate (boiling point 160° C.), and the like.

[0058] Examples of the chain amide solvents include N,N-dimethylformamide (boiling point 153°C), N,N-dimethylpropionamide (boiling point 176°C), etc.

[0059] Examples of heterocyclic compound solvents include piperazine (boiling point 110° C.), morpholine (boiling point 129° C.), N-methylmorpholine (boiling point 115° C.), and N-ethylmorpholine (boiling point 138° C.).

[0060] Other solvents include ethyl lactate (boiling point 155°C), cyclohexanone (boiling point 156°C), methylcyclohexanone (boiling point 171°C), etc.

[0061] Examples of the alkanolamine solvent include, but are not limited to, N,N-dimethylaminoethanol (boiling point 134°C), N,N-diethylaminoethanol (boiling point 162°C), N-methylethanolamine (boiling point 156°C), 2-ethylaminoethanol (boiling point 169°C), N-tert-butylethanolamine (boiling point 177°C), and diethylisopropanolamine (boiling point 159°C). In addition, these organic solvents may be used alone or in combination.

[0062] Among the above-mentioned, as an organic solvent having a boiling point of 190°C or less under 1 atmosphere, the ink contains a dihydric alcohol solvent (glycol solvent) and / or a glycol monoalkyl ether solvent, preferably a dihydric alcohol solvent (glycol solvent) and a glycol monoalkyl ether solvent. The ink may contain one or more selected from the group consisting of a monohydric alcohol solvent, a glycol dialkyl ether solvent and an alkanolamine solvent. In addition, it is preferred to contain one or more selected from the group consisting of a monohydric alcohol solvent and an alkanolamine solvent. By containing at least a dihydric alcohol solvent (glycol solvent) and / or a glycol monoalkyl ether solvent, the ink has better permeability and wetting and spreading properties to various recording media, and suppresses bleeding, beading, feathering and print-through. Furthermore, by improving the solubility of the binder resin, the ejection stability is improved.

[0063] In addition, from the viewpoint of more appropriately expressing the above-mentioned effects, the ink of the embodiment of the present invention preferably contains two or more organic solvents having a boiling point of 190°C or less under 1 atmosphere. At this time, it is preferred to contain two or more organic solvents selected from the group consisting of a monohydric alcohol solvent, a dihydric alcohol solvent, a glycol monoalkyl ether solvent and an alkanolamine solvent. Among them, the ink contains at least a dihydric alcohol solvent (diol solvent) and / or a glycol monoalkyl ether solvent. In addition, it is particularly preferred to contain one or more dihydric alcohol solvents and one or more glycol monoalkyl ether solvents. By containing these organic solvents, bleeding, beading, feathering and print-through can be suppressed regardless of the recording medium, and the inkjet ejection stability is also improved.

[0064] It should be noted that when two or more organic solvents having a boiling point of 190° C. or less at 1 atmosphere are used, the difference in boiling point between the organic solvent having the highest boiling point and the organic solvent having the lowest boiling point at 1 atmosphere is preferably 10 to 100° C., more preferably 25 to 90° C., and particularly preferably 30 to 70° C. By making the difference in boiling point within the above range, bleeding, beading, feathering, and strike-through can be suppressed regardless of the recording medium, and inkjet ejection stability is also improved.

[0065] On the other hand, in the ink of the embodiment of the present invention, the content of the organic solvent having a boiling point of 150°C or more at 1 atmosphere is 3 times or less by mass of the content of the binder resin. It should be noted that when calculating the content of the organic solvent having a boiling point of 150°C or more at 1 atmosphere, the organic solvent having a boiling point of 190°C or less at 1 atmosphere (among which the organic solvent having a boiling point of 150°C or more) is also included in the calculation.

[0066] As an organic solvent having a boiling point of 150°C or higher under 1 atmosphere pressure,

[0067] Monohydric alcohols include n-hexanol (boiling point 157°C), n-heptanol (boiling point 176°C), 2-heptanol (boiling point 160°C), 3-heptanol (boiling point 156°C), n-octanol (boiling point 195°C), 2-octanol (boiling point 179°C), 2-ethylhexanol (boiling point 185°C), 3,5,5-trimethylhexanol (boiling point 194°C), 1-nonanol (boiling point 214°C), n-decanol (boiling point 233°C), n-dodecanol (boiling point 257°C), cyclohexanol (boiling point 161°C), 2-methylcyclo ...3,5,5-trimethylhexanol (boiling point 194°C), 3 174°C), benzyl alcohol (boiling point 205°C), glycidol (boiling point 167°C), furfuryl alcohol (boiling point 170°C), tetrahydrofurfuryl alcohol (boiling point 178°C), α-terpineol (boiling point 221°C), 3-methoxy-1-butanol (boiling point 158°C), 3-methoxy-3-methyl-1-butanol (boiling point 174°C), 2-(2-methoxymethoxy)ethanol (boiling point 168°C), 2-(2-methoxyethoxy)ethanol (boiling point 194°C), 1-butoxyethoxypropanol (boiling point 229°C), etc.

[0068] Divalent alcohols include ethylene glycol (boiling point 198°C), propylene glycol (boiling point 188°C), 1,3-propanediol (boiling point 214°C), 1,2-butanediol (boiling point 191°C), 1,3-butanediol (boiling point 207°C), 1,4-butanediol (boiling point 230°C), 2,3-butanediol (boiling point 182°C), 1,2-pentanediol (boiling point 206°C), 1,3-pentanediol (boiling point 209°C), 1,2-hexanediol (boiling point 223°C), 2-methyl-1,3-propanediol (boiling point 21 4℃), 2,2-dimethyl-1,3-propanediol (boiling point 208℃), 3-methyl-1,3-butanediol (boiling point 203℃), 2-ethyl-2-methyl-1,3-propanediol (boiling point 226℃), 2-ethyl-1,3-hexanediol (boiling point 244℃), diethylene glycol (boiling point 245℃), triethylene glycol (boiling point 287℃), tetraethylene glycol (boiling point 328℃), dipropylene glycol (boiling point 232℃), tripropylene glycol (boiling point 271℃), tetrapropylene glycol (boiling point 271℃), etc.

[0069] Examples of trivalent or higher alcohol solvents (polyol solvents) include glycerol (boiling point 290°C), 1,2,4-butanetriol (boiling point 312°C), trimethylolpropane (boiling point 295°C), etc.

[0070] The alkylene glycol monoalkyl ether solvents include ethylene glycol monobutyl ether (boiling point 171°C), ethylene glycol monoisobutyl ether (boiling point 161°C), ethylene glycol monohexyl ether (boiling point 208°C), ethylene glycol mono-2-ethylhexyl ether (boiling point 229°C), ethylene glycol monobenzyl ether (boiling point 256°C), ethylene glycol monoallyl ether (boiling point 159°C), diethylene glycol monomethyl ether (boiling point 193°C), diethylene glycol monoethyl ether (boiling point 196°C), diethylene glycol monoisopropyl ether (boiling point 207°C), diethylene glycol monobutyl ether (boiling point 230.6°C), diethylene glycol monoisobutyl ether (boiling point 220°C), diethylene glycol monohexyl ether (boiling point 2 ... Diethylene glycol mono-2-ethylhexyl ether (boiling point 272°C), diethylene glycol monobenzyl ether (boiling point 302°C), diethylene glycol monophenyl ether (boiling point 283°C), triethylene glycol monomethyl ether (boiling point 249°C), triethylene glycol monoethyl ether (boiling point 255°C), triethylene glycol monobutyl ether (boiling point 271°C), tetraethylene glycol monobutyl ether (boiling point 304°C), propylene glycol monoethyl ether (boiling point 160°C), propylene glycol mono-n-butyl ether (boiling point 170°C), dipropylene glycol monomethyl ether (boiling point 187°C), dipropylene glycol monopropyl ether (boiling point 231°C), dipropylene glycol mono-n-butyl ether (boiling point 212°C), tripropylene glycol monomethyl ether (boiling point 242°C), etc.

[0071] Examples of the alkylene glycol dialkyl ether solvents include diethylene glycol dimethyl ether (boiling point 162°C), diethylene glycol methyl ethyl ether (boiling point 176°C), diethylene glycol diethyl ether (boiling point 189°C), diethylene glycol dibutyl ether (boiling point 255°C), diethylene glycol methyl butyl ether (boiling point 212°C), triethylene glycol dimethyl ether (boiling point 216°C), triethylene glycol methyl butyl ether (boiling point 261°C), and tetraethylene glycol dimethyl ether (boiling point 275°C).

[0072] Examples of the alkylene glycol monoalkyl ether acetate solvent include ethylene glycol monoethyl ether acetate (boiling point 156° C.), diethylene glycol monoethyl ether acetate (boiling point 218° C.), propylene glycol monoethyl ether acetate (boiling point 160° C.), and the like.

[0073] Examples of nitrogen-containing solvents include N,N-diethylaminoethanol (boiling point 162°C), N,N-dibutylaminoethanol (boiling point 226°C), N-(β-aminoethyl)ethanolamine (boiling point 244°C), N-methylethanolamine (boiling point 156°C), N-methyldiethanolamine (boiling point 245°C), 2-ethylaminoethanol (boiling point 169°C), N-ethyldiethanolamine (boiling point 251°C), mono-n-butylethanolamine (boiling point 199°C), mono-n-butyldiethanolamine (boiling point 270°C), N-tert-butylethanolamine (boiling point 177°C), diethylisopropanolamine (boiling point 159°C), triethanolamine (boiling point 335°C), N-(2-hydroxyethyl)piperazine (boiling point 246°C), 4-(2-hydroxyethyl)morpholine (boiling point 227°C), N,N-dimethylformamide, N,N-di Methyl-β-methoxypropionamide, N,N-dimethyl-β-ethoxypropionamide, N,N-dimethyl-β-butoxypropionamide, N,N-dimethyl-β-pentyloxypropionamide, N,N-dimethyl-β-hexyloxypropionamide, N,N-dimethyl-β-heptyloxypropionamide, N,N-dimethyl-β-2-ethylhexyloxypropionamide, N,N-dimethyl-β-octyloxypropionamide, N,N-diethyl-β-butoxypropionamide, N,N-diethyl-β-pentyloxypropionamide, N,N-diethyl-β-hexyloxypropionamide, N,N-diethyl-β-heptyloxypropionamide, N,N-diethyl-β-octyloxypropionamide, 2-pyrrolidone (boiling point 245°C), N-methylpyrrolidone (boiling point 202°C), N-ethylpyrrolidone (boiling point 218°C), 3-methyl-2- Oxazolidinone, 3-ethyl-2- Oxazolidinone, etc.

[0074] Other solvents include, but are not limited to, ethyl lactate (boiling point 155° C.), isophorone (boiling point 215° C.), methylcyclohexanone (boiling point 171° C.), γ-butyrolactone (boiling point 204° C.), ε-caprolactone (boiling point 214° C.), etc. In addition, these organic solvents may be used alone or in combination.

[0075] From the viewpoint of obtaining printed materials without bleeding, beading, feathering and show-through on various recording media, without destabilizing the binder resin and surfactant (when used) in the ink, and thus obtaining an ink having a low viscosity and excellent ejection stability, the organic solvent having a boiling point of 150° C. or higher at 1 atmosphere is preferably selected from the group consisting of a monohydric alcohol solvent, a dihydric alcohol solvent and a glycol monoalkyl ether solvent, more preferably contains a dihydric alcohol solvent and / or a glycol monoalkyl ether solvent, further preferably contains a dihydric alcohol solvent or a glycol monoalkyl ether solvent, and particularly preferably contains a dihydric alcohol.

[0076] In addition, among the divalent alcohol solvents, it is preferred to use at least one alkanediol having 2 to 6 carbon atoms, more preferably an alkanediol having 3 to 6 carbon atoms, and particularly preferably an alkanediol having 5 to 6 carbon atoms. In particular, by containing an alkanediol having 6 carbon atoms, not only the permeability and wetting and spreading properties to a poorly permeable recording medium are improved, bleeding and beading are suppressed, but also, when a surfactant is used, the compatibility with the surfactant is improved, and the inkjet ejection stability is improved.

[0077] Furthermore, when printing on a poorly permeable recording medium, from the viewpoint of suppressing the deviation of the components in the ink when the ink dries and obtaining a printed material without bleeding and beading, the organic solvent having a boiling point of 150° C. or above under 1 atmosphere is preferably contained in two or more kinds, and particularly preferably contains one or more kinds selected from diol-based solvents and one or more kinds selected from glycol monoalkyl ether-based solvents.

[0078] On the other hand, the content of the organic solvent having a boiling point of 250 to 300° C. at 1 atmosphere contained in the ink of the embodiment of the present invention is preferably 9% by mass or less (or 0% by mass), more preferably 5% by mass or less (or 0% by mass), and particularly preferably 3% by mass or less (or 0% by mass) relative to the total amount of the ink. By limiting the amount of the organic solvent having a boiling point of 250 to 300° C., the ink does not cause poor drying, and when printing on a poorly permeable recording medium, bleeding can be suppressed. Furthermore, when printing on a highly permeable recording medium, feathering and print-through will not occur.

[0079] Examples of the organic solvent having a boiling point of 250 to 300° C. at 1 atmosphere include glycerin (boiling point 290° C.), 1,6-hexanediol (boiling point 250° C.), triethylene glycol monobutyl ether (boiling point 278° C.), triethylene glycol methyl butyl ether (boiling point 261° C.), tetraethylene glycol dimethyl ether (boiling point 275° C.), triethylene glycol (boiling point 287° C.), tripropylene glycol (boiling point 271° C.), tetrapropylene glycol (boiling point 250° C. or higher), polyethylene glycol 200 (boiling point 250° C. or higher), polyethylene glycol 400 (boiling point 250° C. or higher), polyethylene glycol 600 (boiling point 250° C. or higher), N-methyl Oxazolidinone (boiling point 257°C), etc.

[0080] In addition, when printing on a non-permeable recording medium, from the viewpoint of obtaining a printed material without beading and excellent in blocking resistance, in a certain embodiment, the content of an organic solvent having a boiling point exceeding 190°C at 1 atmosphere is preferably 1% by mass or less (it may also be 0% by mass), and particularly preferably 0.5% by mass or less (it may also be 0% by mass), relative to the total amount of ink.

[0081] The weighted average boiling point of the organic solvent used in the present invention at 1 atmosphere is preferably 100 to 235°C, more preferably 120 to 210°C, and particularly preferably 120 to 195°C. In addition, if the image quality (suppression of bleeding and beading, etc.) on poorly permeable recording media such as coated paper is taken into consideration, 120 to 180°C is particularly preferred. If the weighted average boiling point of the organic solvent at 1 atmosphere is 100°C or more, the ejection stability from the inkjet head is improved, and the image quality when printing on a highly permeable recording medium is improved. In addition, if the weighted average boiling point is 235°C or less, poor drying will not occur on the recording medium, and bleeding caused by the fusion of ink droplets due to residual organic solvent will not occur, the image quality is improved, and the friction resistance of the printed matter on poorly permeable recording media such as coated paper is also improved. It should be noted that the calculation of the weighted average value of the boiling point also includes the organic solvent having a boiling point of 250 to 300°C at 1 atmosphere. In addition, when the ink contains two or more organic solvents, the weighted average value of the boiling point at 1 atmosphere refers to the value obtained by adding the product of the boiling point at 1 atmosphere calculated for each organic solvent and the mass ratio relative to the total amount of the organic solvent. Furthermore, when the organic solvent is one, the "weighted average value of the boiling point at 1 atmosphere" is renamed as "the boiling point of the organic solvent at 1 atmosphere".

[0082] In addition, from the viewpoint of controlling the weighted average value of the boiling point within the above-mentioned range, the amount of the organic solvent having a boiling point of 100 to 225°C at 1 atmosphere is preferably 50% by mass or more, more preferably 70% by mass or more, and particularly preferably 85% by mass or more relative to the total amount of the organic solvent in the ink.

[0083] In addition, in one embodiment, when printing on an impermeable recording medium, from the viewpoint of obtaining a printed matter without beading, the weighted average value of the boiling points of water and the organic solvent at 1 atmosphere is preferably 100 to 130° C., more preferably 101 to 125° C., and particularly preferably 102 to 120° C. It should be noted that the “weighted average value of the boiling points of water and the organic solvent at 1 atmosphere” refers to a value calculated using the above-mentioned method for calculating the weighted average value of the boiling points at 1 atmosphere for water and the organic solvent contained in the ink.

[0084] Furthermore, the specific heat of the organic solvent at 20°C is preferably 0.40 to 0.70 cal / g°C, and more preferably 0.45 to 0.65 cal / g°C. When it is 0.40 cal / g°C or more, a sharp temperature change does not occur during the ink drying process, and the drying behavior in the ink droplets is unlikely to deviate, which can suppress beading and bleeding. When it is 0.70 cal / g°C or less, the temperature of the ink is easily increased during the ink drying process, and the ink has excellent drying properties, which not only improves feathering and print-through, but also improves the compatibility of the wax and binder resin contained in the ink, and improves the scratch resistance.

[0085] The specific heat of an organic solvent can be measured, for example, by DSC (differential scanning calorimeter). Specifically, using a high-sensitivity differential scanning calorimeter Thermo plus EV02 DSC8231 (manufactured by Rigaku Corporation), about 10 g of an organic solvent as a measurement object is added to an aluminum sample pan, which is then sealed with a sample sealer, and the obtained substance, the sample pan (empty container), and three substances with known specific heats are measured under the same conditions, and the specific heat of the organic solvent can be calculated from the obtained DSC graph.

[0086] The weighted average static surface tension of the organic solvent used in the present invention at 25°C is preferably 25 to 40 mN / m, more preferably 26 to 35 mN / m, and particularly preferably 27 to 32 mN / m. When the weighted average static surface tension at 25°C is 25 mN / m or more, the wetting spread and permeability on the poorly permeable recording medium are improved, and a printed matter with suppressed bleeding and beading can be obtained. In addition, when the weighted average static surface tension at 25°C is 40 mN / m or less, the permeability of the ink to the highly permeable recording medium is controlled, and a printed matter with suppressed feathering and print-through can be obtained.

[0087] In addition, when the ink contains two or more organic solvents, the weighted average value of the static surface tension at 25°C of the organic solvents refers to the value obtained by adding the product value of the static surface tension at 25°C of each organic solvent and the mass ratio relative to the total amount of the organic solvent. Furthermore, when the organic solvent is one, the "weighted average value of the static surface tension at 25°C" is renamed as "static surface tension at 25°C of the organic solvent".

[0088] The static surface tension at 25° C. is a value measured by the Wilhelmy method, and specifically, is a value that can be measured using CBVP-Z manufactured by Kyowa Interface Science Co., Ltd. and a platinum plate.

[0089] The total amount of the organic solvent used in the present invention is preferably 1 to 29% by mass relative to the total amount of the ink. In addition, from the viewpoint of ensuring ejection stability on the inkjet head and obtaining a printed matter having excellent adhesion, drying properties, and image quality (suppression of bleeding and beading, etc.) even on a poorly permeable recording medium, it is more preferably 3 to 27% by mass in the total amount of the ink, and from the viewpoint of obtaining a printed matter having no beading, excellent wetting and spreading properties, and good blocking resistance when printing on an impermeable recording medium, it is particularly preferably 5 to 25% by mass.

[0090] <Pigment>

[0091] From the viewpoint of obtaining a printed matter with excellent color development and color reproducibility, the color printing inkjet ink of the embodiment of the present invention uses a pigment as a colorant for presenting a color printing color. It should be noted that the "color printing color" in the present invention refers to a color (having lightness, hue and chroma, and achromatic colors) among the four colors used in printing, specifically, the three colors of cyan, magenta and yellow.

[0092] As the pigment that can be used for color printing inkjet ink, there is no particular restriction, and a pigment known in the past can be used. The pigment can use any of an inorganic pigment and an organic pigment. In addition, it can be a pigment commonly used in printing applications and coating applications, and an appropriate pigment can be selected from these pigments according to the desired applications such as color reproducibility, color development and light resistance.

[0093] It should be noted that, in order to present a color print, only a pigment that presents the same color as the color print may be used (for example, only a cyan pigment may be used as a pigment for cyan ink), and from the viewpoint of improving color reproducibility, color development, light resistance, etc., a pigment that does not present the same color as the color print may be used (for example, a green pigment may be used as a pigment for cyan ink). Furthermore, two or more pigments may be used in combination.

[0094] Among the color printing inkjet inks, as pigments that can be used for inks that present cyan (cyan inks), for example, CI Pigment Blue 1, 2, 3, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 60, 62, 64, 66, etc. can be listed. Among them, from the viewpoint of excellent color development and light resistance, it is preferred to contain one or more selected from the group consisting of CI Pigment Blue 15:3 and 15:4. In addition, as described above, in order to improve color reproducibility, green pigments such as CI Pigment Green 7, 36, 43, and 58 can also be mixed.

[0095] The content of the pigment in the cyan ink is preferably 0.1 to 10% by mass, more preferably 1 to 10% by mass, based on the total mass of the cyan ink.

[0096] Among color process inkjet inks, as pigments that can be used for inks that exhibit magenta (magenta inks), naphthol pigments, quinacridone pigments, and diketopyrrolopyrrole pigments are preferably used from the viewpoint of excellent color development and light resistance. Specifically, as naphthol pigments, for example, CI Pigment Red 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50, 50:1, 50:2, 51, 52, 52:1, 52:2, 53, 53:1, 55, 56, 57, 57:1, 57:2, 58, 58:1, 58:2, 60, 60:1, 62, 63:1, 63:2, 64, 64:1, 65, 66, 67, 68, 69, 70, 99, 115, 117, 151, 193, 200, 201, 243, 247 and other laked azo pigments, CI Pigment Red 1, 3, 4, 6, 40, 93, 144 and other β-naphthol pigments, CI Pigment Red 2, 5, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 31, 32, 95, 112, 114, 119, 136, 146, 147, 148, 150, 162, 164, 170, 171, 175, 176, 183, 184, 185, 187, 188, 208, 210, 238, 242, 245, 253, 256, 258, 261, 266, 268, 269 and other naphthol AS pigments,

[0097] As quinacridone pigments, for example, CI Pigment Red 122, 202, 207, 209, CI Pigment Violet 19, etc. can be cited.

[0098] Examples of the diketopyrrolopyrrole pigment include CI Pigment Red 254 and 255.

[0099] Among them, from the viewpoint of excellent color reproducibility, naphthol pigments or quinacridone pigments are preferred, and naphthol AS pigments or quinacridone pigments can be used more preferably. Furthermore, it is particularly preferred to contain naphthol AS pigments. In particular, as naphthol AS pigments, it is preferred to contain one or more selected from the group consisting of CI Pigment Red 31, 32, 122, 146, 147, 150, 176, 184, 185, 202, 209, 282 and 269, and it is more preferred to contain one or more selected from the group consisting of CI Pigment Red 31, 146, 147, 150, 184, 185 and 269.

[0100] The content of the pigment in the magenta ink is preferably 0.1 to 10% by mass, more preferably 2 to 10% by mass, based on the total mass of the magenta ink.

[0101] In the color printing inkjet ink, examples of pigments that can be used for the ink that expresses yellow (yellow ink) include CI Pigment Yellow 10, 11, 12, 13, 14, 17, 20, 24, 74, 83, 86, 93, 94, 95, 109, 110, 117, 120, 125, 128, 137, 138, 139, 147, 148, 150, 151, 154, 155, 166, 168, 180, 185, and 213. Among them, from the viewpoint of excellent color development, one or more selected from the group consisting of CI Pigment Yellow 12, 13, 14, 74, 83, 120, 150, 151, 154, 155, 180, and 185 are preferred.

[0102] <Pigment dispersion resin>

[0103] Examples of methods for stably dispersing and maintaining the above-mentioned pigment in ink include: (1) a method of coating at least a portion of the surface of the pigment with a pigment dispersing resin; (2) a method of adsorbing a water-soluble and / or water-dispersible surfactant onto the surface of the pigment; and (3) a method of chemically or physically introducing hydrophilic functional groups onto the surface of the pigment and dispersing the pigment in the ink without using a dispersing resin or a surfactant (self-dispersing pigment).

[0104] The ink of the embodiment of the present invention preferably selects the method (1) above, i.e., the method of using a pigment dispersion resin. This is because, by selecting and studying the polymerizable monomer composition and / or molecular weight of the resin, the pigment coating ability of the pigment dispersion resin and the charge of the pigment dispersion resin can be easily adjusted, so that even fine pigments can be given dispersion stability, and a printed matter with excellent ejection stability, color development and color reproducibility can be obtained.

[0105] The kind of pigment dispersion resin is not particularly limited, for example, (meth) acrylic resin, styrene (meth) acrylic resin, maleic acid (anhydride) resin, styrene maleic acid (anhydride) resin, olefin maleic acid (anhydride) resin, olefin resin, carbamate resin, ester resin (polycondensate of polycarboxylic acid and polyol) etc. can be used, but are not limited to these. Wherein, from the aspects of ejection stability, the size of material selectivity, the ease of synthesis, etc., preferably use one or more selected from the group consisting of (meth) acrylic resin, styrene (meth) acrylic resin, carbamate resin, ester resin and olefin resin. In addition, from the viewpoint that the dispersion stability of ink and ejection stability become better, when using the binder resin described later, preferably use the same kind of resin as the pigment dispersion resin with the binder resin.

[0106] In addition, in a certain embodiment, although the details are unclear, from the viewpoint of obtaining a printed material without feathering and show-through when printing on a high-permeability recording medium, it is preferred to use one or more selected from the group consisting of styrene maleic acid (anhydride) resins and olefin maleic acid (anhydride) resins as the pigment dispersing resin.

[0107] It should be noted that, in this specification, "(meth) acrylic resin" refers to acrylic resin, methacrylic resin, or acrylic-methacrylic resin. Here, "acrylic-methacrylic resin" refers to a resin using acrylic acid and / or acrylic acid ester and methacrylic acid and / or methacrylic acid ester as polymerizable monomers. In addition, "maleic acid (anhydride)" refers to maleic anhydride or maleic acid.

[0108] The above-mentioned pigment dispersion resin can be synthesized by a known method, or a commercial product can be used. In addition, there is no particular restriction on its structure, for example, a resin having a random structure, a block structure, a comb-shaped structure, a star-shaped structure, etc. can be used. Furthermore, as the pigment dispersion resin, a water-soluble resin or a non-water-soluble resin can be selected. It should be noted that "water-soluble resin" refers to a resin that is transparent to the naked eye when a 1% water mixture at a temperature of 25°C is used as the object, and "non-water-soluble resin" refers to a resin other than a water-soluble resin.

[0109] In the present invention, when a water-soluble resin is used as a pigment dispersion resin, its acid value is preferably more than 100 mgKOH / g and less than 450 mgKOH / g, and more preferably 120 to 400 mgKOH / g. Particularly preferably, it is 150 to 350 mgKOH / g. By making the acid value within the above range, the dispersion stability of the pigment can be maintained, and it can be stably ejected from the inkjet head. In addition, it is also preferred to suppress the viscosity of the pigment dispersion liquid by making the interaction between the pigment dispersion resins suitable while ensuring the solubility of the pigment dispersion resin in water.

[0110] On the other hand, when a water-insoluble resin is used as the pigment dispersing resin, its acid value is preferably 0 to 100 mgKOH / g, more preferably 5 to 90 mgKOH / g, and further preferably 10 to 80 mgKOH / g. When the acid value is within the above range, a printed material having excellent drying properties and abrasion resistance can be obtained.

[0111] It should be noted that the acid value of the resin can be measured using a known device. The acid value of the resin in this specification is a value measured by potentiometric titration according to JIS K 2501. As an example of a specific measuring method, a method of using AT-610 manufactured by Kyoto Electronics Industries, Ltd. to dissolve the resin in a toluene-ethanol mixed solvent, titrate with a potassium hydroxide solution, and calculate the acid value from the titration amount to the end point can be cited.

[0112] In the ink of the embodiment of the present invention, from the viewpoint of improving the adsorption capacity of the pigment and ensuring the dispersion stability, it is preferred to introduce an aromatic group into the pigment dispersion resin. It should be noted that as the aromatic group, phenyl, naphthyl, anthracenyl, tolyl, xylyl, mesityl, anisyl, etc. can be listed, but are not limited to these. Among them, phenyl, naphthyl and tolyl are preferred from the perspective of being able to fully ensure the dispersion stability.

[0113] From the viewpoint of achieving a balance among pigment dispersion stability, ejection stability, printing quality, and drying properties, the amount of the aromatic ring-containing monomer introduced is preferably 5 to 75% by mass, more preferably 5 to 65% by mass, and still more preferably 10 to 50% by mass relative to the total amount of monomers forming the pigment dispersion resin.

[0114] In addition to the aromatic group, it is particularly preferred to introduce an alkyl group having 8 to 36 carbon atoms into the pigment dispersion resin. This is because by setting the carbon number of the alkyl group to 8 to 36, it is possible to achieve a lower viscosity of the pigment dispersion, improve the dispersion stability of the pigment, and improve the ejection stability. It should be noted that the carbon number of the alkyl group is more preferably 10 to 30, and more preferably 12 to 24. In addition, as long as the alkyl group has a carbon number of 8 to 36, any of a straight chain and a branched chain can be used, and a straight chain alkyl group is preferred. Examples of the straight-chain alkyl group include octyl (C8), lauryl (C12), myristyl (C14), cetyl (C16), stearyl (C18), arachidyl (C20), behenyl (C22), lignoceryl (C24), ceryl (C26), montanyl (C28), myristyl (C30), tridecyl (C32), tetratriadecyl (C34), and hexatriadecyl (C36).

[0115] From the viewpoint of achieving both low viscosity of the pigment dispersion and scratch resistance of the printed material, the amount of the monomer containing an alkyl chain having 8 to 36 carbon atoms introduced is preferably 5 to 60% by mass, more preferably 10 to 55% by mass, and particularly preferably 15 to 50% by mass, relative to the total amount of monomers forming the pigment dispersion resin.

[0116] It should be noted that, when a water-soluble resin is used as the pigment dispersion resin, in order to improve the solubility in the ink, the acid groups in the resin are preferably neutralized with a base. Whether the amount of base added is excessive can be confirmed, for example, by preparing a 10% by mass aqueous solution of the pigment dispersion resin and measuring the pH of the aqueous solution. From the viewpoint of improving the dispersion stability and ejection stability of the pigment, the pH of the aqueous solution is preferably 7 to 11, and more preferably 7.5 to 10.5.

[0117] Examples of the base used to neutralize the pigment dispersion resin include organic amine solvents such as triethylamine, monoethanolamine, diethanolamine, triethanolamine, N-methyldiethanolamine, dimethylaminoethanol, diethylaminoethanol, and aminomethylpropanol; aqueous ammonia; alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; alkali metal carbonates such as lithium carbonate, sodium carbonate, sodium bicarbonate, and potassium carbonate, but are not limited to these.

[0118] When a water-soluble resin is used as a pigment dispersing resin, its weight average molecular weight is preferably in the range of 1,000 to 500,000, more preferably in the range of 5,000 to 40,000, further preferably in the range of 10,000 to 35,000, and particularly preferably in the range of 15,000 to 30,000. By making the weight average molecular weight in the above range, the pigment is stably dispersed in water, and it is easy to adjust the viscosity when used in ink. When the weight average molecular weight is 1,000 or more, the pigment dispersing resin is difficult to dissolve in the water-soluble organic solvent added to the ink, so the adsorption of the pigment by the pigment dispersing resin is enhanced, and the dispersion stability and ejection stability are improved. If the weight average molecular weight is 50,000 or less, the viscosity during dispersion is suppressed to a low level, and the dispersion stability of the ink and the ejection stability from the inkjet head are improved, and stable printing can be performed for a long time.

[0119] The weight average molecular weight of the pigment dispersion resin is, for example, a polystyrene conversion value that can be measured by a method based on JIS K 7252. As an example of a specific measurement method, there can be mentioned a method of measuring using HLC-8120GPC manufactured by Tosoh Corporation equipped with a TSKgel column manufactured by Tosoh Corporation and an RI detector, and using THF as a developing solvent.

[0120] The amount of the pigment dispersion resin is preferably 1 to 100% by mass relative to the amount of the pigment. By setting the ratio of the pigment dispersion resin to the above range, the viscosity of the pigment dispersion liquid is suppressed, and the dispersion stability and ejection stability of the ink are improved. As the ratio of the pigment to the pigment dispersion resin, it is more preferably 2 to 50% by mass, and particularly preferably 4 to 45% by mass.

[0121] The pigment dispersing resin may be used alone or in combination of two or more.

[0122] <Dispersion aid>

[0123] In the ink of the embodiment of the present invention, from the viewpoint of significantly improving the dispersion stability and ejection stability of the pigment and improving the color reproducibility of the printed matter by making it possible to finely disperse the pigment, when the method (1) or (2) among the above-mentioned dispersion methods is selected, a dispersion aid may be used in combination. The dispersion aid is a material that helps to increase the adsorption rate of the pigment by the pigment dispersing resin or surfactant. In the present invention, any material known in the past can be used as a dispersion aid, and in particular, compounds called pigment derivatives can be preferably used. Pigment derivatives refer to compounds in which substituents are introduced into organic pigment molecules. Examples of the above-mentioned organic pigments include monoazo pigments, disazo pigments, polyazo pigments, anthraquinone pigments, isoindolinone pigments, isoindolinone pigments, quinacridone pigments, quinophthalone pigments, diazinone pigments, and quinacridone pigments. Oxazine pigments, diketopyrrolopyrrole pigments, threne pigments, thioindigo pigments, naphthalocyanine pigments, phthalocyanine pigments, perinone pigments, perylene pigments, benzimidazolone pigments, metal complex pigments, etc. It should be noted that the above-mentioned "pigment" is a general term for pigments and dyes.

[0124] When a dispersing aid is used in the present invention, the amount thereof is preferably set to 0.1 to 10% by mass, particularly preferably to 0.5 to 5% by mass, relative to the amount of the pigment. By setting it to 0.1% by mass or more, the addition ratio relative to the pigment becomes a sufficient amount, and the dispersion stability and ejection stability are improved. In addition, by setting it to 10% by mass or less, the pigment micronization will not be excessively performed, so the dispersion stability is improved, and the deterioration of the light resistance of the printed matter can be prevented.

[0125] <Binder Resin>

[0126] In the ink according to the embodiment of the present invention, a binder resin is used to prevent bleeding, feathering, and print-through and to improve the scratch resistance of printed matter.

[0127] The "binder resin" in this specification refers to a resin used to bond a layer of a printed material (printing layer, ink layer) to a recording medium. It should be noted that, as described above, the ink of the embodiment of the present invention may contain a pigment dispersion resin, but when the resin contained in the ink is a water-soluble resin, the resin corresponds to a pigment dispersion resin and a binder resin based on the adsorption rate of the pigment. That is, a resin having an adsorption rate of 50% or more to the pigment relative to the total amount of the compounding amount is judged as a pigment dispersion resin, and a resin having an adsorption rate of less than 50% by mass is judged as a binder resin.

[0128] It should be noted that, as an example of a method for measuring the adsorption rate of the pigment, the ink diluted with water is subjected to centrifugal separation treatment (for example, at 30,000 rpm for 4 hours) as needed to separate the pigment and the supernatant. Then, when the solid content contained in the supernatant is measured, if the solid content is 50% by mass or more relative to the total amount of the resin having the same composition contained in the water-based ink, the resin is judged to be a binder resin.

[0129] As the form of binder resin for water-based ink, water-soluble resin and (water-dispersible) resin particles (a form of non-water-soluble resin) are generally known. In the present invention, any one of them can be selected for use, or the two can be used in combination. For example, resin particles are high molecular weight compared to water-soluble resins, which can improve the wiping resistance of printed materials, and the image quality of printed materials is also excellent. In addition, when printing on a high-permeability recording medium, the gap of the high-permeability recording medium can be effectively buried, so feathering is suppressed. On the other hand, the ink using a water-soluble resin as a binder resin has excellent ejection stability.

[0130] The acid value of the binder resin is preferably 1 to 80 mgKOH / g. In addition, from the viewpoint of ensuring the dispersion stability of the pigment, obtaining a printed product with excellent image quality by rapidly moving to the gas-liquid interface, and obtaining a printed product without feathering and print-through by rapidly moving in a manner of filling the gaps of the highly permeable recording medium when using a highly permeable recording medium, the acid value of the binder resin is more preferably 3 to 65 mgKOH / g, further preferably 5 to 45 mgKOH / g, and particularly preferably 15 to 35 mgKOH / g. It should be noted that the acid value of the binder resin can be measured in the same manner as the acid value of the pigment dispersion resin.

[0131] The glass transition temperature of the binder resin can be selected according to the required characteristics, for example, as follows. Specifically, in order to improve the ejection stability and the abrasion resistance of the printed matter, to obtain a printed matter without feathering and print-through when printing on a high-permeability recording medium, and to obtain an ink having excellent drying properties and blocking resistance (a phenomenon in which the printed layer adheres to other recording media when overlapping the printed recording media), the glass transition temperature is preferably 60 to 140°C, more preferably 70 to 135°C, and particularly preferably 80 to 130°C.

[0132] The glass transition temperature is a value measured using a DSC (differential scanning calorimeter), and can be measured, for example, as follows according to JIS K 7121. About 2 mg of a sample after the resin is dried is weighed in an aluminum pan, and the aluminum pan is set as a test container in a holder in a DSC measuring device (for example, DSC-60Plus manufactured by Shimadzu Corporation). Then, the measurement is performed under a temperature increase condition of 5°C / min, and the temperature of the intersection of the baseline on the low temperature side and the tangent line at the inflection point read from the obtained DSC graph is used as the glass transition temperature in this specification.

[0133] As the type of binder resin used in the present invention, there can be mentioned (meth) acrylic resin, styrene (meth) acrylic resin, urethane resin, urethane-(meth) acrylic composite resin, styrene butadiene resin, vinyl chloride resin, styrene maleic acid (anhydride) resin, ester resin, etc. Among them, from the viewpoint of obtaining an ink excellent in dispersion stability and ejection stability, the binder resin preferably uses one or more resins selected from the group consisting of (meth) acrylic resin, styrene (meth) acrylic resin, urethane resin, urethane-acrylic composite resin and polyolefin resin, and more preferably uses one or more resins selected from (meth) acrylic resin and styrene (meth) acrylic resin.

[0134] The binder resin may be synthesized by a known method or a commercially available product may be used. In addition, there is no particular limitation on its structure, and for example, a resin having a random structure, a block structure, a comb structure, a star structure, etc. may be used.

[0135] When a water-soluble resin is used as the binder resin, the weight average molecular weight is preferably 5,000 to 50,000 from the viewpoint of ensuring ejection stability from the inkjet nozzle and obtaining a printed material having excellent abrasion resistance on various recording media, and is more preferably 8,000 to 45,000, and further preferably 10,000 to 40,000 from the viewpoint of being able to suppress feathering and print-through when printing on a high-permeability recording medium. It should be noted that the weight average molecular weight of the binder resin can be measured in the same manner as the weight average molecular weight of the above-mentioned pigment dispersion resin.

[0136] The content of the binder resin relative to the total amount of ink is preferably 1 to 15% by mass, more preferably 2 to 12% by mass, and further preferably 4 to 10% by mass, in terms of solid content. By setting the amount of the binder resin within the above range, dispersion stability and ejection stability will not be reduced, and a printed material with excellent image quality and abrasion resistance can be obtained regardless of the recording medium.

[0137] <Wax>

[0138] The ink of the embodiment of the present invention contains wax. In this specification, "wax" refers to an organic compound that is solid at room temperature (25°C) and becomes liquid when heated. For example, it refers to a substance with a melting point of 40 to 200°C that does not decompose but melts in a temperature environment exceeding the melting point.

[0139] The melting point of the wax is preferably 60 to 200°C, more preferably 80 to 180°C, further preferably 100 to 180°C, and particularly preferably 120 to 160°C from the viewpoint of wiping properties of printed matter.

[0140] The wax may be a water-soluble material or a water-insoluble material, but is preferably a water-insoluble material, and is particularly preferably a resin particle (emulsion). In addition, as examples of chemical structures, there are hydrocarbon waxes, ester waxes (e.g., fatty acid ester waxes), silicone waxes, and polyalkylene glycol waxes.

[0141] It should be noted that, for example, an acrylic-silicone copolymer emulsion having a glass transition temperature of 50° C. or higher is generally unlikely to satisfy the above-mentioned melting point condition and therefore does not belong to the wax in the present invention.

[0142] If the wax that can be used in the present invention is more specifically represented, for example, natural wax and synthetic wax can be cited. As natural wax, paraffin wax, microcrystalline wax, petrolatum, etc. as petroleum wax can be cited; carnauba wax, candelilla wax, rice bran wax, etc. as plant wax can be cited; lanolin, beeswax, etc. as animal wax can be cited; montan wax, ozokerite, etc. as mineral wax can be cited. As synthetic wax, polyolefin wax, Fischer-Tropsch wax, acrylic acid-silicone copolymer, urethane-silicone copolymer, polyethylene glycol, paraffin derivatives, montan wax derivatives, microcrystalline wax derivatives, etc. can be cited. These waxes can be used alone or in combination of two or more in aqueous inkjet inks.

[0143] In the above examples, hydrocarbon wax or silicone wax is preferred from the viewpoint of obtaining abrasion resistance and excellent image quality in various recording media, and polyolefin wax as hydrocarbon wax is more preferred. In particular, by containing polyolefin wax, the binder resin and the polyolefin wax form microscopic clusters respectively, which suppresses the deviation of ink components when the ink is dried and improves beading. Furthermore, the clusters function in a manner to prevent local drying and viscosity increase near the inkjet nozzle, thereby improving ejection stability.

[0144] Examples of polyolefin waxes include polyethylene waxes and polypropylene waxes. Polyethylene waxes are preferred from the viewpoints of spray stability and abrasion resistance. It should be noted that any one wax may be used alone or in combination of two or more waxes.

[0145] In addition, the polyolefin wax is preferably a soft polyolefin having a molecular weight of less than 10,000.

[0146] When the wax is a resin particle, the average particle size is preferably 5 to 300 nm, more preferably 30 to 250 nm, and particularly preferably 40 to 200 nm. If the average particle size of the wax is 5 nm or more, the wiping resistance of the printed matter is improved, and if it is 300 nm or less, not only the inkjet ejection stability is improved, but also a printed matter with excellent image quality can be obtained regardless of the recording medium. It should be noted that the average particle size of the wax can be measured by the same method as the average secondary particle size of the pigment described later.

[0147] The wax in the form of resin particles can be produced by, for example, mixing wax that is solid at room temperature and melted by heating, hot water, and an emulsifier. Moreover, commercially available waxes may be used, for example, AQUACER-507, AQUACER-513, AQUACER-515, AQUACER-526, AQUACER-531, AQUACER-533, AQUACER-535, AQUACER-537, AQUACER-539, AQUACER-552, AQUACER-840, AQUACER-1547 etc. manufactured by BYK-Chemie, Nopcoat PEM-17 etc. manufactured by Sannopco, JONCRYL WAX4, JONCRYL WAX26, JONCRYL WAX28, JONCRYL WAX120 etc. manufactured by BASF, HYTEC E series, HYTEC P series, etc., CHALINE FE 230N, CHALINE FE 502, etc. manufactured by Shin-Etsu Chemical Co., Ltd.

[0148] The wax content is preferably 0.2 to 8% by mass, more preferably 0.3 to 5% by mass, and particularly preferably 0.5 to 4% by mass in the total amount of ink from the perspectives of excellent ejection stability, excellent scratch resistance of printed materials, and the ability to obtain high-concentration printed materials without beading.

[0149] In addition, based on the same reasons as above, when the wax content in the total weight of the ink is set to A (mass %) and the binder resin content is set to B (mass %), B÷A is preferably 0.5 to 20, more preferably 1 to 15, and particularly preferably 5 to 15.

[0150] <Surfactant>

[0151] The ink according to the embodiment of the present invention preferably contains one or more surfactants from the viewpoint of obtaining a printed matter having excellent discharge stability, no bleeding and beading, and excellent image quality.

[0152] As the surfactant, various surfactants such as acetylene glycol-based, acetylene alcohol-based, siloxane-based, acrylic acid-based, fluorine-based, and polyoxyalkylene ether-based surfactants can be cited according to the purpose. Among them, it is preferred to contain at least one nonionic surfactant selected from the group consisting of acetylene glycol-based surfactants, siloxane-based surfactants, and polyoxyalkylene ether-based surfactants, more preferably to contain at least one selected from the group consisting of acetylene glycol-based and siloxane-based surfactants, and particularly preferably to contain a siloxane-based surfactant.

[0153] The surfactant that can be used in the present invention may be water-soluble or water-insoluble. It should be noted that a siloxane-based surfactant that is solid at room temperature and melts when heated, for example, at 40 to 200° C., may also serve as the above-mentioned silicone wax.

[0154] Regarding acetylene glycol surfactants and siloxane surfactants, it can be considered that in the ink droplets after landing on the recording medium, they will not be affected by the pigments present in the above droplets, and will be quickly oriented at the gas-liquid interface and the recording medium-droplet interface. As a result, even on the poorly permeable recording medium, it is possible to achieve the improvement of the wettability of the ink and the rapid smoothing of the above ink droplets. In addition to the improvement of the dryness, it is also possible to obtain a printed product with less bleeding and unevenness of the droplets, less bleeding and beading, and excellent image quality. In addition, when using siloxane surfactants, in addition to the above, the wiping resistance of the printed product is also improved, and although the details are unclear, when printing on a highly permeable recording medium such as non-coated paper, the excessive penetration and diffusion of the ink are suppressed, and an excellent printed product without feathering and print-through can be obtained. In particular, in the present invention, although the details are unclear, in addition to the improvement of the above characteristics, an ink with excellent ejection stability can also be obtained, so it is preferred to use acetylene glycol surfactants and siloxane surfactants in combination.

[0155] Examples of the acetylene glycol surfactant used in the present invention include, but are not limited to, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol, hexadec-8-yne-7,10-diol, 6,9-dimethyl-tetradec-7-yne-6,9-diol, 7,10-dimethylhexadec-8-yne-7,10-diol and ethylene oxide and / or propylene oxide adducts thereof.

[0156] In addition, examples of the silicone surfactants that can be preferably used in the present invention include 8032 ADDITIVE, FZ-2104, FZ-2120, FZ-2122, FZ-2162, FZ-2164, FZ-2166, FZ-2404, FZ-7001, FZ-7002, FZ-7006, L-7001, L-7002, SF8427, SF8428, SH3748, SH3749, SH3771M, SH3772M, SH3773M, SH3775M, SH8400, BYK-331, BYK-333, BYK-345, BYK-346, BYK-347, BYK-348, BYK-349, BYK-UV3500, BYK-UV3510, BYK-UV3530, BYK-UV3570 manufactured by BYK Chemical, TEGO manufactured by Evonik Wet 240, TEGO Wet 250, TEGO Wet260, TEGO Wet 270, TEGO Wet 280, TEGO Glide 410, TEGO Glide 432, TEGO Glide 435, TEGO Glide 440, TEGOGlide 450, TEGO Twin 4000, TEGO Twin4100, KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-640, KF-642, KF-643, KF-644, KF-945, KF-6011, KF-6012, KF-6015, KF-6017, KF-6020, KF-6204, X-22-4515 manufactured by Shin-Etsu Chemical Co., Ltd., Silface SAG series of Nissin Chemical Co., Ltd., etc. It is particularly preferred to use a siloxane surfactant in which one or more ethylene oxide groups and / or one or more propylene oxide groups are introduced into the side chain and / or both ends of the polydimethylsiloxane chain.

[0157] Examples of the polyoxyalkylene ether surfactant that can be preferably used in the present invention include compounds represented by the following general formula (1).

[0158] General formula (1):

[0159] RO-(EO)m-(PO)nH

[0160] In the above general formula (1), R represents an alkyl group having 8 to 22 carbon atoms, an alkenyl group having 8 to 22 carbon atoms, an alkylcarbonyl group having 8 to 22 carbon atoms, or an alkenylcarbonyl group having 8 to 22 carbon atoms. In addition, the above R may also be a branched structure. In addition, EO represents an ethylene oxide group, and PO represents a propylene oxide group. m represents the average number of moles of EO added, which is a number from 2 to 50, and n represents the average number of moles of PO added, which is a number from 0 to 50. It should be noted that when n is not 0, there is no restriction on the order of addition of (EO)m and (PO)n, and the addition may be block or random.

[0161] The surfactant used in the present invention preferably exists in a molecule divided into a hydrophobic group and a hydrophilic group. Therefore, among the surfactants exemplified above, it is particularly preferable to select a surfactant having a hydrophilic ethylene oxide group.

[0162] On the other hand, from the viewpoint of improving affinity with the binder resin, obtaining an ink with excellent pigment dispersion stability and ejection stability, and obtaining a printed product without bleeding and beading when printing on a poorly permeable recording medium and without feathering and show-through when printing on a highly permeable recording medium, it is preferred to use a surfactant having an HLB value of 0 to 5, and it is particularly preferred to contain a surfactant having an HLB value of 0 to 4.

[0163] In particular, from the viewpoint of being able to obtain printed materials with excellent image quality with little bleeding and beading on poorly permeable recording media, and having no feathering and print-through on highly permeable recording media such as uncoated paper, in addition to dispersion stability and ejection stability, and having no beading and excellent wetting and spreading properties on non-permeable recording media, it is preferred to use a surfactant having an HLB value of 0 to 5 (preferably 0 to 4) and a surfactant having an HLB value of 6 to 18 (preferably 7 to 18, more preferably 8 to 16, and particularly preferably 10 to 16) in combination. Among them, from the viewpoint of clearly showing the above effects, it is extremely preferred to use an acetylene glycol-based surfactant and a silicone-based surfactant in combination as the surfactant having an HLB value of 0 to 5 (preferably 0 to 4).

[0164] It should be noted that the HLB (Hydrophile-Lipophile Balance) value is one of the parameters that indicates the hydrophilicity or hydrophobicity of a material, and a smaller value indicates a higher hydrophobicity, and a larger value indicates a higher hydrophilicity. Various methods for calculating the HLB value from a chemical structure are known, and various methods for actual measurement are also known. However, in the present invention, when the structure of the compound is clearly known, such as for acetylene glycol-based surfactants and polyoxyalkylene ether-based surfactants, the Griffin method is used to calculate the HLB value. It should be noted that the Griffin method refers to a method for calculating the HLB value using the molecular structure and molecular weight of the target material using the following formula (2).

[0165] Formula (2):

[0166] HLB value = 20 x (total molecular weight of hydrophilic part) / (molecular weight of material)

[0167] On the other hand, in the case of containing a compound of unknown structure such as a siloxane-based surfactant, the HLB value of the surfactant can be experimentally determined by the following method described in, for example, p. 324 of "Surfactant Handbook" (edited by Nishi Ichiro et al., Industrial Book Co., Ltd., 1960). Specifically, 0.5 g of the surfactant is dissolved in 5 mL of ethanol, and the solution is titrated with a 2% by mass phenol aqueous solution while stirring the solution at 25° C., and the position where the liquid becomes turbid is taken as the end point. When the amount of the phenol aqueous solution required to reach the end point is set as A (mL), the HLB value can be calculated by the following formula (3).

[0168] Formula (3):

[0169] HLB value = 0.89 × A + 1.11

[0170] The content of the surfactant in the present invention is preferably 0.2 to 4% by mass, and more preferably 0.5 to 2% by mass, based on the total amount of the ink.

[0171] <Water>

[0172] The water contained in the ink of the embodiment of the present invention is preferably ion exchanged water (deionized water) rather than ordinary water containing various ions, and its content is preferably in the range of 20 to 90% by mass of the total mass of the ink.

[0173] <Other ingredients>

[0174] In the ink of the embodiment of the present invention, in addition to the above-mentioned components, a pH adjuster may be added as needed to prepare an ink having desired physical property values. As compounds that can be used as pH adjusters, in addition to the above-mentioned alkanolamine solvents, for example,

[0175] Other nitrogen-containing compounds include ammonia, monoethylamine, diethylamine, triethylamine, cyclohexylamine, benzylamine, urea, piperidine, etc.

[0176] Examples of alkali metal hydroxides include lithium hydroxide, sodium hydroxide, potassium hydroxide, and the like.

[0177] Examples of alkali metal carbonates include lithium carbonate, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, and the like.

[0178] Acidic compounds include hydrochloric acid, sulfuric acid, acetic acid, citric acid, maleic acid, maleic anhydride, succinic acid, tartaric acid, malic acid, phosphoric acid, boric acid, fumaric acid, malonic acid, ascorbic acid, glutamic acid, etc., but are not limited to these. It should be noted that the above-mentioned pH adjusting agent can be used alone or in combination of two or more. In addition, the above-mentioned alkanolamine solvent can be a material that serves as both an organic solvent and a pH adjusting agent.

[0179] The amount of the pH adjuster blended is preferably 0.01 to 5% by mass, more preferably 0.1 to 3% by mass, and most preferably 0.2 to 1.5% by mass, based on the total amount of the ink.

[0180] In addition, in the ink of the embodiment of the present invention, in addition to the above-mentioned components, in order to make the ink having the desired physical property values, additives such as defoamers, preservatives, infrared absorbers, and ultraviolet absorbers can be appropriately added as needed. The amount of these additives added is preferably 0.01 to 10% by mass relative to the total mass of the ink. On the other hand, the ink of the embodiment of the present invention preferably does not substantially contain a polymerizable monomer.

[0181] <pKa Values ​​of Nitrogen-Containing Compounds>

[0182] As described above, in the ink of the embodiment of the present invention, a nitrogen-containing compound may be used as an organic solvent and / or a pH adjuster. On the other hand, depending on the nitrogen-containing compound used, it is possible to have an adverse effect on the dispersion stability and ejection stability of the pigment, so in the present invention, it is preferred to limit the amount of the nitrogen-containing compound, especially the amount of the nitrogen-containing compound with a molecular weight of 500 or less that is likely to affect the above-mentioned characteristics.

[0183] It should be noted that, in this specification, nitrogen-containing compounds having a molecular weight of 500 or less are collectively referred to as "nitrogen-containing compounds". Specific examples of the nitrogen-containing compounds include substances having a molecular weight of 500 or less among the substances exemplified as the above-mentioned alkanolamine-based solvents, nitrogen-containing solvents, and other nitrogen-containing compounds.

[0184] Usually, in water-based inks containing pigments, the dispersion state of the pigment particles is maintained by the charge repulsion generated between the pigment particles, thereby ensuring dispersion stability. As a method for maintaining dispersion stability for a long time, there is a method of adjusting the pH of the ink to a neutral to weakly alkaline state. By maintaining the pH at a neutral to weakly alkaline state, the ion concentration in the double electric layer covering the surface of the pigment can be increased, the double electric layer repulsion can be increased, and a large repulsion force can be generated between the pigment particles. However, among nitrogen-containing compounds, there are acidic nitrogen-containing compounds or strongly alkaline nitrogen-containing compounds. By using these compounds and pigments in combination, the dispersion stability of the pigment deteriorates, and the ejection stability may also deteriorate. In addition, when wax is further used in combination, the compatibility of the binder resin with respect to the ink deteriorates, and the image quality and abrasion resistance of the printed matter may also deteriorate.

[0185] The present inventors have conducted intensive studies and have found that, among nitrogen-containing compounds, the total amount of nitrogen-containing compounds having a molecular weight of 500 or less and a pKa value of 2 or less (preferably less than 4) or 10 or more (preferably more than 9.5) at 25° C. is preferably 3% by mass or less, more preferably 1% by mass or less, relative to the total amount of the aqueous inkjet ink. This is because these compounds are acidic or strongly basic, and when added in large amounts, as described above, there is a possibility that the dispersion stability, ejection stability, and the scratch resistance and image quality of the printed matter may be adversely affected.

[0186] On the other hand, when a nitrogen-containing compound is used, a basic organic compound having a pKa value of 4 to 9.5 at 25° C. is preferably used. The detailed reason is not clear, but it is considered that a moderately small acid dissociation constant (pKa value) and an organic compound can suppress damage to the pigment and the binder resin (a-1).

[0187] Specific examples of nitrogen-containing compounds having a pKa value of 4 to 9.5 at 25°C include diethanolamine (pKa=8.9), methyldiethanolamine (pKa=8.5), triethanolamine (pKa=7.8), 1-amino-2-propanol (pKa=9.4), diisopropanolamine (pKa=9.0), triisopropanolamine (pKa=8.0), trishydroxymethylaminomethane (pKa=8.1), imidazole (pKa=7.0), and aniline (pKa=4.6). Among the above, alkanolamines are preferably used from the perspective of high solubility in aqueous media and safety to the human body, and triethanolamine having a small pKa value is particularly preferred. It should be noted that the above compounds may be used alone or in combination of two or more.

[0188] When a nitrogen-containing compound having a pKa value of 4 to 9.5 is used, its content is preferably 1.25% by mass or less relative to the total amount of ink. In addition, it is more preferably 0.1 to 1.0% by mass. Within the above range, the dispersion stability and ejection stability will not be deteriorated, and the deterioration of the scratch resistance and image quality of the printed matter can be prevented.

[0189] It should be noted that from the perspective of comprehensively taking into account the dispersion stability, ejection stability, scratch resistance and image quality of the ink, regardless of the pKa value, the total amount of the nitrogen-containing compound is preferably less than 3% by mass, and more preferably less than 1.25% by mass, relative to the total amount of the aqueous inkjet ink.

[0190] In addition, in an embodiment of the present invention, the pKa value can be measured by a known method, such as a potentiometric titration method. In addition, as an example of a nitrogen-containing compound having a pKa value of 2 or less at 25°C, urea (pKa value = 0.2) can be cited. In addition, as an example of a nitrogen-containing compound having a pKa value of 10 or more at 25°C, cyclohexylamine (pKa value = 10.6), monoethylamine (pKa value = 10.7), diethylamine (pKa value = 11.0), triethylamine (pKa value = 10.7), piperidine (pKa value = 11.2) can be cited.

[0191] <Method for producing ink>

[0192] The ink of the embodiment of the present invention containing the above-mentioned components can be manufactured by a known method. In particular, from the viewpoint of obtaining an ink having excellent dispersion stability and ejection stability, it is preferred to select the following manufacturing method: after pre-manufacturing a pigment dispersion containing a pigment, the pigment dispersion, an organic solvent, a binder resin, a wax, and a surfactant as required are mixed. Below, an example of a manufacturing method of the ink of the embodiment of the present invention is described, but as mentioned above, the above-mentioned manufacturing method is not limited to the following.

[0193] (1) Production of pigment dispersion

[0194] (1-1) Dispersion treatment method using a pigment dispersing resin as a water-soluble resin

[0195] When using water-soluble resin as pigment dispersion resin, the above-mentioned pigment dispersion resin, water and organic solvent as required are mixed and stirred to make pigment dispersion resin aqueous solution. In the above-mentioned pigment dispersion resin aqueous solution, pigment and dispersion aid, additional water and additional organic solvent as required are added, after mixing and stirring (premixing), dispersion machine is used to carry out dispersion treatment. Then, centrifugation, filtration and solid component adjustment are carried out as required to obtain pigment dispersion liquid.

[0196] (1-2) Dispersion treatment method using a pigment dispersing resin which is a water-insoluble resin

[0197] In addition, in the case of manufacturing a dispersion of a pigment coated with a pigment dispersion resin as a non-water-soluble resin, the pigment dispersion resin is dissolved in an organic solvent for dissolving a resin such as methyl ethyl ketone in advance, and the above-mentioned pigment dispersion resin is neutralized as needed to make a pigment dispersion resin solution. In the above-mentioned pigment dispersion resin solution, pigment, water and a dispersing aid, an organic solvent, and an additional organic solvent are added, mixed and stirred (pre-mixed), and then a dispersion machine is used for dispersion treatment. Then, the above-mentioned resin dissolving organic solvent is distilled off by reduced pressure distillation, and centrifugation, filtration, and solid component adjustment are performed as needed to obtain a pigment dispersion liquid.

[0198] In the above methods (1-1) and (1-2), the dispersing machine used during the dispersion treatment of the pigment can be any dispersing machine as long as it is a commonly used dispersing machine, for example, a ball mill, a roller mill, a sand mill, a bead mill and a nano high pressure homogenizer (Nanomizer) etc. can be cited. Among the above, a bead mill is preferably used, specifically, it is commercially available under the trade names of Super Mill, Sand Grinder, Agitator Mill, Glen Mill, DYNO-MILL, Pearl Mill and CoBall Mill.

[0199] In the above methods (1-1) and (1-2), as methods for controlling the particle size distribution of the pigment, there can be cited: adjusting the size of the pulverizing medium used in the above dispersing machine; changing the material of the above pulverizing medium; increasing the filling rate of the above pulverizing medium; changing the shape of the stirring member (stirrer); extending the dispersion treatment time; grading by filtering and centrifugal separation after the dispersion treatment; and a combination of these methods. In order to control the pigment within an appropriate particle size distribution range, it is preferred to set the diameter of the pulverizing medium of the above dispersing machine to 0.1 to 3 mm. In addition, as the material of the pulverizing medium, glass, zircon, zirconium oxide, and titanium dioxide are preferably used.

[0200] (1-3) Method for grinding and kneading using pigment dispersion resin

[0201] Furthermore, in the present invention, the method of using grinding and kneading treatment shown below can also be appropriately used. After the pigment, pigment dispersion resin, organic solvent, inorganic salt and the dispersion aid as required are kneaded by a mixer, water is added to the obtained mixture, mixed and stirred. Then, the inorganic salt and the organic solvent as required are removed by centrifugation, filtration and washing, and the solid content is further adjusted to obtain a pigment dispersion.

[0202] The kneading machine used in the above method (1-3) can be any kneading machine as long as it is a commonly used dispersing machine. From the viewpoint of being able to knead a high-viscosity mixture to form a pigment dispersion containing fine pigments, thereby obtaining a printed material with excellent image quality, color development and color reproducibility, a kneading machine or a three-arm mixer is preferably used. It should be noted that by adjusting the temperature during kneading, the particle size distribution of the obtained pigment dispersion can be controlled.

[0203] In addition, as the above-mentioned inorganic salt, sodium chloride, barium chloride, potassium chloride, sodium sulfate, potassium sulfate, etc. can be preferably used.

[0204] (2) Preparation of ink

[0205] The pigment dispersion obtained above is added with a binder resin, wax, an organic solvent, water, and the surfactant, pH adjuster and other additives listed above as needed, and stirred and mixed. It should be noted that the mixture can also be stirred and mixed while being heated at 40 to 100° C. as needed.

[0206] (3) Removal of coarse particles

[0207] The coarse particles contained in the mixture are removed by filtration, centrifugal separation or the like to prepare an aqueous inkjet ink. As the filtration separation method, a known method can be appropriately used. When a filter is used, the pore size is preferably 0.3 to 5 μm, more preferably 0.5 to 3 μm. In addition, when filtering, a single filter can be used or multiple filters can be used in combination.

[0208] <Ink Characteristics>

[0209] The ink of the embodiment of the present invention preferably adjusts the viscosity at 25°C to 3 to 20 mPa·s. If it is in this viscosity range, it shows stable ejection characteristics not only in the head with a frequency of 4 to 10 KHz, but also in the head with a high frequency of 10 to 70 KHz. In particular, by making the viscosity at 25°C 4 to 10 mPa·s, it can be stably ejected even when used for an inkjet head with a design resolution of more than 600 dpi. It should be noted that the above viscosity can be measured by conventional methods. Specifically, an E-type viscometer (TVE25L viscometer manufactured by Toki Sangyo Co., Ltd.) can be used to measure using 1 mL of ink.

[0210] In addition, from the viewpoint of producing an ink that can be stably ejected and obtaining a printed product with excellent image quality, the static surface tension of the ink according to the embodiment of the present invention at 25° C. is preferably 18 to 35 mN / m, and particularly preferably 20 to 32 mN / m. It should be noted that the static surface tension refers to the surface tension measured by the Wilhelmy method under an environment of 25° C. Specifically, CBVP-Z manufactured by Kyowa Interface Science Co., Ltd. can be used for measurement using a platinum plate.

[0211] Furthermore, from the viewpoint that the surfactant is quickly oriented after landing on the recording medium, and excellent image quality is obtained by obtaining appropriate wettability on the recording medium, the dynamic surface tension of the ink according to the embodiment of the present invention at 10 milliseconds based on the maximum bubble pressure method is preferably 26 to 36 mN / m, more preferably 28 to 36 mN / m, and particularly preferably 30 to 36 mN / m. It should be noted that the dynamic surface tension in this specification is a value measured at 25°C using a bubble pressure dynamic surface tension meter BP100 manufactured by Kruss.

[0212] In order to obtain a printed material with excellent color rendering, the ink of the embodiment of the present invention preferably sets the average secondary particle size (D50) of the pigment to 40 to 500 nm, more preferably 50 to 400 nm, and particularly preferably 60 to 300 nm. In order to control the average secondary particle size within the above-mentioned preferred range, the pigment dispersion treatment process is controlled as described above. It should be noted that the average secondary particle size (D50) of the pigment represents the volume-based median particle size measured by a dynamic light scattering method using a particle size distribution measuring machine (in this specification, Nanotrac UPAEX-150 manufactured by Microtrac BEL is used).

[0213] <Set of aqueous inkjet inks>

[0214] The color printing inkjet ink of the embodiment of the present invention may use only one color. Alternatively, the color printing inkjet inks of three colors, cyan, magenta, and yellow, may be used as a set. Furthermore, the color printing inkjet ink (set) may be combined with an ink that exhibits a color other than the color printing color and used as a set of water-based inkjet inks.

[0215] Among them, the color printing inkjet ink of the embodiment of the present invention is preferably used in combination with an ink that exhibits black color (black ink) because a color printed image having a jet-black feel and excellent image quality can be obtained. Furthermore, when printing on a recording medium other than white, a vivid image can be obtained by using it in combination with an ink that exhibits white color (white ink).

[0216] Furthermore, in addition to black ink and white ink, special inks showing purple, blue, red, orange, green, brown, etc. may be used in combination with (a set of) color process color inkjet inks.

[0217] The black ink and / or white ink used in combination with the color printing inkjet ink of the embodiment of the present invention contains a pigment and water. In addition, the black ink and / or white ink may contain an organic solvent, a pigment dispersion resin, a dispersing aid, a binder resin, a wax, a surfactant, a pH adjuster, and other components in addition to the pigment and water. The details of these components are the same as those of the color printing inkjet ink described above.

[0218] In particular, from the viewpoint of obtaining a printed matter with excellent wiping resistance, it is preferred that the black ink and / or white ink contain wax. As the wax, the wax exemplified above can be used as a wax that can be used in a color printing inkjet ink. From the viewpoint of obtaining an ink with excellent ejection stability and wiping resistance of a printed matter, in the case of black ink, the amount of wax is preferably 0.2 to 8% by mass, more preferably 0.3 to 5% by mass, and particularly preferably 0.5 to 4% by mass in the total amount of the black ink. In addition, in the case of white ink, it is preferably 0.1 to 6% by mass, more preferably 0.3 to 5% by mass, and particularly preferably 0.5 to 4% by mass in the total amount of the white ink.

[0219] In addition, when the black ink contains wax, the amount thereof is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and particularly preferably 1.5% by mass or more, more than the amount of wax in the color inkjet ink. Thus, regardless of the drying method and recording medium, the printing density and image quality of all black inkjet inks, cyan inks, magenta inks, and yellow inks can be improved.

[0220] As the pigment used in the black ink, for example, black organic pigments such as aniline black, perylene black and azo black, and black inorganic pigments such as carbon black, ferrosoferric oxide and copper chrome black can be used. In the present invention, carbon black is preferably used because of its high blackness and colorability, the ability to obtain printed materials with high printing density even when added in small amounts, and the ease of availability.

[0221] As the carbon black, self-dispersible carbon black in which hydrophilic functional groups are chemically or physically introduced on the surface of the carbon black and dispersed in an aqueous medium without using a dispersing resin and a surfactant may also be used. In particular, from the perspective of suppressing feathering in a highly permeable recording medium and obtaining a printed product with excellent image quality, the black ink preferably contains self-dispersible carbon black, and more preferably contains self-dispersible carbon black and a resin-dispersible pigment.

[0222] As an example of the above-mentioned self-dispersible carbon black, there can be listed a self-dispersible carbon black in which at least one functional group selected from carboxyl, carbonyl, hydroxyl, sulfonyl, phosphoric acid, phenyl, quaternary ammonium and their salts is introduced directly or through other functional groups through chemical bonds on the surface of the carbon black. The type and amount of the above-mentioned functional group can be appropriately determined while considering the dispersion stability, printing concentration, ejection stability and drying properties of the self-dispersible carbon black in the ink. Among them, from the aspect of obtaining a printed material with a particularly high printing concentration, as the above-mentioned functional group, it is preferred to have an anionic functional group. As the above-mentioned anionic functional group, for example, a functional group selected from carboxyl, carbonyl, hydroxyl, sulfonyl, phosphoric acid and their salts can be listed. Among them, as the above-mentioned functional group, it is preferred to include a carboxyl, carbonyl and hydroxyl.

[0223] It should be noted that commercially available products may be used as self-dispersible carbon black, and examples of such commercially available products include CAB-O-JET series manufactured by Cabot Corporation, BONJET series manufactured by Orient Chemical Industries, Ltd., Aqua-Black series manufactured by Tokai Carbon Co., Ltd., and Fuji-JET Black series manufactured by Fuji Color Co., Ltd.

[0224] The average secondary particle size of the self-dispersible carbon black is, for example, preferably 30 nm to 200 nm, more preferably 50 nm to 170 nm, and particularly preferably 80 nm to 150 nm. The average secondary particle size (D50) refers to the volume-based median particle size measured by a dynamic light scattering method using a particle size distribution measuring instrument (e.g. Nanotrac UPAEX-150 manufactured by MicrotracBEL).

[0225] The total amount of the pigment in the black ink is preferably 1 to 10% by mass, more preferably 2 to 10% by mass, based on the total mass of the black ink.

[0226] On the other hand, examples of organic pigments used in the white ink include hollow resin particles disclosed in Japanese Patent Laid-Open No. 3-26724, Japanese Patent Laid-Open No. 2009-263553, etc. In addition, examples of inorganic pigments include alkaline earth metal sulfates such as barium sulfate, alkaline earth metal carbonates such as calcium carbonate, fine powder silicic acid, silicon dioxides such as synthetic silicates, calcium silicate, aluminum oxide, aluminum oxide hydrate, titanium oxide, zinc oxide, talc, clay, etc. Among them, titanium oxide is most preferred from the viewpoint of concealability and coloring power.

[0227] The total amount of the pigment in the white ink is preferably 3 to 50 parts by mass, more preferably 5 to 30 parts by mass, based on the total mass of the white ink.

[0228] <Ink-Pretreatment Liquid Set>

[0229] The ink of the embodiment of the present invention can also be combined with a pretreatment liquid containing a coagulant and used in the form of an ink-pretreatment liquid set. By applying the pretreatment liquid containing a coagulant to the recording medium, a layer (ink coagulant layer) that intentionally coagulates the solid components contained in the ink can be formed. Moreover, by allowing the ink to land on the above-mentioned ink coagulant layer, it is possible to prevent color bleeding and color unevenness between ink droplets, and significantly improve the image quality of the printed matter. It should be noted that this effect is significant when using a high-permeability recording medium as the recording medium, and a printed matter that is not only excellent in image quality but also excellent in color development and color reproducibility can be obtained. Furthermore, depending on the material used in the pretreatment liquid, the adhesion, abrasion resistance, and adhesion resistance of the printed matter can also be improved.

[0230] The term "flocculating agent" as used herein refers to a component that can disrupt the dispersion state of the pigment and resin particles contained in the ink to cause them to flocculate, and / or insolubilize the water-soluble resin to thicken the ink. The flocculating agent used in the pretreatment liquid combined with the ink of the embodiment of the present invention preferably contains one or more selected from metal salts and cationic polymer compounds from the viewpoint of significantly improving the image quality, color development and color reproducibility. Among them, from the viewpoint of obtaining excellent image quality, color development and color reproducibility, it is preferred to use a metal salt as the above-mentioned flocculating agent, and it is particularly preferred to contain a metal salt selected from Ca 2+ Mg 2+ 、Zn 2+ and Al 3+ When a metal salt is used as the coagulant, the content thereof is preferably 2 to 30% by mass, particularly preferably 3 to 25% by mass, based on the total amount of the pretreatment liquid.

[0231] In other pretreatment liquids, an organic solvent, a surfactant, a pH adjuster, a defoaming agent, an antiseptic, etc. may be appropriately added. The specific materials that can be used are the same as those in the above-mentioned ink.

[0232] It should be noted that, when used in combination with the ink of an embodiment of the present invention, from the viewpoint of obtaining a printed product with excellent image quality, the static surface tension of the pretreatment liquid is preferably 20 to 45 mN / m, more preferably 23 to 40 mN / m. It is particularly preferably 25 to 37 mN / m. It should be noted that the static surface tension of the pretreatment liquid can be measured by the same method as the static surface tension of the ink.

[0233] <Inkjet Recording Method>

[0234] The ink according to the embodiment of the present invention is used in a recording method (inkjet recording method) in which the ink is ejected from an inkjet head and applied to a recording medium.

[0235] It should be noted that, before being applied to a recording medium, the ink is preferably used in a printing device having an ink circulation mechanism that is connected to an inkjet head, from the viewpoint of preventing the drying of the organic solvent and the film formation of the wax, significantly improving the inkjet ejection stability of the ink, and uniformly dispersing the components in the ink to obtain a printed matter without image defects such as bleeding, beading, feathering and show-through.

[0236] As an example of an ink circulation mechanism configured in a manner connected to an inkjet head, there can be cited a system having an inkjet head, an ink supply flow path, an ink discharge flow path, and a pump, wherein the inkjet head has an ink supply port, a nozzle, an ink connection path, and an ink discharge port, the ink supply flow path is connected to the ink supply port, the ink discharge flow path is connected to the ink discharge port, and the pump is connected to the ink supply flow path and / or the ink discharge flow path. In addition, the ink supply flow path and the ink discharge flow path can be directly connected or connected via other structures. As an example of connection via other structures, there can be cited a structure in which one end of the ink supply flow path and one end of the ink discharge flow path are both connected to the same ink tank.

[0237] In addition, in the above-mentioned inkjet head, the ink supplied from the ink supply port passes through either the nozzle or the ink communication path. The ink flowing into the nozzle is ejected from the inkjet head. On the other hand, the ink flowing into the ink communication path is discharged from the ink discharge port, and returns to the inkjet head again via the ink discharge flow path and the ink supply flow path.

[0238] As the passing mode in the above-mentioned inkjet recording method, any one of the single-pass mode in which the inkjet ink is ejected only once to the recording medium for recording, and the serial mode in which the short-sized shuttle head is made to scan back and forth in a direction orthogonal to the conveying direction of the recording medium while ejecting for recording can be adopted. However, in the case of the serial mode, it is necessary to consider the movement of the inkjet head to adjust the ejection timing, and the landing position is prone to deviation. Therefore, when printing the ink of the embodiment of the present invention, it is preferred to use the single-pass mode, and it is particularly preferred to use a mode in which the recording medium passes through the lower part of the fixed inkjet head.

[0239] The method of ejecting ink is not particularly limited, and known methods can be used, such as a drop-on-demand method (pressure pulse method) using the vibration pressure of a piezoelectric element, a thermal inkjet (Bubble Jet (registered trademark)) method that heats the ink to form bubbles and uses the generated pressure, etc. In the present invention, the drop-on-demand method (pressure pulse method) is preferred.

[0240] In view of the large effect of reducing the drying load and improving color reproducibility and other image qualities, the amount of ink droplets ejected from the inkjet head is preferably 0.2 to 30 picoliters, more preferably 1 to 20 picoliters.

[0241] After the ink of the embodiment of the present invention is applied to the recording medium by inkjet printing, it is preferred to have a drying mechanism for the water-based ink on the recording medium. Examples of drying methods used in the drying mechanism include heating drying, hot air drying, infrared drying (e.g., infrared drying with a wavelength of 700 to 2500 nm), microwave drying, and drum drying.

[0242] In the present invention, from the viewpoint of preventing sudden boiling of the liquid component in the ink and obtaining a printed product with excellent color reproducibility and image quality, when the heat drying method is adopted, the drying temperature is preferably set to 35 to 100° C., and when the hot air drying method is adopted, the hot air temperature is preferably set to 50 to 250° C. In addition, from the same viewpoint, when the infrared drying method is adopted, it is preferred that 50% or more of the cumulative value of the total output of infrared rays used in the infrared irradiation exists in the wavelength region of 700 to 1500 nm.

[0243] In addition, the above drying methods may be used alone, in a plurality of ways in succession, or in combination. For example, by using a heating drying method and a hot air drying method in combination, the water-based ink can be dried more quickly than when each method is used alone.

[0244] <Recording Medium>

[0245] The recording medium of the printing ink of the embodiment of the present invention is not particularly limited, and any known recording medium such as a high-permeability recording medium, a poorly permeable recording medium, and an impermeable recording medium can be used. As described above, the ink of the embodiment of the present invention can obtain a printed matter with excellent image quality, color development, and color reproducibility regardless of the permeability of the recording medium.

[0246] In this specification, the permeability of the recording medium is determined based on the water absorption measured by a dynamic scanning absorptometer. Specifically, the water absorption of pure water with a contact time of 100 msec measured by the following method is less than 1 g / m 2 The recording medium is regarded as an "impermeable recording medium", and 1g / m 2 Above and less than 8g / m 2 The recording medium is regarded as "impermeable recording medium", and 8g / m 2 The above recording medium is referred to as a "high-permeability recording medium".

[0247] The water absorption of the recording medium can be measured under the following conditions: Using a dynamic scanning absorptometer KM500win manufactured by Kumagai Riki Kogyo Co., Ltd., at 23°C and 50% RH, the amount of pure water transferred was measured using a recording medium of about 15 to 20 cm square under the following conditions.

[0248] ·Measurement method: Spiral Method

[0249] · Measurement start radius: 20mm

[0250] ·Measurement end radius: 60mm

[0251] Contact time: 10 to 1,000 msec

[0252] Number of sampling points: 19 (measured at approximately equal intervals relative to the square root of the contact time)

[0253] Scanning interval: 7mm

[0254] ·Speed ​​switching angle of the rotating table: 86.3 degrees

[0255] Tip box conditions: Width 5mm, Slit width 1mm

[0256] Examples of high-permeability recording media include: uncoated paper such as straw paper, medium-quality paper, high-quality paper, recycled paper, etc.; fabrics such as cotton, chemical fiber fabrics, silk, linen, non-woven fabrics, etc.; leather, etc. Among them, uncoated paper such as straw paper, medium-quality paper, high-quality paper, recycled paper, etc. is preferred from the viewpoint of obtaining a printed product with excellent ink color development and image quality.

[0257] In addition, examples of non-permeable recording media or poorly permeable recording media include plastic substrates such as polyvinyl chloride, polyethylene terephthalate (PET), polypropylene, polyethylene, nylon, polystyrene, and polyvinyl alcohol, coated paper substrates such as coated paper, coated paper, and cast-coated paper, metal substrates such as aluminum, iron, stainless steel, and titanium, and glass substrates.

[0258] The recording medium listed above can be a recording medium with a smooth surface, or a recording medium with a concave-convex surface, or any one of a transparent, translucent, or opaque recording medium. In addition, it can be a recording medium formed by laminating two or more of these recording media to each other. Furthermore, a peeling adhesive layer can be provided on the opposite side of the printed surface, and an adhesive layer can also be provided on the printed surface after printing. In addition, the shape of the recording medium used in the inkjet recording method of the embodiment of the present invention can be a roll or a single sheet.

[0259] It should be noted that in order to improve the wettability of the ink of the embodiment of the present invention, improve image quality, color reproducibility and drying properties, and also improve the scratch resistance and adhesion to make the printed surface uniform, it is also preferred to perform surface modification such as corona treatment and plasma treatment on the recording medium listed above.

[0260] <Coating treatment>

[0261] The printed matter produced by the ink of the embodiment of the present invention can be coated on the printed surface as needed. As a specific example of the above-mentioned coating treatment, coating or printing using a coating composition, dry lamination, solvent-free lamination, extrusion lamination, etc. can be listed, and any one of them can be selected, or the two can be combined.

[0262] It should be noted that, when the printed matter is subjected to coating treatment by coating or printing the coating composition, as its coating or printing method, any of the methods of printing the recording medium in a non-contact manner as inkjet printing and printing by contacting the coating composition with the recording medium can be adopted. In addition, when selecting the method of printing the coating composition on the recording medium in a non-contact manner, as the above-mentioned coating composition, it is preferred to use an ink (transparent ink) obtained by removing the pigment from the aqueous inkjet ink of the embodiment of the present invention and substantially not containing a colorant component.

[0263] Example

[0264] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples. In the following description, "parts" and "%" respectively represent "parts by mass" and "% by mass" unless otherwise specified.

[0265] <Production Example of Pigment Dispersion Resin 1>

[0266] 93.4 parts of butanol were added to a reaction vessel equipped with a gas introduction tube, a thermometer, a condenser, and a stirrer, and replaced with nitrogen. After heating the reaction vessel to 110°C, a mixture of 30 parts of acrylic acid, 35 parts of styrene, 35 parts of lauryl methacrylate as polymerizable monomers, and 6 parts of V-601 (produced by Wako Pure Chemical Industries, Ltd.) as a polymerization initiator was added dropwise over 2 hours to carry out a polymerization reaction. After the addition was completed, the reaction was carried out at 110°C for 3 hours, and then 0.6 parts of V-601 was added, and the reaction was continued at 110°C for 1 hour. Then, after cooling the reaction system to room temperature, 39 parts of dimethylaminoethanol were added for neutralization, and then 100 parts of water were added. Then, the mixed solution was heated to above 100°C and the butanol was distilled off, and then adjusted with water so that the solid content was 30%, thereby obtaining an aqueous solution of pigment dispersion resin 1 (solid content 30%). The weight average molecular weight of the pigment dispersion resin 1 measured by the method described above was 16,000, and the acid value was 230. The “aqueous solution” referred to above means a solution containing an aqueous solvent and components dispersed and / or dissolved in the aqueous solvent.

[0267] <Production Example of Pigment Dispersion Resin 2>

[0268] In a reaction container equipped with a gas introduction tube, a thermometer, a condenser, and a stirrer, 40 parts of toluene, 40 parts of benzyl methacrylate as a polymerizable monomer, 0.9 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 3.6 parts of 2-(dodecylthiothiocarbonylthio)-isobutyric acid were added, and the atmosphere was replaced with nitrogen. The reaction container was heated to 75° C. and a polymerization reaction was performed for 3 hours to obtain a polymer (A block) composed of benzyl methacrylate.

[0269] After the polymerization reaction was completed, the reaction system was cooled to room temperature, and 40 parts of toluene, 17.5 parts of methyl methacrylate, 32.5 parts of stearyl methacrylate, and 15 parts of methacrylic acid as polymerizable monomers were added to the reaction container, and the atmosphere was replaced with nitrogen. Then, the reaction container was heated to 75° C. and the polymerization reaction was carried out for 3 hours, thereby obtaining an AB block polymer (pigment dispersion resin 2) in which a copolymer (B block) composed of methyl methacrylate, stearyl methacrylate, and methacrylic acid was added to the A block.

[0270] Then, after the reaction system was cooled to room temperature, 25 parts of dimethylaminoethanol were added to the reaction container for neutralization, and then 200 parts of water were added. Next, the mixed solution was heated to distill off toluene, and then water was used to adjust the solid content to 30%, thereby obtaining an aqueous solution of pigment dispersion resin 2 (solid content 30%). It should be noted that the weight average molecular weight of pigment dispersion resin 2 measured by the method described above was 22,000, and the acid value was 150.

[0271] <Production Example of Pigment Dispersed Resin 3>

[0272] The pigment dispersion resin 3 was synthesized according to the raw materials, input amounts and operations disclosed in Preparation Example 8 of Japanese Patent Application Laid-Open No. 2020-203965. Then, the obtained pigment dispersion resin 3 was mixed with water and adjusted so that the solid content was 30%, thereby obtaining an aqueous solution (solid content 30%) of the pigment dispersion resin 3. It should be noted that the weight average molecular weight of the pigment dispersion resin 3 measured by the method described above was 13,000, and the acid value was 105.

[0273] <Production Example of Pigment Dispersed Resin 4>

[0274] X-200 manufactured by Seikyo PMC Co., Ltd. (weight average molecular weight 12,000, acid value 190, hereinafter referred to as "pigment dispersion resin 4") was mixed with water and adjusted to a solid content of 30%, thereby obtaining an aqueous solution of pigment dispersion resin 4 (solid content 30%).

[0275] <Production Example of Pigment Dispersion Liquid>

[0276] In a mixing container equipped with a stirrer, 15 parts of a pigment, 15 parts of an aqueous solution of a pigment dispersion resin (solid content 30%), and 70 parts of water were sequentially added and pre-mixed. Then, a DYNO-MILL with a volume of 0.6 L and filled with 1800 g of zirconia beads with a diameter of 0.5 mm was used for formal dispersion to obtain a pigment dispersion (pigment concentration 15%).

[0277] The pigments used in the preparation of the pigment dispersion are as follows.

[0278] · CI Pigment Blue 15:3: TOYO Color Co., Ltd. "LIONOGEN BLUE FG-7358G"

[0279] CI Pigment Red 150: "TOSHIKI RED 150TR" manufactured by Tokyo Color Co., Ltd.

[0280] CI Pigment Red 122: DIC Corporation's "FASTGEN SUPER MAGENTA RG"

[0281] · CI Pigment Yellow 12: DIC Corporation's "SYMULER FAST YELLOW GFCONC"

[0282] CI Pigment Yellow 74: Clariant "HANSA YELLOW 5GX01"

[0283] · CI Pigment Yellow 14: DIC Corporation's "SYMULER FAST YELLOW 4400"

[0284] In addition, the combinations of the produced pigment dispersions, the pigments used as raw materials, and the pigment dispersion resins are shown in Table 1 below.

[0285] [Table 1]

[0286] Table 1

[0287]

[0288] <Production Example of Resin Particles 1 to 3 (Styrene Methacrylate Resin Particles)>

[0289] 40 parts of water and 0.2 parts of Aqualon KH-10 (produced by Daiichi Kogyo Seiyaku) as a surfactant were added to a reaction vessel equipped with a gas introduction tube, a thermometer, a condenser, and a stirrer to prepare a surfactant aqueous solution. Separately, 25 parts of styrene as a polymerizable monomer, 3 parts of methacrylic acid, 62 parts of methyl methacrylate, 10 parts of butyl acrylate, 1.8 parts of Aqualon KH-10 as a surfactant, and 51.2 parts of water were added to another mixing vessel and mixed thoroughly to prepare an emulsion precursor.

[0290] 1.5 parts of the prepared emulsion precursor were added to a reaction vessel containing an aqueous surfactant solution and mixed thoroughly. Next, the temperature in the reaction vessel was raised to 60°C, and after replacing with nitrogen, 1 part of a 5% aqueous solution of potassium persulfate and 0.2 parts of a 1% aqueous solution of anhydrous sodium hydrogen sulfite were added, and the polymerization reaction was started while the reaction vessel was kept at 60°C. After reacting at 60°C for 5 minutes, the remaining components (151.5 parts) of the emulsion precursor, 9 parts of a 5% aqueous solution of potassium persulfate and 1.8 parts of a 1% aqueous solution of anhydrous sodium hydrogen sulfite were added dropwise over 1.5 hours, and the reaction was further continued for 2 hours. Then, after the reaction system was cooled to 30°C, diethylaminoethanol was added to adjust the pH of the mixed solution to 8.5, and water was used to adjust the solid content to 30%, thereby obtaining an aqueous dispersion of resin particles 1 (solid content 30%) as styrene methacrylate resin particles.

[0291] In addition, except that the polymerizable monomer was changed to the one described in Table 2, the same operation as the above-mentioned resin particle 1 was carried out to obtain aqueous dispersions (solid content: 30%) of resin particles 2 and 3 which are styrene methacrylate resin particles.

[0292] [Table 2]

[0293] Table 2

[0294]

[0295] In addition, the acid value, glass transition temperature, and weight average molecular weight of resin particles 1 to 3 are also described in Table 2. In addition, the abbreviations of the polymerizable monomers described in Table 2 are as follows.

[0296] St: Styrene

[0297] MAA: Methacrylic acid

[0298] MMA: Methyl methacrylate

[0299] BA: Butyl acrylate

[0300] · PME-400: Methoxy polyethylene glycol methacrylate (Blemmer PME-400 manufactured by NOF Corporation)

[0301] <Production Example of Resin Particles 4 (Urethane Resin Particles)>

[0302] In a reaction vessel equipped with a gas introduction pipe, a thermometer, a condenser, and a stirrer, 150 parts of methyl ethyl ketone, 69 parts of polycarbonate diol (molecular weight 2,000) with 1,6-hexanediol as the main skeleton, 11.8 parts of isophorone diisocyanate, 9 parts of hexamethylene diisocyanate, and 8.3 parts of dimethylol propionic acid were added, and after replacing with nitrogen, the reaction vessel was heated to 80°C and a polymerization reaction was carried out for 6 hours. Then, 1.9 parts of trimethylolpropane was further added, and the reaction was continued at 80°C. Then, after the reaction system was cooled to room temperature, water was added, and then potassium hydroxide aqueous solution was added while stirring to neutralize. Then, the mixed solution was heated under reduced pressure to distill off the methyl ethyl ketone, and then adjusted with water so that the solid content was 40%, thereby obtaining an aqueous dispersion of resin particles 4 (solid content 40%) as urethane resin particles. The weight average molecular weight of the resin particles 4 measured by the method described above was 20,000, and the acid value was 37.

[0303] <Production Examples of Water-Soluble Resins 1 to 3>

[0304] Aqueous solutions (solid content 40%) of water-soluble resins 1 to 3, which are (meth)acrylic acid water-soluble resins or styrene (meth)acrylate water-soluble resins, were obtained by the same operation as the above-mentioned pigment dispersion resin 1, except that the composition of the mixture added dropwise to butanol (the type and amount of polymerizable monomers and the amount of V-601), the amount of V-601 added after reacting at 110° C. for 3 hours, and the amount of dimethylaminoethanol (DMAE) used for neutralization were changed to those described in Table 3. It should be noted that the acid value, glass transition temperature, and weight average molecular weight of the water-soluble resins 1 to 3 are also described in Table 3.

[0305] [Table 3]

[0306] Table 3

[0307]

[0308] <Production Example of Color Process Ink Sets 1 to 56>

[0309] The following materials were sequentially added to a mixing container while being stirred with a disperser, and stirred until fully uniform. Then, the mixture was filtered with a membrane filter having a pore size of 1 μm to prepare cyan ink 1. In addition, magenta ink 1 and yellow ink 1 were prepared in the same manner as the cyan ink, except that pigment dispersions M1 and Y1 were used instead of pigment dispersion C1. The cyan ink 1, magenta ink 1 and yellow ink 1 were used as a set 1 of color process inks.

[0310]

[0311] In addition, color process ink sets 2 to 56 were obtained by the same method as the color process ink set 1 except that the materials described in the following Table 4 were used.

[0312] [Table 4]

[0313] Table 4

[0314]

[0315] [Table 4]

[0316] Table 4 (continued)

[0317]

[0318] [Table 4]

[0319] Table 4 (continued)

[0320]

[0321] [Table 4]

[0322] Table 4 (continued)

[0323]

[0324] It should be noted that the "combination of pigment dispersions" in Table 4 represents the combination of pigment dispersions used in the production of cyan ink, magenta ink, and yellow ink contained in the group of color printing inks. Specifically, the above-mentioned cyan ink, magenta ink, and yellow ink were produced according to the combination shown in Table 5 below.

[0325] [Table 5]

[0326] Table 5

[0327]

[0328] In addition, the materials described in Table 4 are as follows.

[0329] (wax)

[0330] P5300: HYTEC P5300 (manufactured by Toho Chemical Industry Co., Ltd., polypropylene wax, 30% solid content aqueous dispersion, melting point 146°C, average particle size 78 nm)

[0331] AQ515: AQUACER 515 (manufactured by BYK Chemicals, polyethylene wax, 35% solid content aqueous dispersion, melting point 135°C, average particle size 36 nm)

[0332] AQ541: AQUACER 541 (manufactured by BYK Chemicals, polyethylene wax, 30% solid content aqueous dispersion, melting point 80°C, average particle size 180 nm)

[0333] FE230N: CHALINE FE230N (manufactured by Nissin Chemical Industry Co., Ltd., silicone wax, 30% solid content water dispersion, average particle size 270 nm)

[0334] (Water-soluble organic solvent)

[0335] MP: Propylene glycol monomethyl ether (boiling point 121°C, surface tension 26mN / m)

[0336] MB: 3-methoxy-1-butanol (boiling point 158°C, surface tension 29 mN / m)

[0337] ·MMB: 3-methoxy-3-methyl-1-butanol (boiling point 174°C, surface tension 30 mN / m)

[0338] PG: Propylene glycol (boiling point 188°C, surface tension 35mN / m)

[0339] 2,3-BD: 2,3-butanediol (boiling point 182°C, surface tension 35 mN / m)

[0340] IPA: Isopropyl alcohol (boiling point 82°C, surface tension 21mN / m)

[0341] ·DEDG: Diethylene glycol diethyl ether (boiling point 189°C, surface tension 23mN / m)

[0342] 1,2-BD: 1,2-butanediol (boiling point: 191°C, surface tension 32 mN / m)

[0343] HeG: Ethylene glycol monohexyl ether (boiling point: 208°C, surface tension 25 mN / m)

[0344] 1,2-HeD: 1,2-hexanediol (boiling point 223°C, surface tension 26mN / m)

[0345] BDG: diethylene glycol monobutyl ether (boiling point: 230°C, surface tension 28 mN / m)

[0346] ·GY: Glycerin (boiling point: 290°C, surface tension 62mN / m)

[0347] (Surfactant)

[0348] S.104: Surfynol 104 (Nissin Chemical Industry Co., Ltd., acetylene glycol surfactant, HLB value: 3.0)

[0349] S.465: Surfynol 465 (Nissin Chemical Industry Co., Ltd., acetylene glycol surfactant, HLB value: 13.2)

[0350] ·TW280: TEGO Wet 280 (silicone surfactant manufactured by Evonik, HLB value: 3.5)

[0351] (pH adjuster)

[0352] DMAE: dimethylaminoethanol (pKa value: 9.9, boiling point: 133°C)

[0353] APOH: 1-amino-2-propanol (pKa value: 9.4, boiling point: 159°C)

[0354] ·TEA: triethanolamine (pKa value: 7.8, boiling point: 335°C)

[0355] ·NaOH: 20w / v% sodium hydroxide aqueous solution

[0356] (other)

[0357] · Proxel GXL: 1,2-Benzisothiazol-3-one solution (preservative) manufactured by ARCH Chemicals

[0358] [Examples 1 to 51, Comparative Examples 1 to 5]

[0359] The aqueous inkjet inks 1 to 56 produced above were subjected to the following evaluations 1 to 6. The evaluation results are shown in Table 4.

[0360] <Evaluation 1: Evaluation of discharge stability>

[0361] Three Samba G3L (manufactured by FUJIFILM Dimatix) as inkjet heads were set on the upper part of a conveyor capable of conveying recording media, and a pump and an ink tank were prepared for each Samba G3L. In addition, the Samba G3L has a design resolution of 1200 dpi and is equipped with an ink supply port, a nozzle, an ink communication path, and an ink discharge port. Next, three tubes were prepared for one Samba G3L, and the ink supply port of the Samba G3L and the pump, the pump and the ink tank, and the ink tank and the ink discharge port of the Samba G3L were connected respectively.

[0362] Next, the groups 1 to 56 of the color printing ink manufactured above are filled into the above tanks respectively, the above pump is operated, the inkjet head and the flow path are filled with ink, and then the nozzle detection pattern is printed. After confirming that no nozzles have fallen off, stand by for a specified time under an environment of 25°C while the above pump is operated. Then, the nozzle detection pattern is printed again, and the number of nozzles that have fallen off is counted to evaluate the ejection stability. The evaluation criteria are as follows, and the evaluation criteria values ​​2 to 4 are used as the practical range. It should be noted that the evaluation results recorded in Table 4 are the evaluation results of the color with the worst evaluation results among the three color inks evaluated.

[0363] 4: Even after 3 hours of standby, there was no nozzle fall off at all.

[0364] 3: Even after 2 hours of standby, no nozzles fell off at all, but after 3 hours of standby, one or more nozzles fell off.

[0365] 2: Even after standing by for 1 hour, no nozzles fell off at all, but after standing by for 2 hours, one or more nozzles fell off.

[0366] 1: After one hour of standby, one or more nozzles fell off.

[0367] <Evaluation 2: Evaluation of Image Quality (Bleeding)>

[0368] In the inkjet printing device used in Evaluation 1, the above-produced color ink sets 1 to 56 were filled in the order of cyan, magenta, and yellow from the upstream side. After the pump was operated to fill the inkjet head and the flow path with ink, the ink was printed on OK Topcoat+ (coated paper, square meter weight 104.7 g / m2) manufactured by Oji Paper Co., Ltd. 2 ) is printed on a 5cm×5cm solid-color block (printing rate 100%) in the order of cyan, magenta, yellow, and cyan to form an image (solid-color block image).

[0369] Within 10 seconds after printing, the printed material was placed in an air oven at 70°C and dried for 1 minute. Then, the printed material was taken out of the oven, and the degree of bleeding at the boundaries between the color blocks was confirmed by a magnifying glass and visual inspection to evaluate the image quality (bleeding). The evaluation criteria are as follows, and the evaluation criteria values ​​2 to 4 are used as the practical area. It should be noted that the evaluation results recorded in Table 4 are the evaluation results of the worst evaluation results.

[0370] 4: When observed through a magnifying glass and visually, no boundary bleeding was observed.

[0371] 3: Boundary bleeding was slightly observed under a magnifying glass, but the presence or absence of boundary bleeding could not be determined visually.

[0372] 2: Boundary bleeding was observed visually, but the degree was small.

[0373] 1: Clear boundary bleeding is visually observed.

[0374] <Evaluation 3: Evaluation of Image Quality (Beading: Coated Paper)>

[0375] In the inkjet printing device used in Evaluation 1, the above-produced color ink sets 1 to 56 were filled in the order of cyan, magenta, and yellow from the upstream side. After the pump was operated to fill the inkjet head and the flow path with ink, the ink was printed on OK Topcoat+ (coated paper, square meter weight 104.7 g / m2) manufactured by Oji Paper Co., Ltd. 2 ) is printed on a screen with three color blocks arranged at intervals so that the total printing rate (the total printing rate of each color) changes from 30% to 240% by 30% (gradation color block image). In addition, the printing rates of cyan ink, magenta ink, and yellow ink in each color block are set to be the same. For example, a color block with a total printing rate of 240% is an image with a printing rate of cyan ink set to 80%, a printing rate of magenta ink set to 80%, and a printing rate of yellow ink set to 80%.

[0376] Within 10 seconds after printing, the printed material was placed in an air oven at 70°C and dried for 1 minute. The printed material was then taken out of the oven and visually observed for unevenness in density to evaluate beading of the coated paper. The evaluation criteria were as follows, with evaluation criteria values ​​of 2 to 4 being the practical range.

[0377] 4: No unevenness in density was observed at all total printing rates.

[0378] 3: When the total printing rate is 210% or less, no unevenness in density is observed.

[0379] 2: When the total printing rate is 180% or less, no unevenness in density is observed.

[0380] 1: Uneven density was clearly observed at a total printing rate of 180%.

[0381] <Evaluation 4: Evaluation of scratch resistance>

[0382] The inkjet printing device used in Evaluation 1 was filled with the color ink sets 1 to 56 prepared above. The pump was operated to fill the inkjet head and the flow path with ink. Then, the ink was coated with OK Topcoat+ (coated paper, square meter weight 104.7 g / m2) manufactured by Oji Paper Co., Ltd. 2 ) and put the printed matter into an air oven at 70°C within 10 seconds. After drying for 1 minute, take the printed matter out of the oven and wipe it a specified number of times with a test white cotton cloth (KANAKIN No. 3) while applying a load of 200g to each color. Then, visually observe the printed matter after wiping to evaluate the wipe resistance. The evaluation criteria are as follows, and the evaluation criteria values ​​2 to 4 are used as the practical range. It should be noted that the evaluation results recorded in Table 4 are the evaluation results of the colors with the worst evaluation results.

[0383] 4: Even after wiping 20 times, no scratches on the printed surface and no peeling of the ink were found.

[0384] 3: Even after wiping 10 times, no scratches on the printed surface and no peeling of the ink were observed. However, after wiping 20 times, scratches on the printed surface and no peeling of the ink were observed.

[0385] 2: Even after wiping 5 times, no scratches on the printed surface and no ink peeling were observed. However, after wiping 10 times, scratches on the printed surface and no ink peeling were observed.

[0386] 1: After wiping 5 times, scratches on the printed surface and peeling of ink were observed.

[0387] <Evaluation 5: Evaluation of Image Quality (Feathering)>

[0388] The inkjet printing device used in Evaluation 1 was filled with the color printing ink groups 1 to 56 prepared above. After the pump was operated to fill the inkjet head and the flow path with ink, an image (thin line image) of 5 cm long single-color thin lines arranged at intervals was printed on OK Prince (high-quality paper) manufactured by Prince Paper Co., Ltd. It should be noted that the image was printed on OK TopCoat+ (coated paper, square meter weight 104.7 g / m 2 ) is used to print the above-mentioned fine line image, and the image data and the head driving conditions are adjusted in such a way that the width of the above-mentioned single-color fine line becomes 100μm.

[0389] Within 10 seconds after printing, the printed material was placed in an air oven at 70°C and dried for 1 minute. The printed material was then taken out of the oven and visually observed for the presence or absence of fine line bleeding to evaluate feathering. The evaluation criteria are as follows, with evaluation criteria values ​​2 to 4 being the practical range. It should be noted that the evaluation results recorded in Table 4 are the evaluation results of the color with the worst evaluation results.

[0390] 4: Thin lines do not become thicker due to bleeding, and no ink bleeding along paper fibers is observed.

[0391] 3: Although thin lines do not become thicker due to bleeding, ink bleeding along paper fibers is observed at less than 10 locations.

[0392] 2: The thin line becomes slightly thicker due to bleeding, and ink bleeding along the paper fibers is observed at 10 or more and less than 20 locations.

[0393] 1: Thin lines become thicker due to bleeding, and ink bleeding occurs at 20 or more locations along paper fibers.

[0394] <Evaluation 6: Evaluation of print-through>

[0395] In the inkjet printing device used in Evaluation 1, groups 1 to 56 of the color printing inks manufactured above are filled respectively. After the pump is operated to fill the inkjet head and the flow path with ink, a full-page image (printing rate 100%) is printed in each color on NPi form 55 (high-quality paper) manufactured by Nippon Paper Manufacturing Co., Ltd., and the printed material is placed in an air oven at 70°C within 10 seconds. After drying for 1 minute, the printed material is taken out of the oven, and the optical density (OD value) of the back of the full-page image is measured to evaluate the print-through. It should be noted that a spectrophotometer (eXact manufactured by X-RITE Co., Ltd.) is used, the light source is D50, the viewing angle is 2°, the concentration state is ISO Status T, and the concentration white reference is an absolute value. In addition, the evaluation criteria are as follows, and the evaluation criteria values ​​2 to 5 are used as the practical area. The evaluation results recorded in Table 4 are the evaluation results of the colors with the worst evaluation results.

[0396] 5: OD value is less than 0.14

[0397] 4: OD value is above 0.14 and less than 0.17

[0398] 3: OD value is above 0.17 and less than 0.20

[0399] 2: OD value is above 0.20 and less than 0.23

[0400] 1: OD value 0.23 or above

[0401] The evaluation results confirmed that the color printing inkjet ink containing water, pigment, organic solvent, binder resin and wax, and also containing two or more organic solvents with a boiling point of 190°C or less, and the S / R value is 3.0 or less when the amount of the organic solvent with a boiling point of 150°C or more at 1 atmosphere of pressure relative to the total amount of ink is set to S, and the content of the above-mentioned binder resin relative to the total amount of ink is set to R, has excellent ejection stability, and has practical quality for beading, bleeding and abrasion resistance on coated paper, and feathering and print-through when using high-quality paper.

[0402] [Examples 52 to 62]

[0403] The color process ink groups 41 to 51 produced above were further subjected to the following evaluations 7 to 9 to confirm the wetting and spreading, beading, and blocking resistance to the non-permeable recording medium. The evaluation results are shown in Table 6.

[0404] [Table 6]

[0405] Table 6

[0406]

[0407] <Evaluation 7: Evaluation of Image Quality (Beading: Film)>

[0408] Beading of the film was evaluated by the same method and evaluation criteria as in the above Evaluation 3 except that FOR#20 (biaxially stretched polypropylene film, thickness 20 μm) manufactured by FUTAMURA CHEMICAL was used as the recording medium.

[0409] <Evaluation 8: Evaluation of image quality (wetting and spreading properties)>

[0410] In the inkjet printing device used in Evaluation 1, the groups 41 to 51 of the color printing inks manufactured above are filled in the order of cyan, magenta, and yellow from the upstream side. After the pump is operated and the inkjet head and the flow path are filled with ink, a full-page image (printing rate 100%) is printed in each color on FOR#20 (2-axis stretched polypropylene film, thickness 20 μm) manufactured by FUTAMURACHEMICAL, and the printed matter is placed in a 70°C air oven within 10 seconds. After drying for 1 minute, the printed matter is taken out of the oven, and the degree of inversion is confirmed by a magnifying glass and visually, thereby evaluating the wetting and extensibility. The evaluation criteria are as follows, and the evaluation criteria values ​​2 to 4 are used as the practical area. It should be noted that the evaluation results recorded in Table 6 are the evaluation results of the colors with the worst evaluation results.

[0411] 4: No reflection is observed when observing with a magnifying glass or visually.

[0412] 3: Slight whitening is observed under a magnifying glass, but the presence or absence of whitening cannot be determined visually.

[0413] 2: Whitening is observed visually, but the degree is small.

[0414] 1: Clear whitening is visually observed.

[0415] <Evaluation 9: Evaluation of Blocking Resistance>

[0416] In the inkjet printing device used in Evaluation 1, the groups 41 to 51 of the color printing inks manufactured above are filled in the order of cyan, magenta, and yellow from the upstream side. After the pump is operated to fill the inkjet head and the flow path with ink, a full-page color block image is printed on FE2001 (PET film, thickness 12μm) manufactured by FUTAMURA CHEMICAL, and the printed matter is placed in an air oven at 70°C within 10 seconds. After drying for 2 minutes, the printed matter is taken out of the oven and cut into 4cm×4cm squares for each color. It should be noted that for cyan, only one of the two full-page color blocks present in the printed matter is used.

[0417] Next, the printed surface of the cut solid color block was overlapped with the back side (non-printed surface) of FE2001 manufactured by FUTAMURA CHEMICAL to prepare a test piece, which was then placed in a permanent strain tester. The environmental conditions were a load of 10 kg / cm 2, temperature 40 ℃, 80% RH, and stand for 24 hours. Then, after taking out the test piece from the permanent strain tester, the overlapping PET film is instantly stretched and peeled off while maintaining an angle of 90 degrees, and the printed surface after peeling is visually confirmed to evaluate the blocking resistance. The evaluation criteria are as follows, and the evaluation criteria values ​​2 to 4 are used as the practical range. It should be noted that the evaluation results recorded in Table 6 are the evaluation results of the color with the worst evaluation results.

[0418] 4: The printed surface is not removed at all.

[0419] 3: The removal of the printed surface is 10% or less of the total area.

[0420] 2: The removal of the printed surface exceeds 10% and is 30% or less of the total area.

[0421] 1: The removal of the printed surface exceeds 30% of the total area.

[0422] The disclosure of this application is related to the subject matter described in Japanese Patent Application No. 2020-201541 filed on December 4, 2020, and all the disclosed contents are incorporated herein by reference.

Claims

1. A color printing inkjet ink comprising water, a pigment, an organic solvent, a binder resin and a wax, The organic solvent includes an organic solvent having a boiling point of 190° C. or less at 1 atmosphere pressure, The organic solvent having a boiling point of 190° C. or less under 1 atmosphere pressure comprises a divalent alcohol solvent and a glycol monoalkyl ether solvent, and When the amount of the organic solvent having a boiling point of 150° C. or higher at 1 atmosphere relative to the total amount of ink is represented by S, and the content of the binder resin relative to the total amount of ink is represented by R, the S / R value is 1.2 to 2.

8. 2 . The color process inkjet ink according to claim 1 , wherein the weighted average boiling point of the organic solvent at 1 atmosphere is 120 to 180° C.

3. According to the color printing inkjet ink according to claim 1 or 2, the organic solvent having a boiling point of less than 190°C under 1 atmosphere of pressure comprises more than two organic solvents, and among the more than two organic solvents, the difference between the boiling points of the organic solvent with the highest boiling point and the organic solvent with the lowest boiling point is 10 to 100°C.

4. The color process inkjet ink according to claim 1 or 2, wherein the wax comprises a polyolefin wax having a melting point of 80 to 180°C.

5. The process color inkjet ink according to claim 1 or 2, wherein the amount of the organic solvent having a boiling point exceeding 190°C at 1 atmosphere is 1% by mass or less based on the total amount of the ink.

6. Use of the color printing inkjet ink according to any one of claims 1 to 5 in a printing device having an ink circulation mechanism connected to an inkjet head.

Citation Information

Patent Citations

  • Hollow polymer particle and preparation thereof

    JP1991026724A

  • Hollow resin particle

    JP2009263553A

  • Inkjet ink and inkjet recording method

    JP2009280671A

  • Inkjet water-based ink and inkjet recording method

    JP2012001611A

  • Water-based pigment ink for inkjet

    JP2012136573A