Preparation and application of a nucleic acid extraction material of chitosan-modified attapulgite
By acid activation and chitosan modification of concave and convex rod soil, efficient nucleic acid adsorption materials were prepared, which solved the problems of high cost and low efficiency of existing nucleic acid extraction materials, and achieved efficient and low-cost DNA extraction and high purity nucleic acid acquisition.
Patent Information
- Application Number
- CN202310437817.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-21
AI Technical Summary
The existing nucleic acid extraction materials have high cost or low efficiency, especially in the solid-phase carrier adsorption method, the silica and magnetic bead methods have problems such as cumbersome operation and high cost.
By acid activation and chitosan modification of concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and con
The adsorption and extraction of nucleic acids with low cost and high efficiency are achieved. The saturated adsorption of DNA by chitosan-modified concave and convex rod soil is better than that of magnetic beads coated with silica and lithium-modified montmorillonite, and the desorption rate reaches 90%. The above, and the extracted DNA has high purity.
Smart Images

Figure CN116393105B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nucleic acid extraction material preparation, and specifically relates to the preparation and application of a chitosan-modified attapulgite nucleic acid extraction material. Background Art
[0002] Nucleic acid extraction currently focuses on solid phase carrier adsorption method. The operation steps of this method can be mainly divided into three parts: (1) using lysis solution to cause cell rupture and release nucleic acid into the liquid phase; (2) using the carrier's strong affinity and adsorption capacity for nucleic acid to specifically bind the released nucleic acid to a specific carrier, so that other impurities such as proteins, polysaccharides and lipids remain free in the liquid phase and are removed with the removal of the supernatant; (3) by adjusting the ionic strength and pH value of the elution solution, the nucleic acid adsorbed on the carrier is eluted to obtain the purified nucleic acid.
[0003] At present, the solid phase materials reported to have nucleic acid adsorption function mainly include silica and its derivatives and magnetic beads, which bind and separate nucleic acids through electrostatic interaction, covalent bonding and other mechanisms. As inorganic nanoparticles, silica nanoparticles have the characteristics of stable chemical properties, low price and large specific surface area. They can be evenly dispersed in the lysate system and are widely used for nucleic acid solid phase separation. Most of the centrifugal column method nucleic acid extraction uses silica filter membrane as a solid phase carrier, based on the unique property of silica to selectively bind DNA. The principle is that under high salt conditions (pH ≤ 7), sodium ions can destroy the hydrogen bond between hydrogen in water and negatively charged oxygen in silicon. After a large amount of rinsing to remove all impurities, the purified DNA is eluted with buffer or distilled water at low ionic strength (pH ≥ 7), but this method requires tedious operations such as centrifugation and filtration. The main principle of magnetic bead method nucleic acid extraction is to use particles with magnetic properties and surface coated with active groups to separate nucleic acids; the active groups coated on the surface of magnetic beads can be used as solid phase extraction carriers by specifically adsorbing nucleic acids. The magnetic bead extraction method can realize automation and high-throughput operation, and can improve the efficiency of nucleic acid extraction with an automatic nucleic acid extractor, but the magnetic bead extraction method is relatively expensive. Therefore, there is an urgent need for a low-cost and high-efficiency nucleic acid extraction material. Summary of the invention
[0004] In order to solve the problems of high cost or low efficiency of current nucleic acid extraction materials, the present invention provides a preparation method and application of chitosan-modified attapulgite adsorption material by improving attapulgite, thereby achieving the effect of improving the adsorption performance of modified attapulgite for nucleic acids.
[0005] The present invention provides a method for preparing a chitosan-modified attapulgite adsorption material, and the specific operation steps are as follows:
[0006] S1. Acid activation modification: The attapulgite powder is stirred and reacted with an aqueous solution of HCl, filtered, the solid is washed, dried, and then ground and sieved to obtain acid-activated attapulgite.
[0007] S2. Chitosan modification: chitosan and acid-activated attapulgite are added to hydrochloric acid, stirred, the pH is adjusted to neutral, the solution is dried, the solid obtained by grinding and drying is sieved to obtain chitosan-modified attapulgite.
[0008] Furthermore, the mesh size of the attapulgite powder in step S1 is greater than 325 meshes.
[0009] Furthermore, the concentration of the HCl aqueous solution in step S1 is 5-15 wt %, and can be specifically 10 wt %.
[0010] Furthermore, in step S1, the mass volume ratio of the attapulgite powder and the HCl aqueous solution is 1 g: (5-15) mL, and can be specifically 1 g: 10 mL.
[0011] Furthermore, in step S1, the stirring is carried out at 50-90° C. for 1-3 hours, and specifically at 70° C. for 2 hours.
[0012] Furthermore, the sieving in step S1 is through a 325-mesh standard sieve.
[0013] Furthermore, in step S2, the mass ratio of acid-activated attapulgite to chitosan is 10:(0.5-1.5), and can be specifically 10:1.
[0014] Furthermore, in step S2, the concentration of hydrochloric acid is 0.5-1.5 wt %, and can be specifically 1 wt %.
[0015] Furthermore, in step S2, the mass volume ratio of the acid-activated attapulgite and the hydrochloric acid is 2g:(100-500)mL, and can be specifically 2g:300mL.
[0016] Furthermore, in step S2, the stirring is carried out at 50-70° C. for 20-28 hours, and specifically at 60° C. for 24 hours.
[0017] Furthermore, the sieving in step S2 is through a 325-mesh standard sieve.
[0018] The invention provides a chitosan-modified attapulgite adsorption material.
[0019] The chitosan-modified attapulgite adsorption material provided by the invention is applied in the field of nucleic acid adsorption.
[0020] The present invention provides a method for extracting DNA from a chitosan-modified attapulgite adsorption material, and the specific operating steps are as follows:
[0021] The attapulgite suspension is prepared, and the attapulgite suspension, the solution containing DNA and the buffer solution are mixed, shaken, centrifuged and the precipitate after centrifugation is collected.
[0022] Furthermore, the concentration of the attapulgite sample suspension is 10-50 mg / mL, and can be specifically 30 mg / mL.
[0023] Furthermore, the solution containing DNA is a solution containing 1 to 900 μg / mL DNA.
[0024] Specifically, the solution containing DNA is a solution containing 100-200 μg / mL fish sperm DNA, or a Staphylococcus aureus cell lysate containing DNA.
[0025] Furthermore, the volume ratio of the attapulgite sample suspension to the solution containing DNA is 1:(1-20).
[0026] Preferably, the volume ratio of the attapulgite sample suspension to the solution containing DNA is 1:(5-15).
[0027] Furthermore, the buffer solution is a CH3COOH-CH3COONa solution.
[0028] Further, after adding the buffer solution, the pH of the system is 3-8, Na + The concentration is 10~600mM.
[0029] Specifically, the pH of the mixed liquid system is 5, Na + The concentration is 80mM.
[0030] Furthermore, the oscillation was performed at 1000 r / min for 10 min.
[0031] The present invention provides a method for desorbing DNA from a chitosan-modified attapulgite adsorption material, and the specific steps are as follows:
[0032] The precipitate obtained after centrifugation in the DNA extraction method is washed with ethanol, dried, and the elution solution and the dried precipitate are mixed and centrifuged to obtain the supernatant.
[0033] Furthermore, the concentration of ethanol is 50-80%, and specifically can be 70%.
[0034] Furthermore, the eluent is one of water, Tris-EDTA buffer or sodium tripolyphosphate aqueous solution.
[0035] Preferably, the eluent is one of ultrapure water, Tris-EDTA buffer (10 mM Tris, 1 mM EDTA, pH 8.0) or a sodium tripolyphosphate aqueous solution with a concentration of 5 to 50 mM.
[0036] Specifically, the eluent is a 25 mM sodium tripolyphosphate aqueous solution.
[0037] Furthermore, the mass volume ratio of the dried precipitate and the eluent is 300 μg: (80-200) μL.
[0038] Specifically, the mass volume ratio of the dried precipitate and the eluent is 300 μg:100 μL.
[0039] A DNA extraction method comprises the following steps: firstly, DNA is adsorbed according to a DNA extraction method of a chitosan-modified attapulgite adsorption material, and then DNA is desorbed according to a DNA desorption method of a chitosan-modified attapulgite adsorption material.
[0040] Advantages and effects of the present invention:
[0041] (1) The present invention utilizes chitosan to modify attapulgite, optimizes its physical and chemical properties, and greatly improves its nucleic acid adsorption performance while ensuring low cost.
[0042] (2) The advantages of chitosan, such as biocompatibility, biodegradability and high adsorption capacity for nucleic acids, were utilized to solve the problem that chitosan tended to aggregate in water and was difficult to separate from other aqueous solutions.
[0043] (3) The saturated adsorption capacity of chitosan-modified attapulgite for DNA is 23.6479 μg / mg, which is 25.2% higher than that of unmodified attapulgite. By using a suitable desorbent, the desorption rate of chitosan-modified attapulgite for DNA can reach more than 90%. It is reported that the saturated adsorption capacity of DNA by silica-coated magnetic beads (Optimization of influencing factors of nucleic acid adsorption onto silica-coated magnetic particles: Application to viral nucleic acid extraction from serum) is 10.6 μg / mg, and the desorption rate is 93±3.1%; the reported saturated adsorption capacity of DNA by lithium-modified montmorillonite (XIE HY, WAN ZQ, LIU S, et al. Charge-dependent regulation in DNA adsorption on 2D clay minerals [J]. Sci Rep, 2019.) is 8 to 10 μg / mg, which indicates that the saturated adsorption capacity of DNA by the present invention is better than that of silica-coated magnetic beads and lithium-modified montmorillonite, and the desorption rate of DNA can reach more than 90% as that of silica-coated magnetic beads.
[0044] (4) Chitosan-modified attapulgite was used in the extraction of nucleic acid from Staphylococcus aureus, and a high amount of genomic DNA (22.23±0.78μg) was obtained. 260 / A 280 The ratio is between 1.7 and 1.9, indicating that the purity of genomic DNA extracted from chitosan-modified attapulgite is higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is the X-ray diffraction (XRD) characterization diagram of the attapulgite before and after modification prepared in Example 1 of the present invention.
[0046] Figure 2 This is a Fourier transform infrared spectrum (FTIR) analysis diagram of the attapulgite before and after modification prepared in Example 1 of the present invention.
[0047] Figure 3 This is a zeta potential analysis diagram of the attapulgite before and after modification prepared in Example 1 of the present invention.
[0048] Figure 4 (a) is a scanning electron microscope (SEM) image of the attapulgite used. Figure 4 (b) is a SEM image of the acid-modified attapulgite obtained in Example 1 of the present invention, Figure 4 (c) is the SEM image of the chitosan-modified attapulgite prepared in Example 1.
[0049] Figure 5 This is the effect of initial pH on DNA adsorption in the adsorption system of Example 2 of the present invention.
[0050] Figure 6 This is a graph showing the adsorption kinetics of DNA by chitosan-modified attapulgite prepared in Example 2 of the present invention.
[0051] Figure 7 is the Na in the adsorption system of Example 2 of the present invention + Effect of concentration on DNA adsorption.
[0052] Figure 8 This is a diagram showing the desorption conditions of DNA from chitosan-modified attapulgite obtained in Example 2 of the present invention. Figure 8 (a) The effect of different desorption agents on DNA desorption. Figure 8 (b) The effect of the concentration of the optimal desorption agent STPP on DNA desorption. Figure 8 (c) is the desorption equilibrium time of DNA by the desorbent on chitosan-modified attapulgite.
[0053] Fig. 9 This is the electrophoresis diagram of bacterial genomic DNA extraction in Example 4 of the present invention. DETAILED DESCRIPTION
[0054] Materials and Reagents:
[0055] Attapulgite was produced from Oubaite in Xuyi, Jiangsu Province; fish sperm DNA, sodium tripolyphosphate (Reagent Grade, Purity ≥ 98.0%), chitosan, column-based bacterial genomic DNA extraction kit (NO. B518255Ezup), and magnetic bead-based bacterial genomic DNA extraction kit (NO. B518725) were purchased from Shanghai Bioengineering Co., Ltd.; DNA loading buffer (instantview TM Red fluorescent DNA loading buffer (6× containing bromophenol blue) was purchased from Shanghai Biyuntian Co., Ltd.; anhydrous ethanol (analytical grade, Sinopharm Chemical Reagent Co., Ltd.); glacial acetic acid (analytical grade, Shanghai Aladdin Reagent Co., Ltd.); anhydrous sodium acetate (analytical grade, Beijing Inokai Technology Co., Ltd.); ultrapure water used in the experiment was purified using a Milli-Q A10 filtration system (18.2 MΩ·cm); Staphylococcus aureus ATCC 6538: preserved in the Food Safety and Quality Control Research Center of the School of Food Science and Technology, Jiangnan University.
[0056] Instruments and equipment:
[0057] X-ray diffractometer (D2 PHASER, Bruker AXS GmbH, Germany), Fourier transform infrared spectrometer (IS10, Nicolet, USA), field emission scanning electron microscope (Quanta 250FEG, FEI, USA), nanoparticle size and zeta potential analyzer (Zetasizer nano ZS, Malvern, UK).
[0058] Example 1
[0059] Example 1 is a specific preparation process of chitosan-modified attapulgite powder.
[0060] S1. Acid activation modification: 10 g of attapulgite powder (>325 mesh) was mixed with 100 mL of 10 wt% HCl, stirred and reacted at 70 ° C for 2 h, filtered, and the filter residue was washed with deionized water to pH = 6.0. The washed filter residue was placed in an oven at 105 ° C and dried for 12 h, and then ground through a 325 mesh standard sieve to obtain acid-activated attapulgite powder.
[0061] S2. Chitosan modification: 0.2 g chitosan and 2 g acid-activated attapulgite were added to 300 mL 1 wt% hydrochloric acid, stirred at 60°C for 24 h, and then 1.25 mol / L NaOH was added dropwise until neutral. The neutralized solution was placed in an oven at 105°C and dried for 12 h, then ground through a 325 mesh standard sieve to obtain chitosan-modified attapulgite powder.
[0062] The attapulgite, acid-activated attapulgite, and chitosan-modified attapulgite were characterized. X-ray diffraction analysis (XRD) of the attapulgite before and after modification was performed. Figure 1 As shown in Figure 1, the XRD pattern of the attapulgite sample was compared with that of attapulgite (PDF standard card number #31-0783), quartz (PDF standard card number #85-0798) and dolomite (PDF standard card number #36-0426). The results showed that the main mineral composition of the attapulgite sample contained attapulgite, quartz and dolomite. After acid modification, the peak of dolomite disappeared, indicating that hydrochloric acid reacted with dolomite, dissolving dolomite and purifying attapulgite. After further modification by chitosan, the structure of attapulgite did not change significantly.
[0063] The attapulgite before and after modification was analyzed by infrared absorption spectroscopy (FTIR). Figure 2 As shown, the attapulgite sample has a -1 and 3543.5cm -1 The two stretching vibration peaks of (Mg, Al)-OH, 3417 cm -1 The peak at 1645cm is the stretching vibration peak of zeolite water in attapulgite; -1 The bending vibration absorption peak of adsorbed water and crystal water is at 1033cm -1 The peak at 790 cm is the asymmetric stretching vibration peak of Si-O between the tetrahedral layers in the single chain; -1 and 516cm -1 is the bending vibration peak of Si-O. After HCl modification, the clay mineral still shows the characteristic absorption peak of the original attapulgite, and the dolomite CO3 2- At 1448cm -1 and 730cm -1 The characteristic peaks at 3622, 3543 and 3417 cm-1 disappeared. This indicates that the modified material has been purified without destroying the structure and the basic skeleton of the clay mineral is still preserved. After modification by chitosan, the peaks of the clay mineral at 3622, 3543 and 3417 cm-1 -1 It becomes weaker at 3600–3200 cm -1 The adsorption band in the 2920 cm-2 region becomes broad, indicating that the hydrogen bonding interaction between the silanol groups of attapulgite and the hydroxyl and amino groups of chitosan is greatly affected by the overlap of the OH and NH stretching bands of chitosan. -1 The new peaks represent aliphatic C–H stretching vibrations, which indicates that chitosan has been successfully immobilized on the acid-activated attapulgite.
[0064] The Zeta potential test of attapulgite before and after modification was carried out. Figure 3As shown in the figure, within the measured range, the surface of the attapulgite is negatively charged, and the attapulgite modified by HCl and chitosan changes its original charge. 2+ Mg 2+ Dissolution leads to an increase in the overall negative charge of attapulgite, which increases the negative charge of HCl-attapulgite. Compared with HCl-attapulgite, the negative charge of chitosan-attapulgite is significantly reduced, which may be due to the protonation of chitosan amino groups and the reduction of negative charge groups on the surface of HCl-attapulgite coated with chitosan, and its charge zero point is around pH 6.
[0065] Scanning electron microscope (SEM) analysis of attapulgite before and after modification was performed. Figure 4 As shown in Figure (a), nanorods with an average diameter of 50nm and a length of 200-300nm are entangled and aggregated. Figure (b) shows that after acid modification, dolomite is dissolved, the attapulgite is purified, its basic skeleton is still preserved, the gap is enlarged, and the attapulgite crystal bundles are disintegrated to looseness. Figure (c) shows that after the acid-modified attapulgite is modified by chitosan, the attapulgite becomes short and thick, and relatively smooth.
[0066] Example 2
[0067] This embodiment is the application of modified attapulgite to adsorb fish sperm DNA.
[0068] 30 mg of chitosan-modified attapulgite powder was added to 1 mL of ultrapure water to prepare an attapulgite suspension. Then, 10 μL of the attapulgite sample suspension (30 mg / mL) was mixed with 50 μL of the adsorption solution (containing 200 ng / μL fish sperm DNA), 10 μL of CH3COOH-CH3COONa buffer solution, and 30 μL of ultrapure water at pH 5 and Na + The concentration was 80 mM and the total volume was 100 μL. The mixture was shaken at 1000 rpm for 10 min in a constant temperature shaking incubator and centrifuged at 8000×g.
[0069] The DNA concentration in the supernatant was measured using a micro-nucleic acid quantifier. The amount of DNA adsorbed by the adsorption material was calculated based on the change in DNA content in the solution before and after adsorption equilibrium. The saturated adsorption capacity of chitosan-attapulgite for DNA was 23.6479 μg / mg, which means that the adsorption rate for 7 μg of DNA in the system can reach 99.0%.
[0070] Q e =V0(C0-C e ) / W s
[0071] Where: Q e(μg / mg) is the amount of DNA adsorbed when adsorption equilibrium is reached; C e (μg / mL) is the concentration of DNA in the supernatant when adsorption equilibrium is reached; C0 (μg / mL) is the initial concentration of the DNA solution; V0 (mL) is the volume of the DNA solution added; W s is the adsorbent dosage.
[0072] Comparative Example 1
[0073] This comparative example is to investigate the effect of the initial pH of the solution on adsorption. According to the process of Example 2, the amount of CH3COOH in the buffer solution was adjusted to adjust the pH of the system to 3, 4, 6, 7, and 8, and other operations remained unchanged.
[0074] Effect of initial pH on DNA adsorption in adsorption system Figure 5 As shown in the figure, the surface groups of chitosan-modified attapulgite are pH-sensitive groups, which determine the charge at different pH values. Under acidic conditions, the hydrogen ions in the solution make the attapulgite carry more positive charges, and more DNA is adsorbed through electrostatic action. Under alkaline conditions, the attapulgite is negatively charged as a whole, and there is electrostatic repulsion between the attapulgite and DNA in the solution, which hinders the adsorption of DNA and reduces the adsorption rate of DNA. Under experimental conditions, the amino or phosphate groups in the DNA molecules remove protons and carry negative charges. Therefore, it is difficult for DNA to adsorb on the surface of the clay that is also negatively charged. After modification with chitosan, the attapulgite is positively charged, and the negatively charged phosphate groups on the DNA molecules have strong electrostatic attraction with the positively charged amino groups of the modified attapulgite, resulting in a significant increase in the adsorption amount. However, considering the effect of DNA instability under low pH, the optimal pH in the adsorption system was selected as 5.0.
[0075] Comparative Example 2
[0076] This comparative example is to investigate the effect of oscillation time on adsorption. Referring to the process of Example 2, the oscillation time is adjusted to 20, 30, 40, 50, and 60 minutes, and other operations remain unchanged.
[0077] Fitting the adsorption kinetics model: The pseudo-first order model and pseudo-second order model were used to fit the DNA adsorption kinetics. 2 value to judge the quality of the fit.
[0078] The pseudo-first-order model equation is as follows: ln(q e -q t )=ln q e -K1t
[0079] The pseudo-second-order model equation is as follows: t / q t =1 / Kq e 2 +t / q e
[0080] In the formula, q e (μg / mg) is the equilibrium adsorption capacity; q t (mg / g) is the amount of DNA adsorbed by clay when the reaction time is t; t (min) is the adsorption time; K1, K (g·(mg·min) -1 ) is the rate constant.
[0081] like Figure 6 As shown, both attapulgite and chitosan-attapulgite were rapidly adsorbed within the first 10 minutes, with the adsorption percentage reaching more than 90%. After 10 minutes, the adsorption gradually slowed down, indicating that the adsorption gradually approached equilibrium. Therefore, 10 minutes was selected as the reaction time in subsequent experiments.
[0082] The adsorption kinetics of DNA on chitosan-modified attapulgite are shown in Figure 6 As shown in Figure 2, the adsorption data were fitted using pseudo-first-order adsorption kinetics and pseudo-second-order adsorption kinetics models. The R 2 , the pseudo-first-order model is the best fitting model, R 2 The experimental value of equilibrium adsorption capacity is in good agreement with the theoretical value of pseudo-first-order model, and the saturated adsorption capacity of attapulgite and chitosan-attapulgite is predicted to be 18.8972 and 23.6479 μg / mg respectively.
[0083] Comparative Example 3
[0084] This comparative example is to investigate the solution Na + The effect on adsorption was as follows: according to the process of Example 2, the amount of CH3COONa in the buffer solution was adjusted to adjust the Na + The concentrations were 0, 20, 40, 60, 100 and 120 mM, and other operations remained unchanged.
[0085] Effect of initial pH on DNA adsorption in adsorption system Figure 7 As shown, Na + As the concentration increases from 0mM to 80mM, the amount of DNA adsorbed on the surface of the material gradually increases. + As the concentration continued to increase, the amount of DNA adsorption did not change much, so the Na + The optimum concentration is 80 mM.
[0086] Example 3
[0087] Desorption of fish sperm DNA by modified attapulgite: The chitosan-modified attapulgite with DNA adsorbed in Example 2 was washed with 70% ethanol, centrifuged and air-dried, and DNA was eluted with 100 μL of elution solution. The nucleic acid concentration in the elution solution was measured with a micro-nucleic acid quantifier.
[0088] The results of the desorption conditions of chitosan-modified attapulgite for DNA are as follows Figure 8 As shown in the figure, after washing with 70% ethanol and drying, the elution effect of 100μL TE buffer (10mM Tris, 1mM EDTA, pH 8.0) and sodium tripolyphosphate (STPP) on DNA was compared, and the concentration of nucleic acids in the eluent was measured using a micro-UV spectrophotometer. The results showed that the desorption effect of STPP on nucleic acids on modified attapulgite was significantly better than that of TE buffer, and the optimal concentration of STPP desorption was 25mM, and the desorption rate could reach more than 90%. The desorption performance of 25mM STPP on DNA on chitosan-attapulgite was investigated, and the results showed that nucleic acids were rapidly desorbed within 1min, and the desorption rate was more than 90%.
[0089] Example 4
[0090] The embodiment is the application of chitosan-modified attapulgite adsorption material for nucleic acid extraction.
[0091] S1. Bacteria collection: Inoculate the bacterial solution into 3 mL of sterilized tryptic soy broth (TSB) and culture at 37°C and 160 rpm for 18 h. Take 1 mL of overnight cultured bacteria in a 1.5 mL centrifuge tube, centrifuge at 8,000 rpm for 1 min at room temperature, discard the supernatant, and collect the bacteria.
[0092] S2, bacterial lysis: Add 100μl Buffer Digestion, 80μL lysozyme solution (20mg / ml) and 2μL lysostaphin solution (2mg / mL) to resuspend the bacterial solution, and place in a 37℃ water bath for 30min. Add 20μl Proteinase K solution and oscillate to mix. To obtain RNA-free DNA, add 20μl RNase A (10mg / ml) after the water bath and place at room temperature for 2-5min. Place in a 56℃ water bath for 30min until the cells are completely lysed. Add 200μl Buffer BD, mix thoroughly by inversion, and place in a 70℃ water bath for 10min until the solution becomes clear, and obtain bacterial lysis solution.
[0093] S3. Adsorption of bacterial genomic DNA by modified attapulgite
[0094] 30 mg of attapulgite sample was added to 1 mL of ultrapure water to prepare an attapulgite sample suspension. Then, 30 μL of attapulgite sample suspension (30 mg / mL) and bacterial lysate (400 μL) were mixed with 70 μL of CH3COOH-CH3COONa buffer solution, with a system pH of 5 and Na + The concentration is 80mM and the total system is 500μL. The mixture is shaken at 1000r / min in a constant temperature shaking incubator and centrifuged at 8000×g for 10min. The DNA concentration in the supernatant is measured using a micro-nucleic acid quantifier. The amount of adsorbed DNA can be calculated by the difference between the amount of added DNA and the amount of supernatant DNA.
[0095] S4. Desorption of bacterial genomic DNA by modified attapulgite
[0096] The precipitate was washed with 70% ethanol, dried after centrifugation, and the DNA was eluted with 100 μL of elution solution. The nucleic acid concentration in the elution solution was measured using a micro-nucleic acid quantifier.
[0097] Example 5
[0098] The centrifugal column method and magnetic bead method for extracting genomic DNA were used as controls, and Staphylococcus aureus was used as the object of nucleic acid extraction. The yield of bacterial genomic DNA extracted by modified attapulgite and the quality of nucleic acid were evaluated.
[0099] Centrifugal column method: The centrifugal column method for adsorbing nucleic acids is to place the adsorption column in a collection tube, use a pipette to add all 400 μL of the cell lysate obtained in step (1) of Example 4 to the adsorption column, let it stand for 2 minutes, and then centrifuge at 12,000 rpm for 1 minute at room temperature, and discard the waste liquid in the collection tube. Then put the adsorption column back into the collection tube, add 500 μl PW Solution, centrifuge at 10,000 rpm for 30 seconds, and discard the filtrate. Then put the adsorption column back into the collection tube, add 500 μl Wash Solution, centrifuge at 10,000 rpm for 30 seconds, and discard the filtrate. Put the adsorption column back into the collection tube, centrifuge at 12,000 rpm for 2 minutes at room temperature, and remove the residual Wash Solution. Finally, take out the adsorption column, put it into a new 1.5 ml centrifuge tube, add 50-100 μl CEBuffer, let it stand for 3 minutes, centrifuge at 12,000 rpm for 2 minutes at room temperature, and collect the DNA solution. The extracted DNA can be used for the next experiment immediately or stored at -20°C.
[0100] Magnetic bead method: The method for adsorbing nucleic acids by the magnetic bead method is to add 500 μL Buffer MB and 10 μL magnetic beads to 400 μL of the cell lysate obtained in step (1) of Example 4, mix by aspiration or shaking, and let stand at room temperature for 1 min. Place the centrifuge tube on the magnetic rack for 30 seconds, wait for the magnetic beads to be completely absorbed to the tube wall, aspirate and discard the supernatant, and remove the centrifuge tube from the magnetic rack. Add 900 μL 70% ethanol to the centrifuge tube, aspirate or shake to mix, place the centrifuge tube on the magnetic rack for 30 seconds, wait for the magnetic beads to be completely absorbed to the tube wall, aspirate and discard the supernatant, and remove the centrifuge tube from the magnetic rack. Then repeat the above steps once, open the lid and dry at room temperature for 15-20 minutes or open the lid and dry in a 55°C constant temperature box for 5-7 minutes until there is no liquid residue in the tube. Add 50-100 μL TEBuffer to the centrifuge tube, bathe in a 65°C water bath for 5-10 minutes, and mix occasionally. Finally, take out the centrifuge tube and place it on the magnetic rack for 30 seconds. After the magnetic beads are completely absorbed onto the tube wall, carefully pipette the supernatant into a new centrifuge tube to obtain genomic DNA.
[0101] Take 1 μL of DNA extraction product, measure its concentration, A260 and A280 using an ultra-micro nucleic acid quantifier, and calculate the yield (concentration × elution volume) and purity (A260 / A280).
[0102] The extracted genomic DNA was detected by 0.8% agarose gel electrophoresis, with a sample volume of 5 μL and constant voltage electrophoresis of 3-5 V / cm for 2 hours. Observe and take pictures under ultraviolet light with a wavelength of 254 nm. The appearance of a single band of appropriate fragment size in the electrophoresis indicates that the DNA integrity is good.
[0103] Bacterial genomic DNA extraction electrophoresis diagram Fig. 9 As shown, 1 is the band obtained by column extraction method, 2 is the band obtained by magnetic bead extraction method, and 3 is the band obtained by modified attapulgite adsorption method. The extracted Staphylococcus aureus genomic DNA is greater than 15,000 bp in length and is a single band, indicating that the extracted genomic DNA has good integrity.
[0104] The yield and purity of Staphylococcus aureus genomic DNA extracted by different nucleic acid adsorption methods are shown in Table 1. Compared with the commercially available column extraction method and magnetic bead method, the chitosan-modified attapulgite extraction method had a higher DNA yield of 22.23 ± 0.78 μg;
[0105] A 260 / A 280 The ratio is between 1.7 and 1.9, indicating that the purity of genomic DNA extracted from chitosan-modified attapulgite is better.
[0106] Table 1 The amount and purity of genomic DNA extracted by different methods
[0107]
[0108] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for extracting nucleic acid, characterized in that: First, chitosan-modified attapulgite was taken to prepare a 30 mg / mL attapulgite suspension. The attapulgite suspension, the solution containing DNA, and the buffer solution were mixed, shaken for 10 min, centrifuged, and the precipitate after centrifugation was taken; the buffer solution was a CH3COOH-CH3COONa solution; after adding the buffer solution, the pH of the system was 5, and Na + The concentration is 80mM; The centrifuged precipitate is then washed with ethanol, dried, and the dried precipitate is mixed with an eluent and centrifuged to obtain a supernatant; the eluent is a 25 mM sodium tripolyphosphate aqueous solution; the mass volume ratio of the dried precipitate to the eluent is 300 μg: (80-200) μL; The chitosan-modified attapulgite is prepared by the following steps: S1. Acid activation modification: stirring the attapulgite powder with an aqueous solution of HCl, filtering, washing the solid, drying, and then grinding and sieving to obtain acid-activated attapulgite; the concentration of the aqueous solution of HCl is 5 to 15 wt%; the mass volume ratio of the attapulgite powder to the aqueous solution of HCl is 1 g: (5 to 15) mL; S2, chitosan modification: adding chitosan and acid-activated attapulgite to hydrochloric acid, stirring, adjusting the pH to neutral, drying the solution, grinding and drying the obtained solid, sieving, and obtaining chitosan-modified attapulgite; The mass ratio of acid-activated attapulgite to chitosan is 10:(0.5-1.5); the concentration of hydrochloric acid in step S2 is 0.5-1.5wt%.
Citation Information
Cited By
Preparation and application of chitosan modified attapulgite nucleic acid adsorption rod
CN119327428A
