A catalyst for preparing alcohol ether carboxylate and its preparation method and application
Through graphene-supported precious metal/metal organic framework catalyst, the problems of high catalyst cost and poor support stability in precious metal oxidation method are solved, and efficient and low-cost alcohol ether carboxylate synthesis is achieved, which extends the catalyst life and improves the catalytic activity. .
Patent Information
- Application Number
- CN202111632130.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-12-29
AI Technical Summary
In the existing synthesis methods of alcohol ether carboxylate, although the noble metal oxidation method is environmentally friendly, the catalyst cost is high and the noble metal is prone to fall off during use, resulting in a reduced catalytic activity, and the support activated carbon is fragile and has weak binding force, which affects the catalytic effect.
Graphene-loaded precious metal/metal organic framework catalyst is used to form a porous structure through the chemical bond between transition metal and organic imidazole ester, which improves the load area and stability, and uses metal organic frameworks such as ZIF-67 to provide a uniform and firm precious metal load. Avoid precious metal loss and carrier fragmentation.
It improves the service life and catalytic activity of the catalyst, reduces production costs, increases the catalytic active surface area, improves the reaction yield, and avoids the agglomeration of precious metals and supports stacking, enhancing the catalytic effect.
Abstract
Description
Technical Field
[0001] The present application relates to a catalyst for preparing alcohol ether carboxylate and a preparation method and application thereof, belonging to the technical field of catalysts. Background Art
[0002] With the progress of science and technology and economy, people pay more and more attention to sustainable development. As one of the three major green surfactants in the 20th century, alcohol ether carboxylates (AEC) have attracted people's attention due to their excellent biodegradability and have a good development trend. The structure of AEC is R(OCH2CH2)n-OCH2COOM, R represents open-chain alkanes or cycloalkanes, n is an integer, and M is a metal ion. Alcohol ether carboxylates are a type of anionic surfactants, which are resistant to high temperatures, have a wide pH range, are easy to degrade, have low toxicity, good washing performance, and can be perfectly compounded with cationic surfactants. They are widely used in biochemistry, plastics, leather, personal care, home care, industrial cleaning, oil field extraction and other fields.
[0003] At present, the synthesis methods of alcohol ether carboxylates mainly include carboxymethylation and oxidation. Among them, carboxymethylation is the main method currently used in industry, that is, the raw material polyoxyethylene ether (AEO) reacts with chloroacetic acid under alkaline conditions to produce alcohol ether carboxylates. Although the synthesis conditions of this method are mild, a large amount of three wastes will be generated and the product contains residual chlorine elements that cannot be removed. As environmental pressure increases, it will be gradually eliminated.
[0004] The precious metal oxidation method uses precious metals such as platinum / palladium as catalysts to oxidize AEO to AEC in an oxygen / air atmosphere. The advantages of the precious metal oxidation method are green and environmental protection, less waste treatment and less by-products. The prepared products are of high purity and free of harmful substances to the human body. They are widely used in cosmetics and care products and are the trend of future development. However, this method requires the use of precious metals Pt / Pd as catalysts, which are very expensive and the catalyst has the problem of falling off during use. Therefore, it is urgent to develop a catalyst with high efficiency, low cost and good stability.
[0005] In the prior art, CN110665500A discloses a composite catalyst for catalyzing alcohol ethers for synthesizing alcohol ether carboxylates, that is, reacting activated carbon with an aqueous solution of an activating agent under heating conditions to obtain pretreated activated carbon, reacting divalent palladium, divalent non-precious metals, hydrochloric acid and the obtained pretreated activated carbon, adjusting pH to alkalinity, adding a reducing agent, and separating after the reaction to obtain a composite catalyst. However, the carrier of the composite catalyst is activated carbon, which is fragile during the catalytic process, and non-precious metals and precious metals are loaded on the activated carbon by intermolecular forces, so the binding force is weak, and the distribution is uneven, which affects the catalytic effect. Summary of the invention
[0006] In order to solve the above problems, a catalyst for preparing alcohol ether carboxylates and a preparation method and application thereof are provided. The catalyst for preparing alcohol ether carboxylates can not only be used as a co-catalyst in a metal organic framework, but also can provide a larger loading area for precious metal particles, thereby avoiding the reduction of catalytic activity due to the loss of precious metals during the catalytic process and extending the service life of the catalyst; in addition, the transition metal in the metal organic framework is connected to the organic imidazole ester through a chemical bond, which is more stable and further improves the service life of the catalyst; in addition, the high specific surface area of graphene can increase the active sites to load a large amount of precious metals / metal organic frameworks, increase the catalytic active surface area, and improve the reaction yield.
[0007] According to one aspect of the present application, a catalyst for preparing alcohol ether carboxylates is provided, wherein the catalyst is graphene-supported noble metal / metal organic framework.
[0008] Wherein, the noble metal is at least one of Pt, Pd and Au, preferably Pt and Au; the metal organic framework is a methylimidazole organic material of a transition metal, and the transition metal salt is one or more of cobalt, zinc, copper and nickel. Preferably, the metal organic framework is at least one of ZIF-67, ZIF-8, ZIF-90 and ZIF-20. Using graphene as a carrier can provide more active sites for attachment to the metal organic framework, thereby increasing the catalytic activity; in addition, the metal organic framework has a stable structure, which can ensure uniform and firm loading of the noble metal; since the noble metal particles are small, the catalytic specific surface area can be greatly increased.
[0009] Preferably, the loading amount of the noble metal is 0.5%-10% of the mass of the metal organic framework, preferably 2%-8%, and the metal organic framework is 0.5-5 times, preferably 0.5-2 times, the mass of the graphene carrier.
[0010] Preferably, the metal organic framework is ZIF-67. Since ZIF-67 has a dodecahedral structure, it is very stable and can be applied multiple times without loss of precious metals during the application process, which greatly reduces costs and prolongs the service life of the catalyst. The cobalt on ZIF-67 acts as a co-catalyst, which has an isolation and anchoring effect on platinum particles, and can make the platinum particles more evenly loaded on the metal organic framework to avoid agglomeration, thereby exposing more catalytic active sites and improving the catalytic effect of the catalyst.
[0011] According to another aspect of the present application, a method for preparing a catalyst for preparing alcohol ether carboxylate is provided, comprising the following steps:
[0012] (1) adding a metal organic framework and a noble metal compound into hydrochloric acid, stirring and impregnating, to obtain a noble metal / metal organic framework;
[0013] Wherein, the noble metal compound is at least one of soluble compounds of platinum, palladium and gold; preferably at least one of chloroplatinic acid, chloropalladic acid and chloroauric acid.
[0014] (2) dispersing the noble metal / metal organic framework and graphene in a solvent, reacting them in a reactor at 100° C.-140° C. for 6 h-15 h, and obtaining the graphene-loaded noble metal / metal organic framework after separation.
[0015] Preferably, in step (1), the preparation method of the metal organic framework is as follows: 2-methylimidazole, a transition metal salt and a template are dissolved in water, stirred, and separated to obtain the metal organic framework.
[0016] Preferably, the mass ratio of the 2-methylimidazole, the transition metal salt and the template is 1-1.8:1-2:30-50. Preferably, the mass concentration of the transition metal salt in water is 1.0%-7.0%.
[0017] Preferably, the template is one or more of N,N'-dimethylformamide, pyridine, water and acetone; preferably, the template is N,N'-dimethylformamide.
[0018] Preferably, 2-methylimidazole is dissolved in water, the template is added, and the mixture is stirred to obtain a solution A; a transition metal salt is dissolved in water, stirred to obtain a solution A, and the solution A is stirred to obtain a solution B, and the solution B is filtered and dried to obtain the metal organic framework;
[0019] Preferably, the transition metal salt is one of cobalt salt, zinc salt, copper salt and nickel salt. Preferably, the transition metal salt is one of cobalt nitrate hexahydrate, zinc nitrate, copper nitrate, cobalt acetate and nickel nitrate; More preferably, the transition metal salt is cobalt nitrate hexahydrate;
[0020] Preferably, in step (1), the mass ratio of the metal organic framework to the noble metal compound is 10-200:1.
[0021] Preferably, in step (1), the noble metal compound is dissolved in the hydrochloric acid, the metal organic framework is added and stirred for 20-28 hours, and the noble metal / metal organic framework is obtained by suction filtration and drying;
[0022] Preferably, in step (2), the weight ratio of the noble metal / metal organic framework to graphene is 0.5-5:1, and the mass concentration of the graphene in the solvent is 2.0%-8.0%.
[0023] Preferably, in step (2), the noble metal / metal organic framework and graphene are dispersed in a solvent, reacted in a reactor at 110-130° C. for 10-15 h, and filtered and dried to obtain the graphene-loaded noble metal / metal organic framework.
[0024] Preferably, in step (2), the solvent is one or more of N,N'-dimethylformamide, pyridine, water and acetone, preferably N,N'-dimethylformamide.
[0025] According to another aspect of the present application, there is provided a use of the catalyst described in any one of the above items or the catalyst prepared by the preparation method described in any one of the above items in the preparation of alcohol ether carboxylates.
[0026] The present application also provides a method for preparing alcohol ether carboxylate, which uses polyoxyethylene ether and sodium hydroxide as raw materials, and reacts under the action of the catalyst of the present invention to obtain alcohol ether carboxylate.
[0027] Preferably, the mass concentration of the catalyst in the reaction system is 0.5wt%-1.5wt%.
[0028] The beneficial effects of this application include but are not limited to:
[0029] 1. According to the catalyst for preparing alcohol ether carboxylates of the present application, the transition metal in the metal organic framework can be used as a co-catalyst, which can not only play a synergistic catalytic role with the main catalyst noble metal, but also the metal organic framework is cross-linked with organic imidazole ester and transition metal to form a porous structure, which can provide a larger loading area for the noble metal particles, avoid the loss of noble metals during the catalytic process and reduce the catalytic activity, and extend the service life of the catalyst; in addition, the transition metal in the metal organic framework is connected to the organic imidazole ester through a chemical bond, which is more stable and further improves the service life of the catalyst; in addition, the layered structure of graphene provides a large loading area and a large number of loading sites for the noble metal / metal organic framework, so that the loading amount of the noble metal / metal organic framework can be guaranteed, and the noble metal / metal organic framework can also prevent the layered structure of graphene from stacking, so the granular noble metal, the lamellar graphene and the network-like metal organic framework form a "point-line-surface" combined structure, which greatly increases the catalytic reaction sites, increases the catalytic active surface area, and effectively improves the reaction yield.
[0030] 2. According to the preparation method of the catalyst for preparing alcohol ether carboxylates of the present application, the synthesis route is simple, the noble metal / metal organic framework can be synthesized at room temperature, and the production cost is low. DETAILED DESCRIPTION
[0031] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0032] Unless otherwise specified, the raw materials and catalysts in the examples of this application were purchased through commercial channels.
[0033] Example 1 Catalyst 1#
[0034] The preparation steps of catalyst 1# are as follows:
[0035] 1) Synthesis of ZIF-67: 10 g of 2-methylimidazole was dissolved in 200 mL of water, 400 g of N,N'-dimethylformamide was added, and the mixture was stirred to obtain a solution A; 12 g of cobalt nitrate hexahydrate was dissolved in 200 mL of water, stirred to obtain a solution A, and the mixture was added to the solution A and mixed to obtain a solution B; the solution B was filtered, washed, and dried to obtain ZIF-67;
[0036] 2) Synthesis of Pt / ZIF-67: 1 g of chloroplatinic acid was dissolved in 5 mL of hydrochloric acid and 100 mL of water, 10 g of ZIF-67 was added, and the mixture was stirred for 24 h, filtered, washed and dried to obtain Pt / ZIF-67;
[0037] 3) Synthesis of Pt / ZIF-67@G: 3.8 g of Pt / ZIF-67 and 2 g of graphene were dispersed in 50 g of DMF and reacted in a reactor at 120°C for 12 h. After filtration, washing and drying, graphene-loaded Pt / ZIF-67, i.e., Pt / ZIF-67@G, was obtained.
[0038] Example 2 Catalyst 2#
[0039] The preparation method of catalyst 2# is different from that of Example 1 in that the transition metal salt added to catalyst 2# in step 1) is 12 g of zinc nitrate to obtain ZIF-8, and the other conditions are the same as those of Example 1.
[0040] Example 3 Catalyst 3#
[0041] The preparation method of catalyst 3# is different from that of Example 1 in that, in step 1), 20 g of nickel nitrate hexahydrate is added to catalyst 3#, and the other conditions are the same as those of Example 1.
[0042] Example 4 Catalyst 4#
[0043] The preparation method of catalyst 4# is different from that of Example 1 in that 0.5 g of chloropalladic acid is added to catalyst 4# in step 2) instead of chloroplatinic acid, and the other conditions are the same as those of Example 1.
[0044] Example 5 Catalyst 5#
[0045] The preparation method of catalyst 5# is different from that of Example 1 in that 0.3 g of chloroplatinic acid is added to catalyst 5# in step 2), and the other conditions are the same as those of Example 1.
[0046] Example 6 Catalyst 6#
[0047] The preparation method of catalyst 6# is different from that of Example 1 in that 1 g of graphene is added to catalyst 6# in step 3), and the other conditions are the same as those of Example 1.
[0048] Example 7 Catalyst 7#
[0049] The preparation method of catalyst 7# is different from that of Example 1 in that 400 g of acetone is added to catalyst 7# in step 1) instead of N,N'-dimethylformamide, copper nitrate hexahydrate is used instead of cobalt nitrate hexahydrate, the amount of graphene added in step 3) is 3.8 g, and the other conditions are the same as in Example 1.
[0050] Example 8 Catalyst 8#
[0051] The preparation method of catalyst 8# is different from that of Example 1 in that 1 g of chloroauric acid is added to catalyst 4# in step 2) instead of chloroplatinic acid, and the other conditions are the same as those of Example 1.
[0052] Comparative Example 1 Catalyst D1#
[0053] The preparation method of catalyst D1# is different from that of Example 1 in that catalyst D1# does not have step 1), and 3.8 g of activated carbon is added in step 2) to replace ZIF-67, and the other conditions are the same as those of Example 1.
[0054] Comparative Example 2 Catalyst D2#
[0055] The preparation method of catalyst D2# is different from that of Example 1 in that catalyst D1# does not have step 1) and step 2), and in step 3), 0.19 g of chloroplatinic acid and 2 g of graphene are dispersed in 50 g of DMF, and the other conditions are the same as those of Example 1.
[0056] Comparative Example 3 Catalyst D3#
[0057] The preparation method of catalyst D3# is different from that of Example 1 in that catalyst D3# does not have step 2), and in step 3), 3.61 g ZIF-67 and 2 g graphene are dispersed in 50 g DMF, and the other conditions are the same as those of Example 1.
[0058] Comparative Example 4 Catalyst D4#
[0059] The preparation method of catalyst D4# is different from that of Example 1 in that catalyst D4# does not have step 3), and the remaining conditions are the same as those of Example 1.
[0060] Preparation of alcohol ether carboxylates: Add the raw material (AEO) and NaOH (molar ratio of about 1:1.05) to pure water to prepare an aqueous solution with a mass fraction of about 25%, place it in a reactor, add the catalysts 1#-8# and D1-D4# prepared in the above embodiments and comparative examples, and the mass amount of the catalyst relative to the entire reaction system is shown in Table 1. After nitrogen replacement 3 times, add oxygen to pressurize to 0.15Mpa, and the pressure is replenished to the reaction pressure in time during the pressure drop. The temperature is set to 80°C, and the stirring rate is 500r / min. After 5h of reaction, the reaction is stopped. The yield after 3h of reaction, the reaction yield after 5h of reaction, and the reaction yield after catalysis for 3h after 15 cycles are tested respectively, and the results are shown in Table 1.
[0061] Table 1
[0062] Serial number Dosage / wt% Yield after 3h reaction / % Yield after 5h reaction / % Reaction yield after 15 cycles Catalyst 1# 1 78 95 94 Catalyst 2# 1 37 62 58 Catalyst 3# 1 72 89 82 Catalyst 4# 1 75 91 85 Catalyst 5# 1 70 87 86 Catalyst 6# 1 67 83 80 Catalyst 7# 0.5 59 77 69 Catalyst 8# 1.5 74 91 88 Catalyst D1# 1 37 59 42 Catalyst D2# 1 39 60 51 Catalyst D3# 1 3 5 2 Catalyst D4# 1 42 63 49
[0063] As can be seen from Table 1, the catalyst prepared by the method of the present application is used to prepare alcohol ether carboxylates, has higher catalytic activity and high reaction yield, and after multiple cycles of use, the catalytic activity does not decrease significantly. The synthesis route is simple and the production cost is low.
[0064] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A catalyst for preparing alcohol ether carboxylates, It is characterized in that The catalyst is graphene-supported noble metal / metal organic framework, Wherein, the noble metal is at least one of Pt, Pd and Au, the metal organic framework is a methylimidazole organic material of a transition metal, and the transition metal salt is one or more of cobalt, zinc, copper and nickel; the loading amount of the noble metal is 0.5%-10% of the mass of the metal organic framework, and the metal organic framework is 0.5-5 times the mass of the graphene carrier; The method for preparing the catalyst comprises the following steps: (1) adding a metal organic framework and a noble metal compound into hydrochloric acid, stirring and impregnating, to obtain a noble metal / metal organic framework; (2) dispersing the noble metal / metal organic framework and graphene in a solvent, reacting them in a reactor at 100° C.-140° C. for 6 h-15 h, and obtaining the graphene-loaded noble metal / metal organic framework after separation.
2. The catalyst according to claim 1, It is characterized in that The noble metals are Pt and Au.
3. The catalyst according to claim 1, It is characterized in that The metal organic framework is at least one of ZIF-67, ZIF-8, ZIF-90 and ZIF-20.
4. The catalyst according to claim 1, It is characterized in that The loading amount of the noble metal is 2%-8% of the mass of the metal organic framework, and the mass of the metal organic framework is 0.5-2 times of the mass of the graphene carrier.
5. The catalyst according to claim 1, It is characterized in that In step (1), the preparation method of the metal organic framework is as follows: 2-methylimidazole, a transition metal salt, and a template agent are dissolved in water, stirred, and separated to obtain the metal organic framework.
6. The catalyst according to claim 5, It is characterized in that The mass ratio of the 2-methylimidazole, the transition metal salt and the template is 1-1.8:1-2:30-50.
7. The catalyst according to claim 5, It is characterized in that The mass concentration of the transition metal salt in water is 1.0%-7.0%.
8. The catalyst according to claim 5, It is characterized in that The template agent is one or more of N,N'-dimethylformamide, pyridine, water and acetone.
9. The catalyst according to claim 8, It is characterized in that The template agent is N,N'-dimethylformamide.
10. The catalyst according to claim 5, It is characterized in that The transition metal salt is one of cobalt salt, zinc salt, copper salt and nickel salt.
11. The catalyst according to claim 10, It is characterized in that The transition metal salt is one of cobalt nitrate hexahydrate, zinc nitrate, copper nitrate, cobalt acetate and nickel nitrate.
12. The catalyst according to claim 11, It is characterized in that The transition metal salt is cobalt nitrate hexahydrate.
13. The catalyst according to claim 1, It is characterized in that In step (1), the mass ratio of the metal organic framework to the noble metal compound is 10-200:
1.
14. The catalyst according to claim 1, It is characterized in that The noble metal compound is at least one of soluble compounds of platinum, palladium and gold.
15. The catalyst according to claim 1, It is characterized in that In step (1), the noble metal compound is dissolved in the hydrochloric acid, the metal organic framework is added and stirred for 20-28 hours, and the noble metal / metal organic framework is obtained by suction filtration and drying.
16. The catalyst according to claim 1, It is characterized in that In step (2), the weight ratio of the noble metal / metal organic framework to graphene is 0.5-5:1, and the mass concentration of the graphene in the solvent is 2.0%-8.0%.
17. The catalyst according to claim 1, It is characterized in that In step (2), the noble metal / metal organic framework and graphene are dispersed in a solvent, reacted in a reactor at 110-130° C. for 10-15 hours, and filtered and dried to obtain the graphene-loaded noble metal / metal organic framework.
18. The catalyst according to claim 1, It is characterized in that In step (2), the solvent is one or more of N,N'-dimethylformamide, pyridine, water and acetone.
19. The catalyst according to claim 18, It is characterized in that In step (2), the solvent is N,N'-dimethylformamide.
20. Use of a catalyst prepared by the preparation method according to any one of claims 1 to 19 in the preparation of alcohol ether carboxylates.
21. A method for preparing alcohol ether carboxylate, comprising taking polyoxyethylene ether and sodium hydroxide as raw materials, reacting in the presence of the catalyst according to any one of claims 1 to 19 to obtain alcohol ether carboxylate.
22. The preparation method according to claim 21, wherein the mass concentration of the catalyst in the reaction system is 0.5wt%-1.5wt%.