A substrate, preparation method and application
By growing aluminum nitride films on the surface of silicon nitride ceramic substrates and annealing, combining magnetron sputtering and N2 atmosphere annealing processes, the problem of insufficient thermal conductivity and mechanical properties of the substrate in the prior art is solved, and high strength is achieved. The preparation of AlN/Si3N4 ceramic substrate with high thermal conductivity improves the comprehensive performance of the material and simplifies the process.
Patent Information
- Application Number
- CN202111683104.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-31
AI Technical Summary
It is difficult to prepare a packaging substrate with high strength and high thermal conductivity in the prior art, and the excellent properties of silicon nitride and aluminum nitride ceramics are not fully utilized.
After surface treatment, aluminum nitride film was grown after surface treatment, and annealing was performed in a nitrogen atmosphere to prepare an AlN/Si3N4 ceramic substrate, which was combined with magnetron sputtering and N2 atmosphere annealing to improve the thermal conductivity of the material and Mechanical properties.
It significantly improves the thermal conductivity and mechanical properties of the substrate, reduces process complexity and cost, and improves the purity of the aluminum nitride film layer, and enhances the heat dissipation energy efficiency and mechanical properties of the device.
Smart Images

Figure CN116410018B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of packaging substrates, and in particular to an AlN / Si3N4 ceramic substrate with high thermal conductivity and high strength and a preparation method thereof. Background Art
[0002] With the development of large-scale integrated circuits, people have higher and higher requirements for packaging substrates. Among them, high thermal conductivity, high strength and low dielectric constant are the most basic requirements for integrated circuit packaging substrates.
[0003] The packaging substrate should also have good thermal matching with the silicon wafer, easy molding, high surface flatness, easy metallization, easy processing, low cost and certain mechanical properties.
[0004] Silicon nitride ceramics have excellent mechanical properties, with a bending strength of 600-800 MPa and a fracture toughness of 7-9 MPa·m1 / 2. Aluminum nitride (A1N), as a new type of advanced ceramic material with excellent comprehensive performance, has a series of excellent properties such as excellent thermal conductivity, reliable electrical insulation, low dielectric constant and dielectric loss, non-toxicity, and a thermal expansion coefficient that matches silicon. It is considered to be an ideal material for a new generation of high-density semiconductor substrates and electronic device packaging, and has received widespread attention from researchers at home and abroad. In theory, the thermal conductivity of A1N is 320W / (m·K), and the thermal conductivity of polycrystalline aluminum nitride actually prepared in industry can also reach 100-250W / (m), which is 5-10 times the thermal conductivity of traditional substrate material aluminum oxide.
[0005] How to make full use of the respective excellent properties of silicon nitride and aluminum nitride ceramics to prepare a packaging substrate with high strength and high thermal conductivity is a technical issue worthy of study. Summary of the invention
[0006] In view of the above technical problems, the present invention proposes a composite substrate of silicon nitride and aluminum nitride ceramics, and utilizes the advantages of each to prepare a packaging substrate with high strength and high thermal conductivity.
[0007] Specifically, the technical solution proposed by the present invention is as follows:
[0008] A method for preparing an AlN / Si3N4 ceramic substrate comprises the following steps:
[0009] Choose silicon nitride ceramic substrate;
[0010] Performing surface treatment on the silicon nitride ceramic substrate;
[0011] Growing an aluminum nitride film on the surface of the silicon nitride ceramic substrate to obtain a composite ceramic substrate;
[0012] The composite ceramic substrate is annealed to obtain an AlN / Si3N4 ceramic substrate.
[0013] Optionally, the surface treatment includes grinding, polishing and cleaning the surface of the silicon nitride ceramic substrate.
[0014] Optionally, the aluminum nitride film is grown by magnetron sputtering.
[0015] Optionally, the magnetron sputtering growth includes:
[0016] Placing the silicon nitride ceramic substrate in a magnetron sputtering chamber;
[0017] Select Al as the sputtering target;
[0018] Nitrogen gas was introduced to grow the thin film.
[0019] Optionally, the process parameters of the magnetron sputtering growth include a film growth temperature of about 420° C., a sputtering pressure of about 6.2 mTorr, a nitrogen flow ratio of about 85%, and a sputtering power of about 520W.
[0020] Optionally, the annealing includes being performed in a nitrogen atmosphere at a pressure of about 3 MPa and a temperature of about 960° C.
[0021] Optionally, the annealing includes the following heating rate and heat preservation process:
[0022] The heating rate is: 0-500℃ heating rate is 10℃ / min; 500℃ insulation for 0.5h; 500℃-650℃ heating rate is 5℃ / min; 650℃ insulation for 0.5h; 650℃-960℃ heating rate is 2℃ / min; 960℃ insulation for 2h.
[0023] The present invention also provides an AlN / Si3N4 ceramic substrate, comprising a silicon nitride ceramic substrate and an aluminum nitride layer grown on the surface of the silicon nitride ceramic substrate.
[0024] Optionally, the aluminum nitride film layer has a thickness of 0.1-2 microns.
[0025] The present invention also provides a third generation semiconductor power device, comprising the AlN / Si3N4 ceramic substrate provided by the present invention.
[0026] The present invention also provides a light-emitting device, comprising the AlN / Si3N4 ceramic substrate provided by the present invention.
[0027] The present invention has the following advantages:
[0028] (1) Greatly improve the thermal conductivity of Si3N4 ceramic substrates or structural parts, improve the overall heat dissipation efficiency of the material, and prevent the occurrence of thermal mismatch;
[0029] (2) The substrate Si3N4 ceramic has excellent mechanical properties, combined with the high thermal conductivity AlN film, so that the two materials complement each other and achieve composite performance optimization, making its comprehensive performance better than any one of them;
[0030] (3) The coating process using metal Al target instead of AlN target can reduce the complexity of the process and control the cost;
[0031] (4) The combination of magnetron sputtering and N2 atmosphere annealing process can significantly improve the purity of the AlN film layer and reduce the oxygen content of the aluminum nitride coating from 2.8at.% to 0.8at.%, thereby further improving the thermal conductivity of the device and reducing the thermal resistance of the contact interface. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a process flow chart of preparing an AlN / Si3N4 ceramic substrate according to one embodiment of the present invention.
[0033] Figure 2 It is a schematic structural diagram of an AlN / Si3N4 ceramic substrate according to one embodiment of the present invention applied to a third generation semiconductor device.
[0034] Figure 3 It is a structural schematic diagram of an AlN / Si3N4 ceramic substrate applied to a light-emitting device according to one embodiment of the present invention. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.
[0036] Unless otherwise specified, the technical terms or scientific terms used in the present invention shall have the usual meanings understood by persons with ordinary skills in the field to which the present invention belongs. The terms "including" or "comprising" used in the present invention neither limit the shapes, numbers, steps, operations, components, originals and / or their groups mentioned, nor exclude the presence or addition of one or more other different shapes, numbers, steps, actions, operations, components, originals and / or their groups. In addition, the terms "first" and "second" are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number and order of the indicated technical features.
[0037] Example 1
[0038] The present invention provides a method for preparing an AlN / Si3N4 ceramic substrate, such as Figure 1 As shown, the following steps are included:
[0039] S1: Select silicon nitride ceramic substrate;
[0040] S2: performing surface treatment on the silicon nitride ceramic substrate;
[0041] The surface treatment includes grinding, polishing and cleaning the surface of the silicon nitride ceramic substrate. Specifically, the surface of the silicon nitride substrate is ground and polished, and then ultrasonically cleaned in acetone, alcohol and deionized water for 5 minutes each.
[0042] S3: growing an aluminum nitride film on the surface of the silicon nitride ceramic substrate to obtain a composite ceramic substrate; optionally, the growth of this embodiment uses magnetron sputtering growth. Specifically, the silicon nitride substrate is placed in a magnetron sputtering chamber, the sputtering target is an Al target, and reactive sputtering growth of the AlN film is performed; the film growth temperature is 420°C, the sputtering pressure is 6.2mTorr, the nitrogen flow ratio is 85%, and the sputtering power is 520W. The thickness of the final AlN film layer can be adjusted in the range of 0.1 to -2 microns, and the surface roughness is controlled at 0.15 microns.
[0043] S4: annealing the composite ceramic substrate to obtain an AlN / Si3N4 ceramic substrate.
[0044] Specifically, the composite ceramic substrate obtained in step S3 is placed in a boron nitride mold and annealed at 960° C. in nitrogen to obtain a product.
[0045] The annealing was performed in nitrogen at a pressure of 3 MPa and a temperature of 960°C.
[0046] The annealing process includes the following heating rates and holding times: 0-500°C heating rate is 10°C / min; 500°C is kept for 0.5h; 500°C-650°C heating rate is 5°C / min; 650°C is kept for 0.5h; 650°C-960°C heating rate is 2°C / min; 960°C is kept for 2h.
[0047] When the surface roughness is 0.15 microns, the surface contact resistance of the product and the copper foil with the same roughness is 7.2×10 -4 m 2 K / W, better than the standard value of pure silicon nitride (1.5×10 -2 m 2 K / W).
[0048] Example 2
[0049] The present invention also provides an AlN / Si3N4 ceramic substrate obtained by the preparation method of Example 1, the ceramic substrate comprising a silicon nitride ceramic substrate and an aluminum nitride layer grown on the surface of the silicon nitride ceramic substrate. The magnetron sputtered aluminum nitride film layer can cover the surface of the workpiece, the thickness can be adjusted between 0.1 and 2 microns, and the surface roughness is controlled at 0.15 microns.
[0050] Example 3
[0051] like Figure 2 As shown, as an embodiment of the present invention, a third-generation semiconductor power device is disclosed, which generally includes: a ceramic substrate, a power device, a heat sink, a thermal interface material on the heat sink, wire bonding, etc.; the ceramic substrate is used as a ceramic carrier for thermal and electrical separation of the third-generation semiconductor power device. The ceramic substrate adopts the ceramic substrate proposed in Embodiment 2 of the present invention. The power device is, for example, an IGBT device.
[0052] Example 4
[0053] like Figure 3 As shown, as an embodiment of the present invention, a light-emitting device is disclosed, which generally comprises: a ceramic substrate, a conductive metal layer (circuit layer), a light-emitting chip, a dam (or wall), and an external packaging material.
[0054] Among them, the conductive metal layer (circuit layer) is located on the surface of the ceramic substrate. Copper, titanium and other metal films are deposited as seed layers by magnetron sputtering, and then copper thick film deposition is performed by electroplating in a graphic manner such as photoresist or dry film, and the copper metal surface is subjected to final finishing such as chemical nickel plating and chemical gold plating. The material of the metal layer is generally copper, nickel, gold and other materials. The thickness of the copper layer is 0.05-1mm, the thickness of the nickel layer is 2-10μm, and the thickness of the gold layer is 50-250nm. In addition, the surface of the ceramic substrate can be directly coated with copper DBC process to prepare a copper pattern, and the thickness of the copper pattern is 0.05-3mm. The light-emitting chip is connected to the conductive metal layer (circuit layer); the excitation chip array can be bonded to the ceramic substrate with a solid crystal adhesive; the external packaging material is used to encapsulate the excitation chip array and the phosphor, and its material is generally silica gel.
[0055] As a preferred high color rendering white light application solution of the present invention, the phosphor in the light emitting device adopts yttrium aluminum garnet phosphor and (Sr, Ca)AlSiN3:Eu red phosphor;
[0056] As another preferred high color rendering white light application solution of the present invention, the phosphor in the light emitting device adopts yttrium aluminum garnet phosphor, (Sr, Ca) AlSiN3:Eu red phosphor and KSF red phosphor;
[0057] As another preferred high color rendering lighting application solution of the present invention, the phosphor in the light emitting device adopts (Sr, Ca) AlSiN3:Eu nitride red powder and (Sr, Ba) 2SiO4:Eu silicate phosphor;
[0058] As a preferred high color gamut backlight application solution of the present invention, the phosphors in the light-emitting device are β-sialon phosphors and KSF red phosphors.
[0059] The light-emitting chips in the light-emitting chip array may be one or more of ultraviolet, purple, blue, green, red or infrared light-emitting chips.
[0060] For example: the light-emitting chips in the light-emitting chip array use a combination of blue light chips, green light chips and red chips to form RGB full color; the light-emitting chips in the light-emitting chip array use ultraviolet chips for sterilization; the light-emitting chips in the light-emitting chip array use a combination of blue light chips and red light chips for plant lighting; the light-emitting chips in the light-emitting chip array are infrared chips for equipment image recognition.
[0061] When the light-emitting chip in the light-emitting chip array is one or more of ultraviolet, purple, and blue chips, it can also play the role of an excitation chip. In this case, the light-emitting device also includes a phosphor, which emits light when excited by the excitation chip. The phosphor can be one or more of yttrium aluminum garnet phosphor, (Sr, Ca) AlSiN3: Eu red phosphor, KSF red phosphor, β-sialon phosphor, (Sr, Ba) 2SiO4: Eu silicate phosphor.
[0062] The light-emitting chip array may also be a combination of an excitation chip and a light-emitting chip.
[0063] The present invention has the following advantages over the prior art:
[0064] (1) Greatly improve the thermal conductivity of Si3N4 ceramic substrates or structural parts, improve the overall heat dissipation efficiency of the material, and prevent the occurrence of thermal mismatch;
[0065] (2) The substrate Si3N4 ceramic has excellent mechanical properties, combined with the high thermal conductivity AlN film, so that the two materials complement each other and achieve composite performance optimization, making its comprehensive performance better than any one of them;
[0066] (3) The coating process using metal Al target instead of AlN target can reduce the complexity of the process and control the cost;
[0067] (4) The combination of magnetron sputtering and N2 atmosphere annealing process can significantly improve the purity of the AlN film layer.
[0068] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. AlN / Si 3 N 4 Method for preparing ceramic packaging substrate, It is characterized in that The following steps are involved: Choose silicon nitride ceramic substrate; Performing surface treatment on the silicon nitride ceramic substrate; Growing an aluminum nitride film on the surface of the silicon nitride ceramic substrate to obtain a composite ceramic substrate; The composite ceramic substrate is annealed to obtain AlN / Si 3 N 4 Ceramic substrate; The annealing process includes the following heating rate and heat preservation process: Heating rate: 0-500℃ heating rate is 10℃ / min; 500℃ insulation for 0.5h; 500℃-650℃ heating rate is 5℃ / min; 650℃ insulation for 0.5h; 650℃-960℃ heating rate is 2℃ / min; 960℃ insulation for 2h; The thickness of the aluminum nitride film layer can be adjusted in the range of 0.1 to -2 microns; The surface roughness of the aluminum nitride film layer is controlled at 0.15 microns; wherein, The aluminum nitride film is grown by magnetron sputtering, comprising: Placing the silicon nitride ceramic substrate in a magnetron sputtering chamber; Select Al as the sputtering target; Nitrogen gas was introduced to grow the thin film.
2. The AlN / Si according to claim 1 3 N 4 Method for preparing ceramic packaging substrate, It is characterized in that The surface treatment includes grinding, polishing and cleaning the surface of the silicon nitride ceramic substrate.
3. The AlN / Si according to claim 1 3 N 4 Method for preparing ceramic packaging substrate, It is characterized in that The process parameters of the magnetron sputtering growth include a film growth temperature of 420° C., a sputtering pressure of 6.2 mTorr, a nitrogen flow rate of 85%, and a sputtering power of 520W.
4. The AlN / Si according to claim 1 3 N 4 Method for preparing ceramic packaging substrate, It is characterized in that The annealing is performed in a nitrogen atmosphere at a pressure of 3 MPa and a temperature of 960° C.
5. An AlN / Si prepared by the method according to claim 1 3 N 4 Ceramic package substrate, It is characterized in that It comprises a silicon nitride ceramic substrate and an aluminum nitride layer grown on the surface of the silicon nitride ceramic substrate; the oxygen content of the aluminum nitride film layer is 0.8 at.%.
6. A third generation semiconductor power device, It is characterized in that Comprising the AlN / Si according to claim 5 3 N 4 Ceramic package substrate.
7. A light emitting device, It is characterized in that The light emitting device comprises the AlN / Si 3 N 4 Ceramic package substrate.