Preparation method of thermal spray coating sealing agent
Through the combination of alloy powder and dispersant, combined with negative pressure and pressurization technology, the sealing agent is allowed to penetrate deep into the pores of the coating and remelted, solving the pore problem of thermal spray coating, improving the sealing effect and process efficiency, and realizing the coating long-term sealing and automated production.
Patent Information
- Application Number
- CN202310080404.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-02
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-12-02
AI Technical Summary
The presence of pores on the thermal spray coating leads to poor corrosion performance. The traditional sealing method has shallow and uneven penetration depth of the sealing agent, and the process efficiency is low, making it difficult to automate.
The sealing agent is prepared by alloy powder, combining dispersant and carrier solvent, and the sealing agent penetrates the coating pores through negative pressure and pressurization technology, and a better sealing effect is achieved through remelting.
It significantly improves the penetration depth and sealing effect of the sealing agent, extends the service life of the coating, and realizes process automation and improves production efficiency.
Smart Images

Figure BDA0004067325410000081 
Figure HDA0004067325420000011 
Figure HDA0004067325420000012
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application date of December 2, 2020, application number 2020113912631, and invention name "Thermal spray coating sealing agent, preparation method and sealing method thereof". Technical Field
[0002] The invention belongs to the technical field of pore sealing, and in particular relates to a method for preparing a pore sealing agent for a thermal spray coating. Background Art
[0003] Thermal spraying technology is a method of using a heat source to heat the spray material to a molten or semi-molten state, and spraying and depositing it onto a pre-treated substrate surface at a certain speed to form a coating, giving the substrate surface special properties.
[0004] Thermal spray coatings are composed of superimposed particles, and there must be pores between the superimposed particles. These pore defects allow the corrosive medium to quickly diffuse through the channel, significantly reducing the corrosion performance of the coating. In particular, the presence of penetrating pores makes it possible for the corrosive medium to reach the surface of the protected substrate through the pores, causing chemical or electrochemical corrosion between the coating and the substrate, and the accumulation of corrosion products at the interface, causing the thermal spray coating to crack and peel off, and ultimately leading to coating failure.
[0005] The main way to solve the problem of pores in thermal spray coatings is to use sealing technology, that is, to apply and infiltrate a sealing agent (generally an organic material oil) into the thermal spray coating to fill the pores of the thermal spray coating, thereby achieving sealing of the thermal spray coating.
[0006] However, there are two urgent problems to be solved in the current coating sealing field:
[0007] 1. Limited by the structural stability of organic matter, the service temperature of the sealant with pure organic components is limited (generally <300℃).
[0008] Second, the traditional sealing method is the normal pressure brushing method, that is, in a normal pressure environment, the organic sealer is evenly brushed onto the coating surface by hand, and the sealer penetrates into the coating pores by its own fluidity. The normal pressure brushing sealing process has the following disadvantages:
[0009] (1) Technical defects of normal pressure brush sealing process:
[0010] The normal pressure brush-coating sealing process has two major disadvantages: shallow penetration depth of the sealer and uneven penetration depth of the sealer, which restricts the service life of the coating. During the service life of the coating, the coating surface will continue to be worn by the medium. Once the wear exceeds the penetration depth of the sealer, the pores between the particles inside the coating will be exposed to the medium environment, and the corrosive medium can reach the protected substrate through the pores. The coating will easily peel off and lose its anti-corrosion or sealing effect.
[0011] 1. The penetration depth of the sealer is shallow: Under the normal pressure brush coating process, the sealer relies on its own fluidity to penetrate into the tiny pores on the surface of the coating. Because there is air remaining in the pores and the sealer's own fluidity is limited, the sealer can only penetrate into the shallow surface of the coating. The general penetration depth is about 20μm.
[0012] General industrial experience shows that the surface coating of the rotating parts of rotating mechanical equipment operating in a conventional medium environment may fall off after a service life of 1-3 years. If the sealing process is not properly controlled, the coating will fall off and become ineffective after a service life of 1 year.
[0013] 2. Uneven penetration depth of sealer: The normal pressure brushing process is a manual operation. The operator's experience and proficiency, as well as the surface geometry of the coating, affect the uniformity of the sealer brushing. If the coating thickness is uneven, the penetration depth of the sealer may be shallower in the thin coating area than in other areas. Industrial experience shows that the shallowest penetration depth under the brushing process is 50% less than the deepest depth. Shallow penetration areas become weak points in the service life of the coating, affecting the coating life.
[0014] (2) The production efficiency of the normal pressure brush sealing process is low, which is reflected in two aspects:
[0015] 1. The curing time of the sealant is long: The curing time of the sealant refers to the time required from the sealant being brushed onto the coating surface to the sealant solidifying in the pores of the coating.
[0016] The normal pressure brush sealing process relies on the sealant's own fluidity to penetrate into the coating pores, but the sealant's fluidity is generally poor, and the dynamic process of the sealant flowing into and filling the pores takes a long time. Industrial experience shows that the curing time takes at least 24 hours.
[0017] 2. Difficult to automate: As mentioned above, the brush-type sealing process is a manual operation and must rely on experienced personnel to manually construct each piece. At present, there is no automated process in the industry, which restricts large-scale and batch high-efficiency thermal spraying construction activities. Summary of the invention
[0018] In view of this, in order to overcome the defects of the prior art and achieve the above-mentioned purpose, the purpose of the present invention is to provide a method for preparing a thermal spray coating sealant, wherein the prepared sealant can be remelted in situ, has a deep penetration depth and a good sealing effect.
[0019] In order to achieve the above object, the present invention adopts the following technical solutions:
[0020] A thermal spray coating sealer, comprising alloy powder, a dispersant and a carrier, wherein the alloy powder accounts for 5-10% by weight of the sealer, and the viscosity of the sealer is 0.05-0.1 Pa·S at 25° C. The viscosity of the sodium silicate solvent is preferably 0.01-0.05 Pa·S at 25° C.
[0021] The sealing agent prepared from alloy powder can achieve the sealing function after remelting the alloy powder, and has a good continuous effect and is not easy to fail. The dispersant is used to disperse the alloy powder to avoid the agglomeration of the alloy powder, and the carrier solvent is used to disperse and support the alloy powder to achieve the purpose of uniform dispersion of the alloy powder. And by controlling the proportion of alloy powder and the viscosity of the sealing agent, the sealing agent can flow into the pores of the coating and have a greater penetration depth, achieving a better sealing effect.
[0022] According to some preferred embodiments of the present invention, the alloy powder contains 11-19% Cr, 3.5-5.5% Si, 1.5-3.5% B, and the balance is Ni by mass percentage. By reasonably setting the proportion of each element in the alloy powder, the sealing effect and the sustained effect after the sealing agent is remelted are better.
[0023] According to some preferred embodiments of the present invention, the particle size of the alloy powder is in the range of 0.5-5 μm. If the particle size is too small, the remelting and sealing effects are poor, and if the particle size is too large, it cannot enter the pores of the coating, which will affect the remelting and sealing effects.
[0024] According to some preferred implementation aspects of the present invention, the dispersant is acetone, and the carrier is a sodium silicate solvent. Compared with other reagents, the use of acetone and sodium silicate can achieve better alloy powder dispersion and support effects.
[0025] According to some preferred implementation aspects of the present invention, the mass proportion of the dispersant in the sealing agent is 30-40%. Reasonable control of the content of the dispersant can control the dispersion effect of the alloy powder on the one hand, and the viscosity of the product on the other hand.
[0026] The present invention also provides a method for preparing the above-mentioned sealing agent, comprising the following steps: preparing an alloy block, preparing the alloy block to obtain alloy powder, dispersing the alloy powder in a dispersant to obtain an alloy solution, and mixing the alloy solution with a carrier solvent to obtain a sealing agent. The alloy solution is first prepared and then mixed with the carrier solvent to form the sealing agent, thereby avoiding the alloy powder agglomeration and inability to disperse.
[0027] According to some preferred implementation aspects of the present invention, the following steps are specifically included: preparing an alloy block by a physical metallurgical method, using an aerosol method (high-speed airflow) to impact the alloy block to obtain alloy powder, dispersing the alloy powder in acetone by ultrasonic waves to obtain an alloy solution, and adding the alloy solution to a carrier solvent to obtain the sealing agent. Among them, the physical metallurgical method for preparing the alloy block and the aerosol method are both conventional methods in the relevant field. Using ultrasonic waves can further disperse the alloy powder to prevent it from agglomerating.
[0028] The present invention also provides a method for sealing holes using the above-mentioned sealing agent, and the sealing method includes the following steps: placing the coating component to be sealed in a closed container, adding the sealing agent into the closed container and filling the entire closed container with the sealing agent, controlling the closed container to be in a negative pressure state so that the sealing agent flows into the pores inside the coating; discharging the sealing agent in the closed container, cleaning the coating component, taking out the coating component and drying it; then remelting the sealing agent in the coating component so that the alloy powder in the sealing agent solidifies after remelting and fills the pores of the coating component. The above-mentioned process method is used in combination with the aforementioned sealing agent, so that the sealing agent can penetrate deeper into the pores of the coating and be remelted in situ in the pores, so as to achieve a sufficient sealing effect with good sustained effect.
[0029] According to some preferred implementation aspects of the present invention, the sealing method further includes a pressurizing step before discharging the sealing agent in the sealed container, specifically including the following steps: after the pressure in the sealed container is restored to normal pressure, the sealed container is pressurized and maintained for a certain period of time. That is, there is a positive pressure process after the negative pressure, which further allows the sealing agent to better enter the pores of the coating.
[0030] According to some preferred embodiments of the present invention, the cleaning is to add water into the closed container and perform circulating cleaning, and the temperature of the water is not lower than 85°C, so as to better clean the sealer remaining on the surface of the coating part. At the same time, the organic components in the sealer solidify and solidify in a temperature environment above 85°C to fill the pores in the coating.
[0031] In some specific embodiments of the present invention, the sealing method comprises the following steps:
[0032] A. Place the coated parts to be sealed in a sealed container.
[0033] B. Add the aforementioned liquid sealing agent into a sealed container.
[0034] C. Extract the air from the top of the sealed container, and finally fill the entire sealed container with the sealant, and maintain the container in a negative pressure state, the negative pressure is maintained at 0-10pa (absolute pressure), and the maintenance time is 20-30min. The negative pressure state can extract the air in the pores, which helps the sealant flow into the pores inside the coating and achieve a deeper penetration depth.
[0035] D. Connect the container with the atmosphere and restore the pressure inside the sealed container to normal pressure.
[0036] E. Pressurize the sealed container from the top to the inside, maintaining the pressure at no less than 6-50 bar (absolute pressure) for 20-30 minutes. Pressurization further forces the sealant to enter the pores inside the coating and achieve a deeper penetration depth.
[0037] F. Discharge the sealing agent from the sealed container.
[0038] G. Connect the sealed container to the hot water tank, circulate the hot water for 10-15 minutes, and clean the residual sealant attached to the surface of the coating parts. The hot water temperature should not be lower than 85°C. Under the heating of high-temperature water, the sealant remaining in the pores of the coating solidifies and fills the pores.
[0039] H. Remove the coated parts and let dry.
[0040] I. The sealing agent in the pores of the coating is heated and melted by laser heating or other methods, so that the metal powder in the sealing agent is melted in situ, deformed and solidified after melting, and the pores are sealed to achieve the sealing effect. The sealing effect and sustained effect after the metal solidifies are better than the sealing effect of conventional pure organic matter.
[0041] Compared with the prior art, the present invention is beneficial in that: the preparation method of the thermal spray coating self-sealing sealant of the present application uses alloy powder to prepare the sealant, and the alloy powder can be remelted to achieve the function of sealing, and the continuous effect is good and not easy to fail. The dispersant is used to disperse the alloy powder to avoid the agglomeration of the alloy powder, and the carrier solvent is used to disperse and support the alloy powder to achieve the purpose of uniform dispersion of the alloy powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0043] Figure 1 This is a schematic diagram of step A of the sealing method in a preferred embodiment of the present invention;
[0044] Figure 2 This is a schematic diagram of step B of the sealing method in a preferred embodiment of the present invention;
[0045] Figure 3 Schematic diagram of step C of the sealing method in a preferred embodiment of the present invention;
[0046] Figure 4 Schematic diagram of step D of the sealing method in a preferred embodiment of the present invention;
[0047] Figure 5 Schematic diagram of step E of the sealing method in a preferred embodiment of the present invention;
[0048] Figure 6 This is a schematic diagram of step F of the sealing method in a preferred embodiment of the present invention;
[0049] Figure 7 Schematic diagram of step G of the sealing method in a preferred embodiment of the present invention;
[0050] Figure 8 Schematic diagram of step H of the sealing method in a preferred embodiment of the present invention;
[0051] Among them: 1 is a sealing cover of a sealed container, 2 is a coating component, 3 is a sealing agent, 41 is a first opening, 42 is a second opening, 43 is a third opening, and 44 is a fourth opening. DETAILED DESCRIPTION
[0052] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0053] Example Sealing Agent
[0054] The thermal spray coating sealer in this embodiment includes three components: alloy powder, dispersant and carrier solvent. Among them, the mass proportion of alloy powder in the sealer is 5-10%, the mass proportion of dispersant is 30-40%, and the rest is carrier solvent. The viscosity of the sealer is 0.05-0.1 Pa·S at 25°C. The viscosity of the sodium silicate solvent is preferably 0.01-0.05 Pa·S at 25°C.
[0055] The dispersant in this embodiment is acetone, and the carrier is a sodium silicate solvent. The use of acetone and sodium silicate can achieve better dispersion and support effects of alloy powders than other reagents. In the sealing agent of this embodiment, the mass proportion of alloy powder is 8%, and the mass proportion of dispersant acetone is 35%. Reasonable control of the dispersant can control the dispersion effect of the alloy powder on the one hand, and the viscosity of the product on the other hand. The viscosity of the sodium silicate solvent is about 0.05 Pa·S at 25°C, and the viscosity of the sealing agent finally prepared is about 0.1 Pa·S at 25°C.
[0056] In this embodiment, the alloy powder contains 16% Cr, 4.5% Si, 2.5% B, and the balance is Ni, by mass percentage. By reasonably setting the proportion of each element in the alloy powder, the sealing effect and the sustained effect after the sealing agent is remelted are better; and such an element setting can be close to and applicable to most coating components in the nuclear power field, so that the bonding with the coating is stronger when the sealing agent is remelted to seal. In other embodiments, the alloy powder contains 11-19% Cr, 3.5-5.5% Si, 1.5-3.5% B, and the balance is Ni, by mass percentage.
[0057] The particle size of the alloy powder is in the range of 0.5-5 μm. If the particle size is too small, the remelting and sealing effects are poor, and if the particle size is too large, it cannot enter the pores of the coating. The particle size of the alloy powder in this embodiment is 2 μm.
[0058] The sealing agent prepared from alloy powder can achieve the sealing function after remelting the alloy powder, and has a good continuous effect and is not easy to fail. The dispersant is used to disperse the alloy powder to avoid the agglomeration of the alloy powder, and the carrier solvent is used to disperse and support the alloy powder to achieve the purpose of uniform dispersion of the alloy powder. And by controlling the proportion of alloy powder, the viscosity of the sealing agent, and the sealing process and method below, the sealing agent can flow into the pores of the coating and have a greater penetration depth, achieving a better sealing effect.
[0059] Example 2 Preparation method of sealing agent
[0060] This embodiment provides a method for preparing the sealing agent in Embodiment 1, which specifically includes the following steps: preparing an alloy block by a physical metallurgical method, using an aerosol method (high-speed airflow) to impact the alloy block to obtain an alloy powder, dispersing the alloy powder in acetone by ultrasonic waves to obtain an alloy solution, and adding the alloy solution to a carrier solvent to obtain a sealing agent, which is an oily substance. The alloy solution is first prepared and then mixed with the carrier solvent to form a sealing agent, which avoids the alloy powder from agglomerating and being unable to disperse. Ultrasonic waves can further disperse the alloy powder and prevent it from agglomerating.
[0061] Among them, the physical metallurgical method and the aerosol method for preparing alloy blocks are both conventional methods in the relevant fields.
[0062] Embodiment 3 Sealing method
[0063] like Figure 1-8 As shown, this embodiment provides a method for sealing holes using the above-mentioned sealing agent, which specifically includes the following steps:
[0064] A. Place the coated component 2 to be sealed in a sealed container. The sealed container includes a box body at the bottom and a cover 1 at the top. The side wall of the box body is provided with a first opening 41, a second opening 42 and a fourth opening 44. The bottom of the box body is provided with a third opening 43. The first opening 41 and the second opening 42 are located on the same side wall, and the height of the second opening 42 is lower than that of the first opening 41. The fourth opening 44 is located on the other side wall opposite to the box body. Figure 1 shown.
[0065] In this embodiment, the base material of the coating component is carbon steel, the coating material is NiCr alloy, the thickness of the coating is 250 μm, and the coating is prepared by arc spraying.
[0066] B. Open the second opening 42 and feed the liquid sealing agent 3 prepared in Example 1 into the sealed container through the second opening 42. Figure 2 shown.
[0067] C. Figure 3 As shown, the second opening 42 is closed, and the first opening 41 is opened, and the air in the sealed container is extracted from the top of the sealed container through the first opening 41, and finally the sealant 3 fills the entire sealed container, and the container is maintained in a negative pressure state, with a vacuum absolute pressure of 8Pa, for 30 minutes, and then the first opening 41 is closed. The negative pressure state can extract the air in the pores, which helps the sealant to flow into the pores inside the coating and reach a deeper penetration depth. In some other embodiments, the negative pressure is not higher than 10Pa (absolute pressure) and is maintained for 20 minutes.
[0068] D. Open the first opening 41 again, and release the pressure by connecting the container with the atmosphere through the first opening 41, so as to restore the pressure in the sealed container to normal pressure. Figure 4 shown.
[0069] E. Figure 5 As shown, pressure is applied from the top of the sealed container to the inside of the sealed container through the first opening 41, and then the first opening 41 is closed. The pressure is maintained at not less than 6 bar (absolute pressure) for not less than 20 minutes. That is, there is a positive pressure process after the negative pressure, and the pressurization operation can further force the sealing agent to enter the internal pores of the coating and achieve a deeper penetration depth.
[0070] F. Open the third opening 43 to discharge the sealing agent 3 in the sealed container. Figure 6 shown.
[0071] G. Such as Figure 7 As shown, the sealed container is connected to the hot water tank through the third opening 43 and the fourth opening 44 to form a water circuit, and the hot water circulates for 15 minutes to clean the residual sealing agent attached to the surface of the coating part, and the hot water temperature is not lower than 85° C. At the same time, under the heating of high-temperature water, the organic components of the sealing agent remaining in the pores of the coating solidify and fill the pores.
[0072] After all the air in the pores is extracted in step C, there is a negative pressure in the pores, so the sealant in the pores cannot flow out, and hot water can only clean the residual sealant attached to the surface of the coated parts.
[0073] H. Open the cover 1, take out the coated parts and let them dry. Figure 8 shown.
[0074] I. Use laser heating or other methods to heat and melt the sealant in the pores of the coating, so that the metal in the sealant is remelted in situ to form a dense surface structure, achieving the effect of sealing, with good sealing effect and sustained effect. Even at a service temperature of >500℃, the sealing effect is still maintained.
[0075] By adopting the above-mentioned process method in combination with the aforementioned sealing agent, the sealing agent can penetrate deeper into the pores of the coating and be remelted in situ in the pores, thereby fully achieving the sealing effect with good sustained effect.
[0076] Through the above steps A to I, the sealing process can be designed as an assembly line to achieve automated operation.
[0077] Embodiment 4 Sealing method
[0078] This embodiment is basically the same as Embodiment 3, except that the coating material in this embodiment is WC (tungsten carbide) and the coating preparation process is supersonic flame spraying.
[0079] Comparative Example 1
[0080] This comparative example uses the sealing agent in Example 1, but uses the traditional normal pressure brush coating process to seal the holes: brush it on the coating surface and let it stand for 30 minutes.
[0081] Comparative Example 2
[0082] It is basically the same as Example 3, except that the coating material in this embodiment is WC (tungsten carbide) and the coating preparation process is supersonic flame spraying.
[0083] The following is a comparison of the sealing penetration depth results of Examples 3-4 and Comparative Examples 1-2.
[0084]
[0085] The results in the above table show that for the coating prepared by the arc spraying process, the sealing method of Example 3 can achieve 100% penetration filling of the full thickness, while the conventional normal pressure brush sealing method can only penetrate to 20% of the coating thickness; for the coating prepared by the supersonic flame spraying process, the penetration depth of Example 4 is increased by 40% compared with the normal pressure brush sealing method. Therefore, the use of the above sealing agent and sealing method can effectively increase the penetration depth.
[0086] The invention provides a thermal spray coating sealant and a vacuum sealing method, designs a self-sealing metal alloy powder organic composite sealant, and provides a continuous automatic sealing method that utilizes vacuum to solve the technical defects of a brush-coating sealing process, thereby facilitating the automation of the sealing process.
[0087] The present application has the following advantages over traditional sealing agents and sealing processes: (1) The metal alloy powder sodium silicate sealing agent is resistant to high temperatures and corrosion, and can self-heal into a dense oxide film structure at high temperatures. (2) For coated parts prepared by arc spraying, the sealing agent can achieve full-thickness penetration and filling, greatly improving the service life of the coating. (3) The sealing curing time is shortened to 20% of the normal pressure brush sealing process, that is, the sealing curing time of a single coated part does not exceed 5 hours, greatly improving the coating sealing efficiency. (4) The use of the sealing agent and sealing process of the present application can realize a batch automated sealing line for workpieces, greatly improving the production efficiency of thermal spraying.
[0088] The preparation method of the self-sealing sealing agent for thermal spray coating of the present application adopts alloy powder to prepare the sealing agent, and the alloy powder can be remelted to achieve the sealing function, and the continuous effect is good and not easy to fail. The dispersant is used to disperse the alloy powder to avoid the agglomeration of the alloy powder, and the carrier solvent is used to disperse and support the alloy powder to achieve the purpose of uniform dispersion of the alloy powder. And by controlling the proportion of the alloy powder and the viscosity of the sealing agent, combined with the sealing process and method, the sealing agent can flow into the pores of the coating and have a greater penetration depth, achieving a better sealing effect.
[0089] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a thermal spray coating sealing agent, characterized in that: The sealing agent comprises alloy powder, dispersant and carrier; the preparation method comprises the following steps: dispersing the alloy powder in the dispersant to obtain an alloy solution, and mixing the alloy solution with a carrier solvent to obtain the sealing agent; The alloy powder contains 11-19% Cr, 3.5-5.5% Si, 1.5-3.5% B, and the balance is Ni; the mass proportion of the alloy powder in the sealing agent is 5-10%; the particle size range of the alloy powder is 0.5-5μm; the dispersant is acetone; the mass proportion of the dispersant in the sealing agent is 30-40%; the carrier is a sodium silicate solvent; the viscosity of the sodium silicate solvent is 0.01-0.05Pa·S at 25°C; the viscosity of the sealing agent is 0.05-0.1Pa·S at 25°C.
2. The method for preparing the sealing agent according to claim 1, characterized in that: The alloy powder is prepared by the following steps: preparing an alloy block by a physical metallurgical method, and impacting the alloy block by an aerosol method to obtain the alloy powder.
3. The method for preparing the sealing agent according to claim 1, characterized in that: The dispersion is to disperse the alloy powder in a dispersant by ultrasonic wave to obtain an alloy solution.
4. The method for preparing the sealing agent according to any one of claims 1 to 3, characterized in that: The sealing agent is an oily substance.