Composite adsorbent for decontamination of fluorosilicic acid and preparation method thereof
By using polymetal oxide-loaded activated carbon adsorbent in wet phosphoric acid production, the problem of synchronous removal of arsenic, iodine and chlorine impurities in fluosilicate is solved, and efficient, economical and safe demulsification effect is achieved, and the process is simplified process.
Patent Information
- Application Number
- CN202310446249.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-24
AI Technical Summary
The prior art is difficult to simultaneously remove arsenic, iodine and chlorine impurities in fluosilicate during the wet phosphoric acid production process, and the industrial series demixing process is complex and has poor economicality.
Using a composite adsorbent prepared by sol-gel and carbonization method from water-soluble polymers and soluble metal nitrates, arsenic, iodine and chlorine are achieved using its porous structure and oxidation capacity of metal oxides. synchronous adsorption.
It realizes efficient synchronous removal of arsenic, iodine and chlorine in fluosilicate, has excellent acid and corrosion resistance, simplifies the process flow, reduces costs, and is recyclable and used.
Smart Images

Figure CN116422306B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a composite adsorbent for removing impurities from by-product fluorosilicic acid from phosphoric acid and a preparation method thereof. Background Art
[0002] Fluorosilicic acid is mainly a by-product of wet-process phosphoric acid. During the concentration of wet-process phosphoric acid, fluorine escapes in the form of silicon tetrafluoride and is absorbed by water to become a fluosilicic acid solution, with an output of about 5%-6% of the output of wet-process phosphoric acid. However, during the production of wet-process phosphoric acid, arsenic, iodine and chlorine in phosphate rock also enter the wet-process phosphoric acid and escape together with silicon tetrafluoride as the wet-process phosphoric acid is concentrated, and eventually remain in the fluosilicic acid solution as impurities, affecting the quality of fluosilicic acid and a series of downstream fluorine-containing chemicals produced with it as raw materials, such as sodium fluosilicate, cryolite, ammonium fluoride, and hydrofluoric acid.
[0003] The impurities contained in the byproduct of phosphoric acid, fluorosilicic acid, are mainly arsenic, iodine and chlorine. The content depends on the content of impurities in the phosphate ore. The content of impurities in the phosphate ore is related to its origin and grade, but in general, the impurity content in fluorosilicic acid is at a trace level. Regarding the public literature on the removal of impurities from fluorosilicic acid, CN111252770A uses electrolysis to remove chlorine from fluorosilicic acid; CN111017930A uses hydrogen peroxide oxidation and falling film evaporation to remove iodine from fluorosilicic acid; CN111908425A and CN 101033067A use oxidation and precipitation methods to remove arsenic from fluorosilicic acid, respectively.
[0004] However, the above reports are only for the removal of single impurities in fluosilicic acid. If the above methods are used in series for synergistic removal of impurities in industry, not only the process is complicated but also the economic efficiency is poor. Up to now, there has been no report on the technology for the simultaneous removal of arsenic, iodine and chlorine impurities in fluosilicic acid.
[0005] The main methods for removing impurities from solutions at home and abroad include precipitation, adsorption, ion exchange, extraction, biological method, reverse osmosis, etc. Among them, the adsorption method uses solid adsorbents to remove impurities in the liquid phase. It can not only achieve the effect of impurity removal by solid-liquid separation, but also is not easy to introduce other impurities to cause secondary pollution. It is especially suitable for solution systems with large processing volume and low impurity content. It has developed into a commonly used solution removal method in industrialization. The excellent impurity removal performance depends on the adsorption material. Summary of the invention
[0006] The purpose of the present invention is to solve the above technical problems and to provide a method for preparing a composite adsorbent for removing impurities from fluorosilicic acid, which has a simple method of use, low cost, can realize continuous processing, can simultaneously remove arsenic, iodine and chlorine impurities in fluorosilicic acid, has high impurity removal efficiency, and is safe and environmentally friendly.
[0007] Another object of the present invention is to provide a composite adsorbent prepared by the above method.
[0008] The technical solution includes the following steps:
[0009] (1) dissolving a water-soluble polymer containing a carboxylate, phosphate or sulfonate functional group in deionized water to obtain an aqueous solution of the water-soluble polymer;
[0010] (2) dissolving a soluble metal nitrate in deionized water to obtain an aqueous solution, adding the aqueous solution to the above-mentioned water-soluble polymer solution, mixing evenly and standing to obtain a hydrogel, and washing the hydrogel in deionized water for multiple times until no free metal salt ions are present;
[0011] (3) drying the hydrogel to obtain an aerogel;
[0012] (4) Carbonizing the aerogel at high temperature under an inert atmosphere to obtain a composite adsorbent.
[0013] In the step (1), the water-soluble polymer containing carboxylate, phosphate or sulfonate is one of polyacrylic acid, polyacrylic acid-acrylamide, phytic acid, lignin sulfonic acid, polystyrene sulfonic acid and TEMPO oxidized cellulose nanofibers.
[0014] The aqueous solution concentration of the water-soluble polymer containing carboxylate, phosphate or sulfonate obtained in step (1) is 0.5-5wt%.
[0015] In step (2), the soluble metal nitrate is selected from at least two of cerium nitrate, aluminum nitrate and magnesium nitrate, preferably all three are used simultaneously, cerium nitrate, magnesium nitrate and aluminum nitrate, and the molar ratio of the three is 1: (0.5-1.5): (0.5-1.5).
[0016] The concentration of the soluble metal nitrate aqueous solution in step (2) is 0.1 to 5 wt%.
[0017] The solid weight ratio of the metal nitrate to the water-soluble polymer in step (2) is 1:(1-50).
[0018] The drying method of the hydrogel in step (3) is natural drying, heating drying, supercritical drying, vacuum drying or freeze drying.
[0019] In step (3), the hydrogel is frozen and then dried at low temperature in a freeze dryer, and the freeze drying temperature is -10°C to -50°C.
[0020] The carbonization temperature in step (4) is 500-2000°C.
[0021] The composite adsorbent for removing impurities from fluorosilicic acid of the present invention is prepared by the above method.
[0022] The impurity removal method of the adsorbent prepared by the present invention is extremely simple. The specific operation listed is to add the composite adsorbent of the present invention to the fluosilicic acid solution, and filter after standing for adsorption to obtain a fluosilicic acid solution with low impurity content. The ratio of the composite adsorbent to the fluosilicic acid solution is 1g: (10-1000) mL, preferably 1g: (10-500) mL, and the standing adsorption time is 1-48h, preferably (10-30)h.
[0023] Furthermore, the adsorbed composite adsorbent can be regenerated by the following desorption method, which is: adding the adsorbed composite adsorbent to a NaOH solution or an NH4OH solution, shaking it in a shaker for 10-48 hours, filtering and drying it, and then reusing it.
[0024] The present invention adopts sol-gel and carbonization methods to prepare a multi-metal oxide loaded activated carbon adsorbent. A water-soluble polymer with carboxylate, phosphate or sulfonate functional groups on the surface is used as a carbon precursor, and carboxylate, phosphate or sulfonate is used as an ion crosslinking site. A hydrogel with a three-dimensional spatial network structure is formed by metal ion crosslinking. The hydrogel is dried to form a porous aerogel. The aerogel is carbonized at high temperature to become activated carbon. The metal ions are converted into cerium, magnesium, and aluminum multi-metal oxides loaded on the activated carbon during the carbonization process. In principle, firstly, the porous structure of activated carbon is very conducive to the adsorption of impurities. Secondly, CeO2 in the multi-metal oxide can be used as an oxidant to oxidize the highly toxic As(III) in the fluosilicic acid solution into As(V) with low toxicity, and selectively adsorb it; the magnesium-aluminum-containing multi-metal oxide can form a layered hydrotalcite structure, which can selectively adsorb chloride ions and iodide ions. The three work together to achieve the purpose of synchronous removal of arsenic, iodine and chlorine impurities. Preferably, the molar ratio of cerium nitrate, magnesium nitrate and aluminum nitrate is 1:(0.5-1.5):(0.5-1.5), wherein further, the weight ratio of the metal nitrate to the water-soluble polymer is 1:(1-50), more preferably 1:(1-20), to ensure that the metal ions and the water-soluble polymer are fully cross-linked to construct a three-dimensional network structure to form a shape-stable hydrogel. Relative to the water-soluble polymer, too high an addition amount of the metal nitrate will lead to flocculation and precipitation of the water-soluble polymer, while too low an addition amount will result in the polymer aqueous solution being unable to fully cross-link to form a hydrogel structure.
[0025] Beneficial effects of the present invention:
[0026] (1) The composite adsorbent of the present invention can simultaneously remove arsenic, iodine and chlorine impurities in fluorosilicic acid and has excellent acid and corrosion resistance, which can overcome the problem that other solid adsorbents have a single adsorption performance and cannot be used due to the high acidity of fluorosilicic acid.
[0027] (2) The multi-metal ions in the modified activated carbon of the present invention are combined with the polymer matrix material in the form of ion pairs, wherein the metal ions not only serve as a cross-linking agent, but also as a modifier to load the activated carbon with multi-metal oxides. Not only is the loading capacity large but it is also not easy to fall off, thereby increasing the adsorption performance of the activated carbon for impurities and can be used directly without complicated activation treatment.
[0028] (3) The composite adsorbent of the present invention can construct activated carbon using water-soluble polymers as carbon precursors, and the pore structure in the activated carbon can be adjusted by process conditions. The pore structure with micropore size can provide a larger specific surface area and a larger adsorption capacity.
[0029] (4) The preparation method of the adsorbent of the present invention is simple, the raw material cost is low, continuous processing can be achieved, the arsenic, iodine and chlorine impurities in fluorosilicic acid can be removed simultaneously, the impurity removal efficiency is high, and it is safe and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a scanning electron microscope (SEM) image of pure TOCN aerogel.
[0031] Figure 2 This is a scanning electron microscope (SEM) image of the CeO2-MgO-Al2O3 loaded TOCN aerogel prepared in Example 6. DETAILED DESCRIPTION
[0032] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0033] Example 1
[0034] Polyacrylic acid is used as a carbon precursor, added into deionized water and dissolved with mechanical stirring, and then dispersed for 2 minutes with a high-speed stirrer at a speed of 6000r / min to prepare a uniform aqueous solution with a concentration of 0.5wt%; Ce(NO3)2 and Mg(NO3)2 are dispersed in deionized water at a molar ratio of 1:1 to prepare an aqueous solution with a concentration of 5wt%; 100mL of the polyacrylic acid aqueous solution is placed in a beaker, 50mL of the above-mentioned metal nitrate aqueous solution is added for cross-linking, and the hydrogel is allowed to stand at room temperature for 48h to obtain the hydrogel, the hydrogel is washed and replaced with deionized water for 5 times, and then quickly frozen with liquid nitrogen and freeze-dried at -45°C to obtain the aerogel; finally, the above-mentioned aerogel is placed in a tubular furnace and carbonized for 4h at 650°C in an argon atmosphere to obtain CeO2-MgO loaded activated carbon.
[0035] The raw material fluorosilicic acid was taken and the arsenic content was determined to be 50 mg / L, the chlorine content was 1.8 wt %, and the iodine content was 28 mg / L.
[0036] Weigh 10 g of the CeO2-MgO loaded activated carbon mentioned above and add it to 100 mL of fluorosilicic acid raw material. After standing at 25°C for 24 hours, filter it. After analysis, the arsenic content in the filtrate is 40 mg / L, the chlorine content is 1.4 wt%, and the iodine content is 26 mg / L.
[0037] Example 2
[0038] Polyacrylic acid is used as a carbon precursor, added into deionized water and dissolved with mechanical stirring, and then dispersed for 2 minutes with a high-speed stirrer at a speed of 6000r / min to prepare a uniform aqueous solution with a concentration of 2wt%; Ce(NO3)2 and Mg(NO3)2 are dispersed in deionized water at a molar ratio of 1:1 to prepare an aqueous solution with a concentration of 5wt%; 100mL of the polyacrylic acid aqueous solution is placed in a beaker, 50mL of the above-mentioned metal nitrate aqueous solution is added for cross-linking, and the hydrogel is allowed to stand at room temperature for 48h to obtain the hydrogel, the hydrogel is washed and replaced with deionized water for 5 times, and then quickly frozen with liquid nitrogen and freeze-dried at -45°C to obtain the aerogel; finally, the above-mentioned aerogel is placed in a tubular furnace and carbonized for 4h at 650°C in an argon atmosphere to obtain CeO2-MgO loaded activated carbon.
[0039] The raw material fluorosilicic acid was taken and the arsenic content was determined to be 50 mg / L, the chlorine content was 1.8 wt %, and the iodine content was 28 mg / L.
[0040] Weigh 10 g of the CeO2-MgO loaded activated carbon mentioned above and add it to 100 mL of fluorosilicic acid raw material. After standing at 25°C for 24 hours, filter it. After analysis, the arsenic content in the filtrate is 24 mg / L, the chlorine content is 0.5 wt%, and the iodine content is 13 mg / L.
[0041] Example 3
[0042] Polyacrylic acid is used as a carbon precursor, added into deionized water and dissolved with mechanical stirring, and then dispersed for 2 minutes with a high-speed stirrer at a speed of 6000r / min to prepare a uniform aqueous solution with a concentration of 5wt%; Ce(NO3)2 and Mg(NO3)2 are dispersed in deionized water at a molar ratio of 1:1 to prepare an aqueous solution with a concentration of 5wt%; 100mL of the polyacrylic acid aqueous solution is placed in a beaker, 50mL of the above-mentioned metal nitrate aqueous solution is added for cross-linking, and the hydrogel is allowed to stand at room temperature for 48h to obtain the hydrogel, the hydrogel is washed and replaced with deionized water for 5 times, and then quickly frozen with liquid nitrogen and freeze-dried at -45°C to obtain the aerogel; finally, the above-mentioned aerogel is placed in a tubular furnace and carbonized for 4h at 650°C in an argon atmosphere to obtain CeO2-MgO loaded activated carbon.
[0043] The raw material fluorosilicic acid was taken and the arsenic content was determined to be 50 mg / L, the chlorine content was 1.8 wt %, and the iodine content was 28 mg / L.
[0044] Weigh 10 g of the CeO2-MgO loaded activated carbon mentioned above and add it to 100 mL of fluorosilicic acid raw material. After standing at 25°C for 24 hours, filter it. After analysis, the arsenic content in the filtrate is 30 mg / L, the chlorine content is 0.8 wt%, and the iodine content is 15 mg / L.
[0045] Example 4
[0046] The decontamination operation in Example 2 was repeated for the fluorosilicic acid obtained in Example 2. 20 g of CeO2-MgO-loaded activated carbon was weighed and added to 100 mL of fluorosilicic acid raw material. The mixture was allowed to stand at 25°C for 24 h and then filtered. Analysis showed that the arsenic content in the fluorosilicic acid filtrate was 15 mg / L, the chlorine content was 0.36 wt%, and the iodine content was 10 mg / L.
[0047] Example 5
[0048] A TEMPO oxidized cellulose nanofiber slurry with a water content of 70wt% was used as a carbon precursor (TEMPO oxidized cellulose nanofibers were prepared using the method disclosed in the paper "TEMPO-oxidized cellulose nanofibers"), and then the slurry was added to deionized water, and a 1wt% aqueous solution was obtained after mechanical stirring and dispersion by a high-pressure homogenizer. Ce(NO3)2 and Mg(NO3)2 were dispersed in deionized water at a molar ratio of 1:1 to prepare an aqueous solution with a concentration of 5wt%; 100mL of the aqueous solution was placed in a beaker, and 30mL of the above metal nitrate aqueous solution was added for cross-linking, and the hydrogel was obtained by standing at room temperature for 48h, and then the aerogel was obtained by freeze-drying at -45℃ after quick freezing with liquid nitrogen; the above aerogel was placed in a tubular furnace and carbonized for 2.5h at 800℃ in an argon atmosphere to obtain CeO2-MgO loaded activated carbon.
[0049] The raw material fluorosilicic acid was taken and the arsenic content was determined to be 50 mg / L, the chlorine content was 1.8 wt %, and the iodine content was 28 mg / L.
[0050] Weigh 10 g of the above-mentioned CeO2-MgO loaded activated carbon and add it to 100 mL of fluorosilicic acid raw material. After standing at 25°C for 24 hours, filter it and repeat the above-mentioned decontamination operation on the obtained filtrate. After analysis, the arsenic content in the fluorosilicic acid filtrate was 12 mg / L, the chlorine content was 0.18 wt% and the iodine content was 10 mg / L.
[0051] Example 6
[0052] A TEMPO-oxidized cellulose nanofiber oxidized pulp with a water content of 70wt% was used as a carbon precursor (TEMPO-oxidized cellulose nanofibers were prepared using the method disclosed in the paper "TEMPO-oxidized cellulose nanofibers"), and then the oxidized pulp was added to deionized water, and a 1wt% aqueous solution was obtained after mechanical stirring and dispersion by a high-pressure homogenizer. Ce(NO3)2, Mg(NO3)2 and Al(NO3)3 were dispersed in deionized water at a molar ratio of 1:1:1 to prepare an aqueous solution with a concentration of 5wt%; 100mL of the aqueous solution was placed in a beaker, and 30mL of the above metal nitrate aqueous solution was added for cross-linking, and the hydrogel was obtained by standing at room temperature for 48h, and then the aerogel was obtained by freeze-drying at -45℃ after quick freezing with liquid nitrogen; the above aerogel was placed in a tubular furnace and carbonized for 2.5h at 800℃ in an argon atmosphere to obtain CeO2-MgO-Al2O3-loaded activated carbon.
[0053] The raw material fluorosilicic acid was taken and the arsenic content was determined to be 50 mg / L, the chlorine content was 1.8 wt %, and the iodine content was 28 mg / L.
[0054] Weigh 10 g of the above-mentioned CeO2-MgO-Al2O3 loaded activated carbon and add it to 100 mL of fluorosilicic acid raw material. After standing at 25°C for 24 hours, filter it and repeat the above-mentioned decontamination operation on the obtained filtrate. After analysis, the arsenic content in the fluorosilicic acid filtrate was 12 mg / L, the chlorine content was 0.16wt% and the iodine content was 8 mg / L.
[0055] from Figure 1 It can be seen that in pure TOCN aerogel, under the action of intramolecular and intermolecular hydrogen bonds, carbon nanofibers form a three-dimensional network structure; SEM image of CeO2-MgO-Al2O3 loaded TOCN aerogel prepared in Example 6 ( Figure 2 ), it can be clearly seen that a large amount of metal oxides are loaded on the surface of the carbon nanofibers, and the presence of the coating indicates that the loading amount of the metal oxides is large.
[0056] Example 7
[0057] The CeO2-MgO-Al2O3 loaded activated carbon adsorbed in Example 6 was regenerated, and the composite adsorbent after adsorption was added to a NaOH solution or an NH4OH solution with a concentration of 1 mol / L. After shaking in a shaking table for 24 hours, the regeneration was completed by filtering and drying. 20 g of the regenerated CeO2-MgO-Al2O3 loaded activated carbon was added to 100 mL of fluorosilicic acid raw material according to the method in Example 6, and filtered after standing at 25°C for 24 hours. The above-mentioned decontamination operation was repeated for the obtained filtrate. After analysis, the arsenic content in the fluorosilicic acid filtrate was 14 mg / L, the chlorine content was 0.19wt%, and the iodine content was 9 mg / L.
Claims
1. A method for preparing a composite adsorbent for decontamination of fluorosilicic acid, characterized in that: The following steps are involved: (1) dissolving a water-soluble polymer containing a carboxylate, phosphate or sulfonate functional group in deionized water to obtain an aqueous solution of the water-soluble polymer; (2) dissolving a soluble metal nitrate in deionized water to obtain an aqueous solution, adding the aqueous solution to the above-mentioned water-soluble polymer solution, mixing evenly and standing to obtain a hydrogel, and washing the hydrogel in deionized water for multiple times until no free metal salt ions are present; the soluble metal nitrate is selected from at least two of cerium nitrate, aluminum nitrate and magnesium nitrate; (3) drying the hydrogel to obtain an aerogel; (4) Carbonizing the aerogel at high temperature under an inert atmosphere to obtain a composite adsorbent.
2. The method for preparing a composite adsorbent for removing impurities from fluorosilicic acid according to claim 1, characterized in that: In the step (1), the water-soluble polymer containing carboxylate, phosphate or sulfonate is one of polyacrylic acid, polyacrylic acid-acrylamide, phytic acid, lignin sulfonic acid, polystyrene sulfonic acid and TEMPO oxidized cellulose nanofibers.
3. The method for preparing a composite adsorbent for removing impurities from fluorosilicic acid according to claim 1, characterized in that: The aqueous solution concentration of the water-soluble polymer containing carboxylate, phosphate or sulfonate obtained in step (1) is 0.5-5wt%.
4. The method for preparing a composite adsorbent for removing impurities from fluorosilicic acid according to claim 1, wherein: The concentration of the soluble metal nitrate aqueous solution in step (2) is 0.1 to 5 wt%.
5. The method for preparing a composite adsorbent for removing impurities from fluorosilicic acid according to claim 4, characterized in that: The solid weight ratio of the metal nitrate to the water-soluble polymer in step (2) is 1:(1-50).
6. The method for preparing a composite adsorbent for removing impurities from fluorosilicic acid according to claim 1, characterized in that: The drying method of the hydrogel in step (3) is supercritical drying or freeze drying.
7. The method for preparing a composite adsorbent for removing impurities from fluorosilicic acid according to claim 6, characterized in that: In step (3), the hydrogel is frozen and then dried at low temperature in a freeze dryer, and the freeze drying temperature is -10°C to -50°C.
8. The method for preparing a composite adsorbent for removing impurities from fluorosilicic acid according to claim 1, characterized in that: The carbonization temperature in step (4) is 500-2000°C.
9. A composite adsorbent for dedoping fluorosilicic acid, characterized in that: Prepared by the method of any one of claims 1 to 8.