A seawater-degradable film and preparation method thereof

By using bio-based materials PLGA, PHBH and corn starch, combined with PPC and PBAT, the problem of high carbon emissions of seawater-degradable materials has been solved, and a low-carbon emission and biodegradable seawater film has been achieved, which has excellent mechanical properties and meets flow requirements. Shelf life.

CN116426099BActive Publication Date: 2024-10-29DANYANG HENGLV NEW MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310441598.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-10-29
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

Existing seawater degradation materials have high carbon emissions and affect the environment.

Method used

It uses bio-based seawater-degradable materials PLGA, PHBH and corn starch as the main base materials, and adds low-carbon emission PPC and extremely flexible PBAT, combined with multi-composite modification technology and reactive additive organic peroxide to enhance the material With high compatibility and processing stability, seawater-degradable films with excellent mechanical properties can be prepared.

Benefits of technology

While ensuring the seawater degradation properties, it also greatly reduces the carbon emissions of the material. The film can be completely biodegraded after being discarded into the sea, does not form microplastics, meets the shelf life required for circulation, and provides excellent mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004194174680000021
    Figure BDA0004194174680000021
  • Figure BDA0004194174680000041
    Figure BDA0004194174680000041
  • Figure BDA0004194174680000051
    Figure BDA0004194174680000051
Patent Text Reader

Abstract

The invention provides a seawater degradable film and a preparation method thereof, and relates to the technical field of biodegradable films. The seawater degradable film provided by the invention uses bio-based seawater degradable materials PLGA, PHBH and corn starch as main substrates, and greatly reduces the carbon emission of the materials while ensuring the seawater degradation characteristics. At the same time, biodegradable materials with a long degradation cycle, including PPC with low carbon emission and PBAT with excellent flexibility, are added to the formula system to ensure that the final film has a shelf life that meets the circulation requirements. In addition, based on the multi-component composite modification technology of degradable materials, the invention selects reactive auxiliary organic peroxides to break through the compatibility problem between the multiphase interfaces of PLGA, PHBH, PPC, PBAT and corn starch, and provides a guarantee for the processing stability of PLGA and PHBH, so as to prepare a composite material with excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biodegradable films, and in particular to a seawater degradable film and a preparation method thereof. Background Art

[0002] According to statistics, more than 8 million tons of plastic are abandoned in the ocean every year, accounting for 80% of marine garbage. Such a large amount of discarded plastic entering the ocean will seriously endanger the safety of marine life. There have been quite a few reports that a large amount of discarded plastic has been found in the bodies of marine animals such as turtles and sharks. In addition, as time goes by, plastic garbage in the ocean will be powdered into microplastics, enter the sea salt, and eventually accumulate in the human body. At present, there have been reports that a large amount of microplastics have been found in human blood. Therefore, the governance of plastic pollution in the ocean is urgent.

[0003] The promotion and use of seawater degradable materials is considered to be the most fundamental and effective way to solve marine plastic pollution. Therefore, the research on seawater degradable materials has become a hot topic of concern for many scientific researchers in recent years. For example, the invention patent with application publication number CN113307959A improves its hydrophilicity by introducing an imine structure on the PBS main chain, reduces the activation energy of PBS degradation in seawater, and thus improves the degradation rate of PBS in seawater. The prepared PBS copolyester material is degradable in seawater and has a regulated cycle, and has good application prospects. The invention patent with application publication number CN113121803A improves its non-enzymatic hydrolysis of seawater by introducing an ethanolic acid structure on the PEF main chain, and improves its enzymatic hydrolysis of seawater by introducing a caprolactone structure, thereby improving the degradation rate of PEF in seawater. The invention patent with application publication number CN108624020A mixes thermoplastic modified polyvinyl alcohol, polyester and compatibilizer in proportion, and obtains seawater degradable materials with adjustable service cycle and degradation cycle by extrusion granulation and injection molding.

[0004] The above inventions all provide seawater-degradable materials with good comprehensive performance, but all of them are based on petroleum-based resins and have relatively high overall carbon emissions. Summary of the invention

[0005] The technical problem to be solved by the present invention is: in order to solve the problem of high carbon emissions of seawater degradable materials in the prior art, the present invention provides a seawater degradable film, which uses bio-based seawater degradable materials PLGA, PHBH and corn starch as main substrates. While ensuring the seawater degradation characteristics, the carbon emissions of the materials are greatly reduced, solving the problem of high carbon emissions of seawater degradable materials in the prior art.

[0006] The technical solution adopted by the present invention to solve its technical problem is:

[0007] A seawater-degradable film, comprising the following components in parts by weight:

[0008]

[0009] Optionally, the molecular weight M of the polylactic acid-glycolic acid copolymer is W ≥60000, the mass content of GA in the molecular structure unit is ≥80%, the melt flow rate MFR ≤7g / 10min (190℃, 2.16KG), and the melting point ≤175℃.

[0010] Optionally, the molecular weight M of the 3-hydroxybutyrate-co-3-hydroxyhexanoate is W ≥50000, melt flow rate MFR≤5g / 10min (165℃, 5KG), melting point≤150℃.

[0011] Optionally, the plasticizer is selected from at least one of glycerol and sorbitol.

[0012] Optionally, the starch treating agent is selected from at least one of stearic acid and a polyhydroxy polymer superdispersible modifier.

[0013] Optionally, the organic peroxide is MH.

[0014] Optionally, the ethylene-vinyl acetate copolymer is 2504.

[0015] Optionally, the antioxidant is a mixture of the antioxidant 1010 and the antioxidant 168, and the mass ratio of the antioxidant 1010 to the antioxidant 168 is 1:2.

[0016] Another object of the present invention is to provide a method for preparing the seawater-degradable film as described above, comprising the following steps:

[0017] S1: According to the formula amount, corn starch and starch treatment agent are added into a high-speed mixer, and mixed at a speed of 200 rpm; then a plasticizer is added, and mixed at a speed of 600 rpm; finally adipic acid and citric acid are added, and mixed at a speed of 200 rpm to prepare plasticized corn starch;

[0018] S2: According to the formula, polylactic acid-glycolic acid copolymer, 3-hydroxybutyrate-co-3-hydroxycaproate, polypropylene carbonate, polybutylene adipate / terephthalate, organic peroxide and white oil are added to a mixer with a fixed speed of 80 rpm and mixed; then ethylene-vinyl acetate copolymer and antioxidant are added and mixed; finally, the plasticized corn starch is added, mixed, and stirred evenly to prepare a mixed masterbatch;

[0019] S3: adding the mixed masterbatch into a parallel twin-screw extruder, melt blending and air-cooling pelletizing to prepare a seawater-degradable blown film material;

[0020] S4: forming the seawater-degradable film-blowing material by film blowing to obtain a seawater-degradable film.

[0021] The beneficial effects of the present invention are:

[0022] The seawater degradable film provided by the present invention uses bio-based seawater degradable materials PLGA, PHBH and corn starch as main substrates, while ensuring the seawater degradation characteristics, greatly reducing the carbon emission of the materials; at the same time, biodegradable materials with a long degradation cycle are added to the formula system, including PPC with low carbon emissions and PBAT with excellent flexibility, so as to ensure that the final film has a shelf life that meets the circulation requirements; after the film is discarded into the sea, most of the materials will be degraded by seawater to form film fragments of PPC and PBAT, because the film fragments have the characteristics of biodegradation, they will not cause harm to the marine ecology, and will not eventually form microplastics; in addition, the present invention is based on the multi-component composite modification technology of degradable materials, and selects reactive auxiliary organic peroxides to break through and solve the compatibility problem between the multiphase interfaces of PLGA, PHBH, PPC, PBAT and corn starch, and provide a guarantee for the processing stability of PLGA and PHBH, so as to prepare a composite material with excellent mechanical properties. DETAILED DESCRIPTION

[0023] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0024] In order to solve the problem of high carbon emission of seawater degradable materials in the prior art, the present invention provides a seawater degradable film, which comprises the following components in parts by weight:

[0025]

[0026]

[0027] The seawater degradable film provided by the present invention uses bio-based seawater degradable materials PLGA, PHBH and corn starch as main substrates, while ensuring the seawater degradation characteristics, greatly reducing the carbon emission of the materials; at the same time, biodegradable materials with a long degradation cycle are added to the formula system, including PPC with low carbon emissions and PBAT with excellent flexibility, so as to ensure that the final film has a shelf life that meets the circulation requirements; after the film is discarded into the sea, most of the materials will be degraded by seawater to form film fragments of PPC and PBAT, because the film fragments have the characteristics of biodegradation, they will not cause harm to the marine ecology, and will not eventually form microplastics; in addition, the present invention is based on the multi-component composite modification technology of degradable materials, and selects reactive auxiliary organic peroxides to break through and solve the compatibility problem between the multiphase interfaces of PLGA, PHBH, PPC, PBAT and corn starch, and provide a guarantee for the processing stability of PLGA and PHBH, so as to prepare a composite material with excellent mechanical properties.

[0028] In order to take into account both the degradation performance and mechanical properties of the seawater-degradable film, the molecular weight M of the polylactic acid-glycolic acid copolymer is preferably W ≥60000, the mass content of GA in the molecular structural unit is ≥80%, the melt flow rate MFR ≤7g / 10min (190℃, 2.16KG), the melting point ≤175℃; preferably the molecular weight M of 3-hydroxybutyrate-co-3-hydroxyhexanoate W ≥50000, melt flow rate MFR≤5g / 10min (165℃, 5KG), melting point≤150℃.

[0029] The preferred plasticizer of the present invention is selected from at least one of glycerol and sorbitol; the preferred starch treating agent is selected from at least one of stearic acid and a polyhydroxy polymer superdispersible modifier, and the specifically preferred polyhydroxy polymer superdispersible modifier is JL-G02FX-P.

[0030] The preferred organic peroxide of the present invention is Arkema MH; preferably ethylene-vinyl acetate copolymer is 2504; Preferably, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168, and the mass ratio of antioxidant 1010 to antioxidant 168 is 1:2.

[0031] Another object of the present invention is to provide a method for preparing the seawater-degradable film as described above, comprising the following steps:

[0032] S1: According to the formula amount, corn starch and starch treatment agent are added to a high-speed mixer, and mixed at a speed of 200 rpm, preferably for 2 minutes; then a plasticizer is added, and mixed at a speed of 600 rpm, preferably for 8 minutes; finally adipic acid and citric acid are added, and mixed at a speed of 200 rpm, preferably for 1 minute, to prepare plasticized corn starch;

[0033] S2: According to the formula amount, polylactic acid-glycolic acid copolymer, 3-hydroxybutyrate-co-3-hydroxycaproate, polypropylene carbonate, polybutylene adipate / terephthalate, organic peroxide and white oil are added to a mixer with a fixed speed of 80 rpm and mixed, preferably for 30 seconds; then ethylene-vinyl acetate copolymer and antioxidant are added, mixed, preferably for 30 seconds; finally, plasticized corn starch is added, mixed, preferably for 1 minute, and stirred evenly to prepare a mixed masterbatch;

[0034] S3: adding the mixed masterbatch into a parallel twin-screw extruder, melt blending and air-cooling pelletizing to prepare a seawater-degradable blown film material; preferably, in this step, the temperature of zones 1-9 of the twin-screw extruder is set to 130° C., 180° C., 180° C., 180° C., 175° C., 170° C., 170° C., 170° C., 170° C., and the die head temperature is 170° C.;

[0035] S4: Blowing the seawater degradable film material into film to obtain a seawater degradable film; preferably using an ordinary high-pressure PE film blowing machine for film blowing, setting the temperatures of zones 1-5 of the film blowing machine to 130°C, 180°C, 180°C, 180°C, 180°C, and the die head temperature to 175°C, and finally obtaining a seawater degradable film with a thickness of 40 μm and a width of 600 mm.

[0036] Since the decomposition temperature of pure starch is lower than the plasticization temperature and it does not have processing fluidity, step S1 of the present invention increases the plasticity of the starch by plasticizing and modifying the corn starch to facilitate subsequent blow molding. In this step, adipic acid and citric acid are compounded to esterify the hydroxyl groups in the starch to improve the hydrophobic properties.

[0037] The method for preparing a seawater-degradable film provided by the present invention has a simple process. In the preparation process, bio-based seawater-degradable materials PLGA, PHBH and corn starch are used as main substrates, and the carbon emission of the materials is greatly reduced while ensuring the seawater degradation characteristics. At the same time, biodegradable materials with a long degradation cycle are added to the formula system, including PPC with low carbon emissions and PBAT with excellent flexibility, so as to ensure that the final film has a shelf life that meets the circulation requirements. After the film is discarded into the sea, most of the materials will be degraded by seawater to form film fragments of PPC and PBAT. Since the film fragments have the characteristics of biodegradation, they will not cause harm to the marine ecology, and will not eventually form microplastics. In addition, the present invention is based on the multi-component composite modification technology of degradable materials, and the reactive auxiliary agent organic peroxide is selected to break through the compatibility problem between the multiphase interface of PLGA, PHBH, PPC, PBAT and corn starch, and the processing stability of PLGA and PHBH is guaranteed, so as to prepare a composite material with excellent mechanical properties. Ethylene-vinyl acetate copolymer is added as a sealing agent in the preparation process to improve the heat sealing performance of the prepared film.

[0038] Compared with traditional film bags, the low-carbon seawater degradable film provided by the present invention can achieve a weight loss rate of more than 40% after degradation in seawater within 3 months. The degradation products will not cause harm to the marine ecology and will not ultimately form microplastics. At the same time, the shelf life can meet the circulation requirements of production, sales and use, which is of great significance for solving the problem of marine pollution caused by discarded plastics.

[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0040] Example 1

[0041] This embodiment provides a method for preparing a seawater degradation membrane, comprising the following steps:

[0042] S1: First, 20 parts by weight of corn starch and 0.1 parts by weight of stearic acid were added to a high-speed mixer, and mixed at a speed of 200 rpm for 2 minutes; then, 5 parts by weight of glycerol were added, and mixed at a speed of 600 rpm for 8 minutes; finally, 0.2 parts by weight of adipic acid and 0.2 parts by weight of citric acid were added, and mixed at a speed of 200 rpm for 1 minute to prepare plasticized corn starch;

[0043] S2: 10 parts by weight of PLGA, 15 parts by weight of PHBH, 10 parts by weight of PPC, 45 parts by weight of PBAT, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch;

[0044] S3: adding the mixed masterbatch prepared in step S2 into a parallel twin-screw extruder, setting the temperatures of zones 1-9 of the twin-screw extruder to 130° C., 180° C., 180° C., 175° C., 170° C., 170° C., 170° C., 170° C., and the die temperature to 170° C., melt blending, air cooling, and pelletizing to prepare seawater-degradable blown film material;

[0045] S4: The film blowing material obtained in step S3 is formed by film blowing using a common high-pressure PE film blowing machine, and the temperatures of zones 1-5 of the film blowing machine are set to 130°C, 180°C, 180°C, 180°C, 180°C, and the die head temperature is 175°C, and finally a low seawater degradation film with a thickness of 40 μm and a width of 600 mm is obtained.

[0046] Example 2

[0047] This embodiment provides a method for preparing a seawater degradation membrane, comprising the following steps:

[0048] S1: First, 20 parts by weight of corn starch and 0.1 parts by weight of polyhydroxy polymer superdispersible modifier JL-G02FX-P were added to a high-speed mixer and mixed at a speed of 200 rpm for 2 minutes; then 5 parts by weight of sorbitol were added and mixed at a speed of 600 rpm for 8 minutes; finally, 0.2 parts by weight of adipic acid and 0.2 parts by weight of citric acid were added and mixed at a speed of 200 rpm for 1 minute to prepare plasticized corn starch;

[0049] S2: 15 parts by weight of PLGA, 20 parts by weight of PHBH, 10 parts by weight of PPC, 35 parts by weight of PBAT, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch;

[0050] S3: adding the mixed masterbatch prepared in step S2 into a parallel twin-screw extruder, setting the temperatures of zones 1-9 of the twin-screw extruder to 130° C., 180° C., 180° C., 175° C., 170° C., 170° C., 170° C., 170° C., and the die temperature to 170° C., melt blending, air cooling, and pelletizing to prepare seawater-degradable blown film material;

[0051] S4: The film blowing material obtained in step S3 is formed by film blowing using a common high-pressure PE film blowing machine, and the temperatures of zones 1-5 of the film blowing machine are set to 130°C, 180°C, 180°C, 180°C, 180°C, and the die head temperature is 175°C, and finally a seawater-degradable film with a thickness of 40 μm and a width of 600 mm is obtained.

[0052] Example 3

[0053] This embodiment provides a method for preparing a seawater degradation membrane, comprising the following steps:

[0054] S1: First, 20 parts by weight of corn starch, 0.05 parts by weight of polyhydroxy polymer superdispersible modifier JL-G02FX-P and 0.05 parts by weight of stearic acid were added to a high-speed mixer, and mixed at a speed of 200 rpm for 2 minutes; then 2 parts by weight of glycerol and 3 parts by weight of sorbitol were added, and mixed at a speed of 600 rpm for 8 minutes; finally, 0.2 parts by weight of adipic acid and 0.2 parts by weight of citric acid were added, and mixed at a speed of 200 rpm for 1 minute to prepare plasticized corn starch;

[0055] S2: 20 parts by weight of PLGA, 25 parts by weight of PHBH, 10 parts by weight of PPC, 25 parts by weight of PBAT, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch;

[0056] S3: adding the mixed masterbatch prepared in step S2 into a parallel twin-screw extruder, setting the temperatures of zones 1-9 of the twin-screw extruder to 130° C., 180° C., 180° C., 175° C., 170° C., 170° C., 170° C., 170° C., and the die temperature to 170° C., melt blending, air cooling, and pelletizing to prepare seawater-degradable blown film material;

[0057] S4: The film blowing material obtained in step S3 is formed by film blowing using a common high-pressure PE film blowing machine, and the temperatures of zones 1-5 of the film blowing machine are set to 130° C., 180° C., 180° C., 180° C., 180° C., and the die head temperature is 175° C.; finally, a seawater-degradable film with a thickness of 40 μm and a width of 600 mm is obtained.

[0058] Comparative Example 1

[0059] This comparative example provides a method for preparing a seawater degradation membrane, comprising the following steps:

[0060] S1: First, 20 parts by weight of corn starch, 0.05 parts by weight of polyhydroxy polymer superdispersible modifier JL-G02FX-P and 0.05 parts by weight of stearic acid were added to a high-speed mixer, and mixed at a speed of 200 rpm for 2 minutes; then 2 parts by weight of glycerol and 3 parts by weight of sorbitol were added, and mixed at a speed of 600 rpm for 8 minutes; finally, 0.2 parts by weight of adipic acid and 0.2 parts by weight of citric acid were added, and mixed at a speed of 200 rpm for 1 minute to prepare plasticized corn starch;

[0061] S2: 30 parts by weight of PLGA, 50 parts by weight of PHBH, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch;

[0062] S3: adding the mixed masterbatch prepared in step S2 into a parallel twin-screw extruder, setting the temperatures of zones 1-9 of the twin-screw extruder to 130° C., 180° C., 180° C., 175° C., 170° C., 170° C., 170° C., 170° C., and the die temperature to 170° C., melt blending, air cooling, and pelletizing to prepare seawater-degradable blown film material;

[0063] S4: The film blowing material obtained in step S3 is formed by film blowing using a common high-pressure PE film blowing machine, and the temperatures of zones 1-5 of the film blowing machine are set to 130° C., 180° C., 180° C., 180° C., 180° C., and the die head temperature is 175° C.; finally, a seawater-degradable film with a thickness of 40 μm and a width of 600 mm is obtained.

[0064] Comparative Example 2

[0065] The difference between this comparative example and Example 3 is that the content of step S2 is as follows:

[0066] 45 parts by weight of PLGA, 10 parts by weight of PPC, 25 parts by weight of PBAT, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch.

[0067] Comparative Example 3

[0068] The difference between this comparative example and Example 3 is that the content of step S2 is as follows:

[0069] 45 parts by weight of PHBH, 10 parts by weight of PPC, 25 parts by weight of PBAT, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch.

[0070] Comparative Example 4

[0071] The difference between this comparative example and Example 3 is that the content of step S2 is as follows:

[0072] 20 parts by weight of PLGA, 25 parts by weight of PHBH, 35 parts by weight of PPC, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch.

[0073] Comparative Example 5

[0074] The difference between this comparative example and Example 3 is that the content of step S2 is as follows:

[0075] 20 parts by weight of PLGA, 25 parts by weight of PHBH, 35 parts by weight of PBAT, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch.

[0076] Comparative Example 6

[0077] The difference between this comparative example and Example 3 is that the content of step S2 is as follows:

[0078] 20 parts by weight of polylactic acid PLA, 25 parts by weight of PHBH, 10 parts by weight of PPC, 25 parts by weight of PBAT, 0.2 parts by weight of MH and 0.3 parts by weight of white oil were added to a mixer with a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch.

[0079] Comparative Example 7

[0080] The difference between this comparative example and Example 3 is that the content of step S2 is as follows:

[0081] 20 parts by weight of PLGA, 25 parts by weight of PHBH, 10 parts by weight of PPC, 25 parts by weight of PBAT, 0.2 parts by weight of hydroquinone dihydroxyethyl ether and 0.3 parts by weight of white oil were added to a mixer at a fixed speed of 80 rpm and mixed for 30 seconds; then 2 parts by weight of 2504, 0.1 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168, mixed for 30 seconds; finally, the plasticized corn starch prepared in step S1 was added, mixed for 1 minute, and stirred evenly to prepare a mixed masterbatch.

[0082] Comparative Example 8

[0083] The difference between this comparative example and Example 3 is that the content of step S1 is as follows:

[0084] First, 20 parts by weight of corn starch, 0.05 parts by weight of a polyhydroxy polymer superdispersible modifier JL-G02FX-P and 0.05 parts by weight of stearic acid were added to a high-speed mixer and mixed at a speed of 200 rpm for 2 minutes; then 2 parts by weight of glycerol and 3 parts by weight of sorbitol were added and mixed at a speed of 600 rpm for 8 minutes; finally, 0.4 parts by weight of adipic acid were added and mixed at a speed of 200 rpm for 1 minute to prepare plasticized modified corn starch.

[0085] Comparative Example 9

[0086] The difference between this comparative example and Example 3 is that the content of step S1 is as follows:

[0087] First, 20 parts by weight of corn starch, 0.05 parts by weight of a polyhydroxy polymer superdispersible modifier JL-G02FX-P and 0.05 parts by weight of stearic acid were added to a high-speed mixer and mixed at a speed of 200 rpm for 2 minutes; then 2 parts by weight of glycerol and 3 parts by weight of sorbitol were added and mixed at a speed of 600 rpm for 8 minutes; finally, 0.4 parts by weight of citric acid was added and mixed at a speed of 200 rpm for 1 minute to prepare plasticized corn starch.

[0088] Comparative Example 10

[0089] Low-density polyethylene (FB 3000 from LG Company) was blown through a common PE film blowing machine, and the temperature of each zone of the film blowing machine was 145° C. The film thickness was 40 μm and the width was 600 mm.

[0090] The physical and mechanical properties (including tensile strength, elongation at break and heat sealing strength) of the seawater degradable membranes prepared in the above embodiments and comparative examples were tested. The physical and mechanical properties were tested on a universal tensile testing machine (CMT-4304, Shenzhen Xinsansi Co., Ltd.), where the tensile strength and elongation at break were tested in accordance with GB / T1040.3-2006 at a test rate of 250 mm / min, and the heat sealing strength was tested in accordance with QB / T2358-1998 at a test rate of 300 mm / min.

[0091] The test results are shown in Table 1.

[0092] Table 1

[0093]

[0094]

[0095] It can be seen from the data in the above table that the seawater degradable film provided by the present invention has significantly superior transverse and longitudinal tensile strength compared with the traditional PE film, and the elongation at break and the heat sealing strength are basically equivalent, and the mechanical properties can meet the normal use requirements; Compared with Example 3, Comparative Example 1 does not add PPC and PBAT. By comparing the data of the two, it can be seen that the addition of biodegradable materials PPC and PBAT can significantly improve the transverse and longitudinal elongation at break and the heat sealing strength of the prepared film, but will cause a decrease in the transverse and longitudinal tensile strength; Compared with Example 3, Comparative Example 2 does not add PHBH. The transverse and longitudinal tensile strength of the film provided by Comparative Example 2 is increased, but the transverse and longitudinal elongation at break is reduced, and the heat sealing strength is also reduced; Compared with Example 3, Comparative Example 3 does not add PLG A. Although the transverse and longitudinal elongation at break and the heat sealing strength of the film provided in Comparative Example 3 increased slightly, the transverse and longitudinal tensile strength decreased; Compared with Example 3, Comparative Example 4 did not add PBAT, and the heat sealing strength of the film provided in Comparative Example 4 increased, but the transverse and longitudinal tensile strength and elongation at break decreased; Compared with Example 3, Comparative Example 5 did not add PPC, and the transverse and longitudinal tensile strength and fracture productivity of the film provided in Comparative Example 5 increased, but the heat sealing strength decreased; Compared with Example 3, Comparative Example 6 replaced PLGA with PLA, and the transverse and longitudinal fracture productivity of the film provided in Comparative Example 6 increased significantly, and the heat sealing strength was also better, but the transverse and longitudinal tensile strength decreased significantly; Compared with Example 3, Comparative Example 7 replaced hydroquinone dihydroxyethyl ether with MH, the transverse and longitudinal tensile strength and elongation at break of the film provided by Comparative Example 7 are significantly reduced, and the heat sealing strength is also reduced; Compared with Example 3, Comparative Example 8 does not add citric acid during the preparation of the plasticized modified corn starch, and the transverse and longitudinal tensile strength, transverse and longitudinal fracture productivity and heat sealing strength of the film provided by Comparative Example 8 do not show significant changes; Compared with Example 3, Comparative Example 9 does not add adipic acid during the preparation of the plasticized modified corn starch, and the transverse and longitudinal tensile strength, transverse and longitudinal fracture productivity and heat sealing strength of the film provided by Comparative Example 9 do not show significant changes.

[0096] The seawater degradation performance and shelf life of the seawater degradable films prepared in the above embodiments and comparative examples were tested. The test of seawater degradation performance was carried out by weight loss method. The film samples were placed in a seawater tank (taken from the Yellow Sea near Qingdao). The seawater was replaced once a week. The test time was 3 months. The samples were sampled every 15 days. After the samples were taken out, they were dried to constant weight and weighed. The test results are shown in Table 2 for details. The shelf life test was carried out in a constant temperature and humidity laboratory (temperature 25°C, humidity 50% RH). The test period was 10 months. Samples were taken from 5 types of films every 2 months to test the changes in their transverse tensile strength (see above for the test method). The test results are shown in Table 3 for details.

[0097] Table 2

[0098]

[0099]

[0100] Note: The part marked with "*" indicates that the test film begins to fragment.

[0101] It can be seen from the data in Table 2 that the films prepared in Examples 1-3 of the present invention have significant seawater degradation characteristics, and the weight loss rate of seawater degradation can reach more than 40% within 3 months. As the proportion of PBAT and PPC in the formulation system increases, the speed and degree of seawater degradation of the film are significantly reduced. Compared with Example 3, Comparative Example 2 does not add PHBH. When the seawater degradation time of the film provided by Comparative Example 2 is the same, the weight loss rate is slightly lower; Compared with Example 3, Comparative Example 3 does not add PLGA. When the seawater degradation time of the film provided by Comparative Example 3 is the same, the weight loss rate is slightly higher; Compared with Example 3, Comparative Example 4 does not add PBAT. When the seawater degradation time of the film provided by Comparative Example 4 is the same, the weight loss rate does not change significantly; Compared with Example 3, Comparative Example 5 does not add PPC. When the seawater degradation time of the film provided by Comparative Example 5 is the same, the weight loss rate does not change significantly; Compared with Example 3, Comparative Example 6 replaces PLGA with PLA. When the seawater degradation time of the film provided by Comparative Example 6 is the same, the weight loss rate is significantly reduced; Compared with Example 3, Comparative Example 7 replaces hydroquinone dihydroxyethyl ether with hydroquinone dihydroxyethyl ether. MH, when the seawater degradation time of the film provided in Comparative Example 7 is the same, the weight loss rate has no obvious change; when Comparative Example 8 is compared with Example 3, citric acid is not added during the preparation of the plasticized modified corn starch, and when the seawater degradation time of the film provided in Comparative Example 8 is the same, the weight loss rate has no obvious change; when Comparative Example 9 is compared with Example 3, adipic acid is not added during the preparation of the plasticized modified corn starch, and when the seawater degradation time of the film provided in Comparative Example 9 is the same, the weight loss rate has no obvious change; the traditional PE film was immersed in seawater for 3 months without obvious degradation and weight loss.

[0102] Table 3

[0103]

[0104]

[0105] It can be seen from the data in Table 3 that with the extension of time, the transverse tensile strength of the films prepared in Examples 1 to 3 and Comparative Example 1 shows a downward trend, wherein the films prepared in Examples 1 to 3 still have certain mechanical properties after 10 months, while the film prepared in Comparative Example 1 has completely lost its mechanical properties after 6 months and cannot meet the use requirements; Compared with Example 3, Comparative Example 2 does not add PHBH, and the transverse tensile strength of the film provided by Comparative Example 2 decreases faster, indicating that its degradation rate is faster and the shelf life is shorter, which is difficult to meet the use requirements; Compared with Example 3, Comparative Example 3 does not add PLGA, and the transverse tensile strength of the film provided by Comparative Example 3 decreases faster. Compared with Example 3, Comparative Example 4 does not add PBAT, and the speed of reduction of the transverse tensile strength of the film provided by Comparative Example 4 does not change significantly, and the shelf life of the prepared film is equivalent to that of Example 3; Compared with Example 3, Comparative Example 5 does not add PPC, and the speed of reduction of the transverse tensile strength of the film provided by Comparative Example 5 does not change significantly, and the shelf life of the prepared film is equivalent to that of Example 3; Compared with Example 3, Comparative Example 6 replaces PLGA with PLA, and the speed of reduction of the transverse tensile strength of the film provided by Comparative Example 6 is significantly slowed down, and the shelf life is significantly extended; Compared with Example 3, Comparative Example 7 replaces hydroquinone dihydroxyethyl ether with hydroquinone dihydroxyethyl ether. MH, the transverse tensile strength of the film provided by Comparative Example 7 decreases faster, indicating that its degradation rate is faster, the shelf life is shorter, and it is difficult to meet the use requirements; Compared with Example 3, Comparative Example 8 does not add citric acid during the preparation of the plasticized modified corn starch, and the transverse tensile strength of the film provided by Comparative Example 8 decreases faster, indicating that its degradation rate is faster, the shelf life is shorter, and it is difficult to meet the use requirements; Compared with Example 3, Comparative Example 9 does not add adipic acid during the preparation of the plasticized modified corn starch, and the transverse tensile strength of the film provided by Comparative Example 9 decreases faster, indicating that its degradation rate is faster, the shelf life is shorter, and it is difficult to meet the use requirements; and the PE film prepared in Comparative Example 10 did not show obvious decline in mechanical properties within the 10-month test period.

[0106] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A seawater-degradable film, It is characterized in that According to parts by weight, it includes the following components: 10-20 parts of polylactic acid-glycolic acid copolymer; 3-hydroxybutyrate-co-3-hydroxyhexanoate 15-25 parts; 20 parts corn starch; 10 parts of polypropylene carbonate; Polybutylene adipate / terephthalate 25-45 parts; 5 parts of plasticizer; Adipic acid 0.2 parts; 0.2 parts of citric acid; 0.1 part of starch treatment agent; 0.2 parts of organic peroxide; 2 parts of ethylene-vinyl acetate copolymer; 0.3 parts of antioxidant; 0.3 parts of white oil; The molecular weight M of the polylactic acid-glycolic acid copolymer W ≥60000, the mass content of GA in the molecular structure unit is ≥80%, the melt flow rate MFR under the temperature of 190℃ and the pressure of 2.16kg is ≤7g / 10min, and the melting point is ≤175℃.

2. The seawater degradable film according to claim 1, It is characterized in that The molecular weight M of the 3-hydroxybutyrate-co-3-hydroxyhexanoate W ≥50000, at 165℃, melt flow rate MFR ≤5g / 10min under 5kg pressure, melting point ≤150℃.

3. The seawater degradable film according to claim 1, It is characterized in that The plasticizer is selected from at least one of glycerol and sorbitol.

4. The seawater degradable film according to claim 1, It is characterized in that The starch treating agent is selected from at least one of stearic acid and a polyhydroxy polymer super-dispersible modifier.

5. The seawater degradable film according to claim 1, It is characterized in that The antioxidant is a mixture of the antioxidant 1010 and the antioxidant 168, and the mass ratio of the antioxidant 1010 to the antioxidant 168 is 1:

2.

6. A method for preparing a seawater-degradable film according to any one of claims 1 to 5, It is characterized in that The steps include: S1: According to the formula amount, corn starch and starch treatment agent are added into a high-speed mixer, and mixed at a speed of 200 rpm; then a plasticizer is added, and mixed at a speed of 600 rpm; finally adipic acid and citric acid are added, and mixed at a speed of 200 rpm to prepare plasticized corn starch; S2: According to the formula, polylactic acid-glycolic acid copolymer, 3-hydroxybutyrate-co-3-hydroxycaproate, polypropylene carbonate, polybutylene adipate / terephthalate, organic peroxide and white oil are added to a mixer with a fixed speed of 80 rpm and mixed; then ethylene-vinyl acetate copolymer and antioxidant are added and mixed; finally, the plasticized corn starch is added, mixed, and stirred evenly to prepare a mixed masterbatch; S3: adding the mixed masterbatch into a parallel twin-screw extruder, melt blending and air-cooling pelletizing to prepare a seawater-degradable blown film material; S4: forming the seawater-degradable film-blowing material by film blowing to obtain a seawater-degradable film.

7. The method for preparing the seawater-degradable film according to claim 6, It is characterized in that In step S3, the temperatures in zones 1-9 of the twin screw extruder are set to 130°C, 180°C, 180°C, 180°C, 175°C, 170°C, 170°C, 170°C, and the die temperature is 170°C; in step S4, the temperatures in zones 1-5 of the film blowing machine are set to 130°C, 180°C, 180°C, 180°C, and the die temperature is 175°C.

Citation Information

Patent Citations

  • Seawater degradation material with adjustable use cycle and degradation cycle and preparation method of seawater degradation material

    CN108624020A

  • Seawater degradable furandicarboxylic acid glycol copolyester and preparation method thereof

    CN113121803A

  • Seawater degradable butanediol succinate copolyester and preparation method thereof

    CN113307959A

  • Controlled degradation type full-biodegrade agricultural mulching film

    CN104072953A

  • Polyester modified material, film product thereof and preparation method of film product

    CN107304285A