A copper-chromium alloy and its preparation method and application
By controlling the chemical composition in copper-chromium alloy and adopting composite heat treatment technology, the problem of difficult to replace the C18150 and C18400 copper alloy materials in the prior art is solved, and a copper-chromium alloy with excellent comprehensive performance is prepared, which is suitable for high-performance electronic devices.
Patent Information
- Application Number
- CN202310404943.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
It is difficult to develop new copper alloy materials that can replace the C18150 and C18400 copper alloy materials, especially when meeting the high performance requirements in the 5G communications, transportation and consumer electronics fields.
Copper-chromium alloy is used, with chemical compositions of Cr 0.4-1.2%, Zr 0.02-0.15%, Fe 0.02-0.25%, P 0.02-0.15%, and the balance is copper and inevitable impurities. It is prepared by composite heat treatment technology, including uniformity. Steps such as systolic annealing, hot rolling, solid solution treatment, cold rolling and aging treatment.
The prepared copper-chromium alloy has medium strength, medium elongation, high hardness, high conductivity and high bending properties. It has excellent comprehensive performance and can replace C18150 and C18400 copper alloy materials. It is suitable for Type-C, automotive connectors or leads. Framework and other electronic devices.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper alloy materials, and in particular to a copper-chromium alloy and a preparation method and application thereof. Background Art
[0002] As an important component responsible for signal and current transmission in circuit units, connectors are widely used in 5G communications, transportation, consumer electronics and other fields. In recent years, with the construction of 5G network communication equipment, the explosive growth of new energy vehicles, and the popularization of the Internet of Things and AI, wireless base stations, large-capacity server power supplies, DC charging piles, etc. used in communication equipment and new energy vehicles are developing in the direction of miniaturization, high current and high voltage. Connectors used in this environment need to meet good forming properties, mechanical properties, electrical properties and excellent thermal stability.
[0003] Cu-Cr alloys are widely used in the fields of machinery manufacturing, integrated circuits and contact wires due to their advantages of high strength, high electrical conductivity, high thermal conductivity and wear resistance. In recent years, foreign companies such as KME, Olin and Furukawa have developed a series of Cu-Cr alloys, such as C18150 and C18400. These alloys not only meet the requirements of mechanical and electrical properties, but also have excellent thermal stability and forming properties. They are the most ideal copper alloy materials for connectors in the context of high current and high voltage applications. For example, the composition of the C18400 alloy is, by mass content, 0.4-1.2% chromium, 0.2-0.7% zinc, 0-0.15% iron, 0-0.1% silicon, 0-0.05% phosphorus, 0-0.05% lithium, 0-0.005% arsenic, 0-0.005% calcium, and the balance is copper and unavoidable impurities. The strength of the C18400 alloy is 400-560 MPa, and the conductivity is ≥80% IACS; the composition of the C18150 alloy is 0.5-1.5% chromium, 0.05-0.25% zirconium, and the balance is copper and unavoidable impurities. The strength of the C18150 alloy is 450-550 MPa, and the conductivity is ≥80% IACS.
[0004] In order to further accelerate the development of my country in the fields of 5G communications, transportation, and consumer electronics, the development of new copper alloy materials that can replace C18150 and C18400 is a technical problem that needs to be solved urgently. Summary of the invention
[0005] The purpose of the present invention is to provide a copper-chromium alloy and a preparation method and application thereof. The copper-chromium alloy provided by the present invention has the characteristics of medium strength, medium elongation, high hardness, high conductivity and high bendability, excellent comprehensive performance and strong application value.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a copper-chromium alloy, which comprises the following chemical components by mass content:
[0008] Cr 0.4~1.2%, Zr 0.02~0.15%, Fe 0.02~0.25%, P 0.02~0.15%, and the balance is copper and inevitable impurities.
[0009] Preferably, the following chemical components are included:
[0010] Cr 0.6~1.0%, Zr 0.04~0.12%, Fe 0.06~0.20%, P 0.05~0.13%, and the balance is copper and inevitable impurities.
[0011] Preferably, the following chemical components are included:
[0012] Cr 0.7~0.8%, Zr 0.06~0.10%, Fe 0.10~0.15%, P 0.08~0.10%, and the balance is copper and inevitable impurities.
[0013] The present invention provides a method for preparing the copper-chromium alloy described in the above technical solution, comprising the following steps:
[0014] According to the chemical composition of the copper-chromium alloy described in the above technical solution, the raw materials are prepared, smelted and cast to obtain an ingot;
[0015] The ingot is sequentially subjected to homogenization annealing, hot rolling, solution treatment, first cold rolling, aging treatment, second cold rolling and low-temperature annealing to obtain a copper-chromium alloy.
[0016] Preferably, the homogenization annealing temperature is 850-900° C., and the holding time is 6-16 hours.
[0017] Preferably, the hot rolling temperature is 900-950° C., the holding time is 1-3 hours, and the total deformation of the hot rolling is 70-95%.
[0018] Preferably, the temperature of the solution treatment is 950-1000° C., and the holding time is 0.2-2 h.
[0019] Preferably, the total deformation of the first cold rolling is 40-60%; the temperature of the aging treatment is 460-540° C., and the holding time is 3-5 hours.
[0020] Preferably, the total deformation of the second cold rolling is 30-50%; the temperature of the low-temperature annealing is 350-450° C., and the holding time is 2-4 hours.
[0021] The present invention provides the application of the copper-chromium alloy described in the above technical solution or the copper-chromium alloy prepared by the preparation method described in the above technical solution in Type-C, automotive connectors or lead frames.
[0022] The present invention provides a copper-chromium alloy, which comprises the following chemical components by mass content: Cr0.4-1.2%, Zr 0.02-0.15%, Fe 0.02-0.25%, P 0.02-0.15%, and the balance is copper and inevitable impurities. The copper-chromium alloy provided by the present invention strictly limits the content of alloying elements, so that the copper-chromium alloy has the characteristics of medium strength, medium elongation, high hardness, high conductivity and high bendability, and also has the characteristics of high purity and low alloying, and has relatively excellent or even higher comprehensive performance than foreign patented alloys, and has strong application value. The results of the embodiment show that the copper-chromium alloy provided by the present invention has the following properties: tensile strength of 480-650MPa, hardness of 150-200HV, elongation ≥4%, conductivity ≥85-90%IACS, and 180° bending R / t of 1.0-1.5.
[0023] The present invention provides a method for preparing the copper-chromium alloy, comprising the following steps: according to the chemical composition of the copper-chromium alloy, preparing raw materials and then smelting and casting to obtain an ingot; the ingot is subjected to homogenization annealing, hot rolling, solution treatment, first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy. The present invention performs a composite heat treatment on the ingot, and the resulting copper-chromium alloy has the characteristics of medium strength, medium elongation, high hardness, high conductivity and high bendability, and can be processed into copper-chromium alloy plates and strips according to actual needs, and is widely used in the manufacture of electronic devices such as Type-C, automotive connectors or lead frames. DETAILED DESCRIPTION
[0024] The present invention provides a copper-chromium alloy, which comprises the following chemical components by mass content:
[0025] Cr 0.4~1.2%, Zr 0.02~0.15%, Fe 0.02~0.25%, P 0.02~0.15%, and the balance is copper and inevitable impurities.
[0026] According to the mass content, the chemical composition of the copper-chromium alloy in the present invention includes Cr 0.4-1.2%, preferably 0.6-1.0%, and more preferably 0.7-0.8%. In the present invention, the eutectic temperature of the copper-chromium binary alloy is 1072°C, at which the maximum solubility of chromium in copper is 0.65%. As the temperature decreases, the solid solubility of chromium drops sharply, and the alloy precipitates a chromium single-substance nanoparticle phase during aging treatment after solid solution, which significantly enhances the strength of the alloy, and the chromium atoms have little effect on the electrical conductivity of copper, so the copper-chromium alloy can also retain a relatively high electrical conductivity. In addition, the addition of chromium can also significantly increase the recrystallization temperature of copper, thereby improving its thermal stability. When the chromium content is less than 0.4%, the solid solution and aging strengthening effects of the alloy are weak, resulting in a relatively low strength of the alloy. After solution treatment, the chromium atoms in the alloy are dissolved in the copper matrix, but because the content is lower than the maximum solubility, the solid solution strengthening effect of the alloy fails to reach the maximum; after aging treatment, the chromium atoms dissolved in the matrix are precipitated in the form of chromium element, but the precipitated phase content is small, resulting in the alloy's aging strengthening effect is not obvious enough, which ultimately affects the alloy's mechanical properties. When the chromium content is higher than 1.2%, coarse chromium element will precipitate during the solidification process of the alloy, and the chromium element cannot be dissolved back in the subsequent heat treatment. The coarse chromium element has a weak contribution to strength and will reduce the electrical conductivity and bending performance of the alloy. The alloy is prone to produce microcracks near the coarse chromium element during deformation. Therefore, the present invention controls the content of chromium element to 0.4-1.2%, which is conducive to ensuring that the copper-chromium alloy has excellent comprehensive performance.
[0027] According to the mass content, the chemical composition of the copper-chromium alloy in the present invention includes Zr 0.02-0.15%, preferably 0.04-0.12%, more preferably 0.06-0.10%, and further preferably 0.07-0.08%. In the present invention, after adding zirconium to the copper-chromium alloy, zirconium and chromium will interact with each other, the precipitation behavior of chromium in the copper matrix will be affected, the zirconium will be enriched around the chromium phase, and the chromium precipitation phase will be refined by inhibiting the relative growth of chromium, and its precipitation phase can be closer to spherical; the zirconium element will also generate a variety of copper-zirconium precipitation phases with the copper element, enhancing the precipitation strengthening effect of the alloy; in addition, the addition of zirconium can also improve the grain boundary strength of the alloy, thereby improving the strength of the alloy.
[0028] According to the mass content, the chemical composition of the copper-chromium alloy in the present invention includes Fe 0.02-0.25%, preferably 0.06-0.20%, more preferably 0.08-0.15%, and further preferably 0.10-0.12%. In the present invention, at 1050°C, the solubility of iron in copper can reach 3.5%, while the solubility at 635°C drops to 0.15%. Adding iron elements to copper alloys can play a beneficial role in refining copper grains, delaying the recrystallization process of copper, and improving its strength and hardness, because iron atoms will be dissolved in the copper matrix and play a role of solid solution strengthening. The iron atoms dissolved in the copper matrix will cause lattice distortion of the copper matrix, scattering the transmission of electrons, and reducing the electrical conductivity of the alloy. Therefore, the present invention controls the addition amount of iron elements to no more than 0.25%, which is conducive to avoiding the problem that the electrical conductivity of the copper-chromium alloy is greatly reduced due to its excessive content, so that the copper-chromium alloy has excellent comprehensive properties.
[0029] According to the mass content, the chemical composition of the copper-chromium alloy in the present invention includes P 0.02-0.15%, preferably 0.05-0.13%, and more preferably 0.08-0.10%. In the present invention, adding phosphorus to the copper alloy can purify the oxygen content in the melt. By eliminating the oxygen in the alloy, the impurity content in the alloy can be effectively reduced, and the bending performance of the alloy can be improved. Phosphorus can generate a large number of inclusion particles, which prevents the movement of subgrain boundaries, inhibits grain growth, and refines grains. And phosphorus atoms will be distributed on the interface between the precipitated phase and the matrix, hindering the migration of the interface. The above effects can all improve the strength of the alloy. When the phosphorus content is higher than 0.15%, a large number of coarse inclusions will be formed on the grain boundaries, resulting in reduced plasticity and bending performance of the alloy. The present invention controls the addition amount of phosphorus to no more than 0.15%, so that the copper-chromium alloy has excellent comprehensive properties.
[0030] The chemical composition of the copper-chromium alloy in the present invention includes the balance of copper and inevitable impurities by mass content. In the present invention, the total mass content of the inevitable impurities is preferably <0.01%.
[0031] The chemical composition of the copper-chromium alloy in the present invention may be any one of the following:
[0032] Cr 0.40%, Zr 0.02%, Fe 0.02%, P 0.05%, the balance is copper and inevitable impurities;
[0033] Cr 0.40%, Zr 0.02%, Fe 0.06%, P 0.05%, the balance is copper and inevitable impurities;
[0034] Cr 0.60%, Zr 0.02%, Fe 0.10%, P 0.05%, the balance is copper and inevitable impurities;
[0035] Cr 0.60%, Zr 0.04%, Fe 0.10%, P 0.05%, the balance is copper and inevitable impurities;
[0036] Cr 0.80%, Zr 0.06%, Fe 0.20%, P 0.10%, the balance is copper and inevitable impurities;
[0037] Cr 0.80%, Zr 0.08%, Fe 0.20%, P 0.10%, the balance is copper and inevitable impurities;
[0038] Cr 1.00%, Zr 0.08%, Fe 0.20%, P 0.15%, the balance is copper and unavoidable impurities;
[0039] Cr 1.00%, Zr 0.10%, Fe 0.25%, P 0.15%, the balance is copper and unavoidable impurities;
[0040] Cr 1.20%, Zr 0.12%, Fe 0.25%, P 0.15%, the balance is copper and unavoidable impurities;
[0041] Cr 1.20%, Zr 0.15%, Fe 0.25%, P 0.10%, the balance is copper and inevitable impurities;
[0042] Cr 0.80%, Zr 0.10%, Fe 0.20%, P 0.05%, the balance is copper and inevitable impurities;
[0043] Cr 0.80%, Zr 0.08%, Fe 0.02%, P 0.05%, the balance is copper and inevitable impurities;
[0044] Cr 0.80%, Zr 0.08%, Fe 0.02%, P 0.15%, the balance is copper and inevitable impurities;
[0045] Cr 0.80%, Zr 0.10%, Fe 0.10%, P 0.02%, the balance is copper and inevitable impurities;
[0046] Cr 0.80%, Zr 0.10%, Fe 0.25%, P 0.02%, and the balance is copper and inevitable impurities.
[0047] The present invention provides a method for preparing the copper-chromium alloy described in the above technical solution, comprising the following steps:
[0048] According to the chemical composition of the copper-chromium alloy described in the above technical solution, the raw materials are prepared, smelted and cast to obtain an ingot;
[0049] The ingot is sequentially subjected to homogenization annealing, hot rolling, solution treatment, first cold rolling, aging treatment, second cold rolling and low-temperature annealing to obtain a copper-chromium alloy.
[0050] According to the chemical composition of the copper-chromium alloy, the raw materials are prepared and then smelted and cast to obtain an ingot. In the present invention, the raw materials preferably include electrolytic copper, pure chromium and copper-zirconium master alloy, copper-iron master alloy and copper-phosphorus master alloy. The present invention preferably adopts horizontal continuous casting for smelting and casting. In the present invention, the smelting temperature is preferably 1200-1250°C, specifically 1200°C, 1225°C or 1250°C; the casting temperature is preferably 1170-1220°C, specifically 1170°C, 1195°C or 1220°C. The present invention preferably heats the raw materials to the smelting temperature after the raw materials are prepared, and after the raw materials are completely melted, keep warm for 10-15 minutes, stir thoroughly for 10-30 minutes, and stand for 3-5 minutes before casting. In an embodiment of the present invention, the smelting is preferably carried out in an industrial frequency induction furnace.
[0051] After obtaining the ingot, the present invention performs homogenization annealing on the ingot to obtain a homogenization annealed billet. In the present invention, the temperature of the homogenization annealing is preferably 850-900°C, specifically 850°C, 860°C, 870°C, 875°C, 880°C, 890°C or 900°C; the holding time is preferably 6-16h, more preferably 8-14h, and further preferably 10-12h. The present invention preferably performs homogenization annealing under the above conditions, which can dissolve back some inclusions distributed near the grain boundaries in the alloy, and can make the solute atoms fully diffuse in the matrix, ensuring the uniformity of precipitation of the precipitated phase during the aging treatment.
[0052] After obtaining the homogenized annealed billet, the present invention hot-rolls the homogenized annealed billet to obtain a hot-rolled material. In the present invention, the hot rolling temperature is preferably 900-950°C, specifically 900°C, 910°C, 920°C, 925°C, 930°C, 940°C or 950°C; the holding time is preferably 1-3h, more preferably 1.5-2.5h, and further preferably 2h; the total deformation of the hot rolling is preferably 70-95%, more preferably 72-90%, further preferably 74-85%, and further preferably 75-80%. The present invention preferably performs hot rolling under the above conditions, which can eliminate the cast structure of the alloy and obtain a more uniform structure morphology, which is conducive to obtaining a more uniform structure by solution treatment, and makes the hardness distribution of the final copper-chromium alloy have better uniformity.
[0053] After obtaining the hot-rolled material, the present invention performs a solution treatment on the hot-rolled material to obtain a solution material. In the present invention, the solution treatment is preferably an online solution treatment; the temperature of the solution treatment is preferably 950 to 1000°C, specifically 950°C, 960°C, 970°C, 980°C, 990°C or 1000°C; the holding time is preferably 0.2 to 2h, more preferably 0.5 to 1h. The present invention preferably performs a solution treatment under the above conditions, which can fully dissolve the chromium, iron and phosphorus elements in the alloy, which is conducive to a large amount of uniform precipitation during the aging process, and improves the hardness of the copper-chromium alloy finally obtained.
[0054] After obtaining the solid solution material, the present invention performs a first cold rolling on the solid solution material to obtain a first cold rolled material. In the present invention, the total deformation of the first cold rolling is preferably 40-60%, specifically 40%, 45%, 50%, 55% or 60%. The present invention performs the first cold rolling after the solid solution treatment to eliminate part of the quenching stress, so that the plate shape of the alloy is better, and the deformation will introduce dislocations in the alloy, which increases the driving force for atomic precipitation and provides a rapid atomic diffusion channel, which is beneficial to the rapid precipitation of the precipitated phase during the aging treatment; the present invention preferably performs the first cold rolling under the above conditions, which can introduce dislocations in the alloy, which is beneficial to the rapid and sufficient precipitation of solute atoms during the aging process.
[0055] After obtaining the first cold-rolled material, the present invention performs an aging treatment on the first cold-rolled material to obtain an aging-treated material. In the present invention, the temperature of the aging treatment is preferably 460-540°C, specifically 460°C, 475°C, 490°C, 500°C, 515°C or 540°C; the holding time is preferably 3-5h, specifically 3h, 4h or 5h. The present invention preferably performs an aging treatment under the above conditions, which can cause a large amount of precipitation phase to precipitate, and the precipitation phase can be controlled to a smaller size, which is beneficial to improving the strength, hardness and conductivity of the final copper-chromium alloy.
[0056] After obtaining the aging treated material, the present invention preferably performs a second cold rolling on the aging treated material to obtain a second cold rolled material. In the present invention, the total deformation of the second cold rolling is preferably 30-50%, specifically 30%, 35%, 40%, 45% or 50%. The present invention preferably performs the second cold rolling under the above conditions, which can increase the dislocation density of the copper-chromium alloy, and is beneficial to improving the strength and hardness of the copper-chromium alloy.
[0057] After obtaining the second cold-rolled material, the present invention performs low-temperature annealing on the second cold-rolled material to obtain a copper-chromium alloy. In the present invention, the temperature of the low-temperature annealing is preferably 350-450°C, specifically 350°C, 375°C, 390°C, 400°C, 410°C, 425°C or 450°C; the holding time is preferably 2-4h, specifically 2h, 2.5h, 3h, 3.5h or 4h. In the present invention, the low-temperature annealing is preferably bell-type annealing. The present invention preferably performs low-temperature annealing under the above conditions, which can further fully precipitate the solute atoms dissolved in the matrix, and can simultaneously improve the strength and conductivity of the alloy.
[0058] In the present invention, the copper-chromium alloy is preferably a copper-chromium alloy sheet and strip. The present invention can prepare a copper-chromium alloy sheet and strip with medium strength, medium elongation, high hardness, high conductivity and high bendability according to the above method.
[0059] The present invention provides the application of the copper-chromium alloy described in the above technical solution or the copper-chromium alloy prepared by the preparation method described in the above technical solution in Type-C, automotive connectors or lead frames.
[0060] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0061] Example 1
[0062] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are sequentially added to an industrial frequency induction furnace, and the temperature is raised to 1200° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1170° C. to obtain an ingot.
[0063] The ingot is subjected to homogenization annealing, hot rolling and online solution treatment in sequence to obtain a solution material; wherein the homogenization annealing temperature is 850°C, the holding time is 12h; the hot rolling temperature is 900°C, the holding time is 2h, and the total deformation is 75%; the online solution treatment temperature is 980°C, the holding time is 1h;
[0064] The solid solution material is subjected to a first cold rolling, an aging treatment, a second cold rolling and a low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 40%; the temperature of the aging treatment is 500°C, and the holding time is 4h; the total deformation of the second cold rolling is 30%; the low-temperature annealing is a bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 2h.
[0065] Example 2
[0066] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1225°C. After the raw materials are completely melted, the mixture is kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1195°C to obtain an ingot.
[0067] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 875°C, the holding time is 12h; the hot rolling temperature is 925°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0068] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 40%; the temperature of the aging treatment is 500°C, and the holding time is 5h; the total deformation of the second cold rolling is 30%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 2h.
[0069] Example 3
[0070] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are sequentially added to an industrial frequency induction furnace, and the temperature is raised to 1250° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1195° C. to obtain an ingot.
[0071] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 900°C, the holding time is 12h; the hot rolling temperature is 950°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0072] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 40%; the temperature of the aging treatment is 500°C, and the holding time is 3h; the total deformation of the second cold rolling is 30%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 2h.
[0073] Example 4
[0074] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are sequentially added to an industrial frequency induction furnace, and the temperature is raised to 1200° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1170° C. to obtain an ingot.
[0075] The ingot is subjected to homogenization annealing, hot rolling and online solution treatment in sequence to obtain a solution material; wherein the homogenization annealing temperature is 850°C, the holding time is 12h; the hot rolling temperature is 900°C, the holding time is 4h, and the total deformation is 75%; the online solution treatment temperature is 980°C, the holding time is 1h;
[0076] The solid solution material is subjected to a first cold rolling, an aging treatment, a second cold rolling and a low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 50%; the temperature of the aging treatment is 500°C, and the holding time is 1 hour; the total deformation of the second cold rolling is 40%; the low-temperature annealing is a bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 2 hours.
[0077] Example 5
[0078] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1225°C. After the raw materials are completely melted, the mixture is kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1195°C to obtain an ingot.
[0079] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 875°C, the holding time is 12h; the hot rolling temperature is 925°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0080] The solid solution material is subjected to a first cold rolling, an aging treatment, a second cold rolling and a low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 60%; the temperature of the aging treatment is 500°C, and the holding time is 3 hours; the total deformation of the second cold rolling is 50%; the low-temperature annealing is a bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 2 hours.
[0081] Example 6
[0082] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are sequentially added to an industrial frequency induction furnace, and the temperature is raised to 1200° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1170° C. to obtain an ingot.
[0083] The ingot is subjected to homogenization annealing, hot rolling and online solution treatment in sequence to obtain a solution material; wherein the homogenization annealing temperature is 850°C, the holding time is 12h; the hot rolling temperature is 900°C, the holding time is 2h, and the total deformation is 75%; the online solution treatment temperature is 980°C, the holding time is 1h;
[0084] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 40%; the temperature of the aging treatment is 500°C, and the holding time is 4h; the total deformation of the second cold rolling is 30%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 3h.
[0085] Example 7
[0086] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are sequentially added to an industrial frequency induction furnace, and the temperature is raised to 1200° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1170° C. to obtain an ingot.
[0087] The ingot is subjected to homogenization annealing, hot rolling and online solution treatment in sequence to obtain a solution material; wherein the homogenization annealing temperature is 850°C, the holding time is 12h; the hot rolling temperature is 900°C, the holding time is 2h, and the total deformation is 75%; the online solution treatment temperature is 980°C, the holding time is 1h;
[0088] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 40%; the temperature of the aging treatment is 500°C, and the holding time is 4h; the total deformation of the second cold rolling is 30%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 4h.
[0089] Example 8
[0090] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are sequentially added to an industrial frequency induction furnace, and the temperature is raised to 1200° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1170° C. to obtain an ingot.
[0091] The ingot is subjected to homogenization annealing, hot rolling and online solution treatment in sequence to obtain a solution material; wherein the homogenization annealing temperature is 850°C, the holding time is 12h; the hot rolling temperature is 900°C, the holding time is 2h, and the total deformation is 75%; the online solution treatment temperature is 980°C, the holding time is 1h;
[0092] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 50%; the temperature of the aging treatment is 500°C, and the holding time is 5h; the total deformation of the second cold rolling is 40%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 3h.
[0093] Example 9
[0094] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are sequentially added to an industrial frequency induction furnace, and the temperature is raised to 1200° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1170° C. to obtain an ingot.
[0095] The ingot is subjected to homogenization annealing, hot rolling and online solution treatment in sequence to obtain a solution material; wherein the homogenization annealing temperature is 850°C, the holding time is 12h; the hot rolling temperature is 900°C, the holding time is 2h, and the total deformation is 75%; the online solution treatment temperature is 980°C, the holding time is 1h;
[0096] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 60%; the temperature of the aging treatment is 500°C, and the holding time is 4h; the total deformation of the second cold rolling is 40%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 4h.
[0097] Example 10
[0098] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1225°C. After the raw materials are completely melted, the mixture is kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1195°C to obtain an ingot.
[0099] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 875°C, the holding time is 12h; the hot rolling temperature is 925°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0100] The solid solution material is subjected to a first cold rolling, an aging treatment, a second cold rolling and a low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 50%; the temperature of the aging treatment is 500°C, and the holding time is 4 hours; the total deformation of the second cold rolling is 40%; the low-temperature annealing is a bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 3 hours.
[0101] Embodiment 11
[0102] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1250° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1220° C. to obtain an ingot.
[0103] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 900°C, the holding time is 12h; the hot rolling temperature is 950°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0104] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 60%; the temperature of the aging treatment is 500°C, and the holding time is 4h; the total deformation of the second cold rolling is 40%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 4h.
[0105] Example 12
[0106] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1250° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1220° C. to obtain an ingot.
[0107] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 900°C, the holding time is 12h; the hot rolling temperature is 950°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0108] The solid solution material is subjected to first cold rolling, aging treatment, second cold rolling and low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 60%; the temperature of the aging treatment is 500°C, and the holding time is 4h; the total deformation of the second cold rolling is 40%; the low-temperature annealing is bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 4h.
[0109] Embodiment 13
[0110] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1250° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1220° C. to obtain an ingot.
[0111] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 900°C, the holding time is 12h; the hot rolling temperature is 950°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0112] The solid solution material is subjected to a first cold rolling, an aging treatment, a second cold rolling and a low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 60%; the temperature of the aging treatment is 500°C, and the holding time is 5h; the total deformation of the second cold rolling is 40%; the low-temperature annealing is a bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 4h.
[0113] Embodiment 14
[0114] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1250° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1220° C. to obtain an ingot.
[0115] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 900°C, the holding time is 12h; the hot rolling temperature is 950°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0116] The solid solution material is subjected to a first cold rolling, an aging treatment, a second cold rolling and a low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 60%; the temperature of the aging treatment is 500°C, and the holding time is 5h; the total deformation of the second cold rolling is 40%; the low-temperature annealing is a bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 4h.
[0117] Embodiment 15
[0118] After the alloy components are prepared according to Table 1, the alloy is melted and casted by horizontal continuous casting. Specifically, electrolytic copper, copper-zirconium master alloy, copper-iron master alloy, pure chromium and copper-phosphorus master alloy are added to the industrial frequency induction furnace in sequence, and the temperature is raised to 1250° C. until the raw materials are completely melted, and then the raw materials are kept warm for 15 minutes, stirred for 10 minutes, and left to stand for 5 minutes before being taken out of the furnace for casting. The casting temperature is 1220° C. to obtain an ingot.
[0119] The ingot is subjected to homogenization annealing, hot rolling and online solid solution treatment in sequence to obtain a solid solution material; wherein the homogenization annealing temperature is 900°C, the holding time is 12h; the hot rolling temperature is 950°C, the holding time is 2h, and the total deformation is 75%; the online solid solution treatment temperature is 980°C, the holding time is 1h;
[0120] The solid solution material is subjected to a first cold rolling, an aging treatment, a second cold rolling and a low-temperature annealing in sequence to obtain a copper-chromium alloy; wherein the total deformation of the first cold rolling is 60%; the temperature of the aging treatment is 500°C, and the holding time is 2 hours; the total deformation of the second cold rolling is 40%; the low-temperature annealing is a bell-type annealing, the temperature of the low-temperature annealing is 400°C, and the holding time is 4 hours.
[0121] Table 1 Composition formula of copper-chromium alloy in Examples 1 to 15 (wt%)
[0122]
[0123]
[0124] The copper-chromium alloy prepared in Examples 1 to 15 was tested for performance, and the specific results are shown in Table 2, wherein the tensile strength was tested according to the room temperature tensile test method for copper and copper alloy materials in GB / T34505-2017 standard; the hardness was tested according to the Vickers hardness test method for metal materials in GB / T4340-2009 standard; the elongation was tested according to the GB / T34505-2017 method; the conductivity was tested according to the eddy current test method for the conductivity of copper and copper alloys in GBT 32791-2016 standard; and the bending performance was tested according to the "Metallic Material Bending Test Method" (GB / T232-2010). As can be seen from Table 2, the copper-chromium alloy provided by the present invention has medium strength, medium elongation, high hardness, high conductivity and high bendability.
[0125] Table 2 Performance test results of copper-chromium alloys prepared in Examples 1 to 15
[0126]
[0127]
[0128] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A copper-chromium alloy, characterized in that: By mass content, it is composed of the following chemical components: Cr 0.4~1.2%, Zr 0.02~0.15%, Fe 0.02~0.25%, P 0.02~0.15%, the balance is copper and unavoidable impurities; The preparation method of the copper-chromium alloy comprises the following steps: According to the chemical composition of the copper-chromium alloy, the raw materials are prepared, then smelted and cast to obtain an ingot; The ingot is sequentially subjected to homogenization annealing, hot rolling, solution treatment, first cold rolling, aging treatment, second cold rolling and low-temperature annealing to obtain a copper-chromium alloy.
2. The copper-chromium alloy according to claim 1, characterized in that: It is composed of the following chemical components: Cr 0.6~1.0%, Zr 0.04~0.12%, Fe 0.06~0.20%, P 0.05~0.13%, and the balance is copper and inevitable impurities.
3. The copper-chromium alloy according to claim 2, characterized in that: It is composed of the following chemical components: Cr 0.7~0.8%, Zr 0.06~0.10%, Fe 0.10~0.15%, P 0.08~0.10%, the balance is copper and inevitable impurities.
4. The method for preparing the copper-chromium alloy according to any one of claims 1 to 3, characterized in that: The following steps are involved: According to the chemical composition of the copper-chromium alloy according to any one of claims 1 to 3, preparing raw materials, smelting and casting to obtain an ingot; The ingot is sequentially subjected to homogenization annealing, hot rolling, solution treatment, first cold rolling, aging treatment, second cold rolling and low-temperature annealing to obtain a copper-chromium alloy.
5. The preparation method according to claim 4, characterized in that: The temperature of the homogenization annealing is 850-900° C., and the holding time is 6-16 hours.
6. The preparation method according to claim 4, characterized in that: The hot rolling temperature is 900-950° C., and the holding time is 1-3 hours; the total deformation of the hot rolling is 70-95%.
7. The preparation method according to claim 4, characterized in that: The temperature of the solution treatment is 950-1000° C., and the holding time is 0.2-2 hours.
8. The preparation method according to claim 4, characterized in that: The total deformation of the first cold rolling is 40-60%; the temperature of the aging treatment is 460-540° C., and the holding time is 3-5 hours.
9. The preparation method according to claim 4, characterized in that: The total deformation of the second cold rolling is 30-50%; the temperature of the low-temperature annealing is 350-450° C., and the holding time is 2-4 hours.
10. Use of the copper-chromium alloy according to any one of claims 1 to 3 or the copper-chromium alloy prepared by the preparation method according to any one of claims 4 to 9 in automotive connectors or lead frames.
11. Application of the copper-chromium alloy according to any one of claims 1 to 3 or the copper-chromium alloy prepared by the preparation method according to any one of claims 4 to 9 in Type-C.
Citation Information
Patent Citations
Easy machining, high strength and high conductive copper alloy
CN1498978A
Cited By
High-thermal-conductivity copper-chromium alloy and preparation method thereof
CN122235511A