A method for processing durable and fresh cotton Tencel fabric garments

By using wool, liquid ammonia treatment and fiber protective agent cross-linking technology during the processing of cotton tinsil fabrics, the problems of whitening and scratching of the fabric after washing are solved, and new durability and excellent fabrics are achieved. The washing fastness improves the durability and appearance quality of the fabric.

CN116427174BActive Publication Date: 2024-11-26NINGBO YOUNGOR YINGCHENG UNIFORM +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310388768.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-11-26
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

Cotton Tennis fabrics are prone to fibrillation due to mechanical friction during dyeing, finishing or taking, causing the fabric to bleed, pilled, lose its luster, whitening and scratches after washing, which affects the consumption experience and daily care.

Method used

A method of processing of durable new cotton Tennis fabric ready-made garments, including woven fabrics, wool burning, desizing, wool burning, liquid ammonia treatment, soap washing, drying, new shaping, pre-shrinking and garment protection Insert and other processes, fiber protectors are used to cross-link with cotton tinsili fibers to reduce fiber damage, and a stable cross-linking layer is formed through the anti-scaling finishing solution to improve the durability and water washing of the fabric. Fastness.

Benefits of technology

Effectively improve the whitening and scratching problems of cotton tensile fabrics after multiple washings, improve the durability, appearance flatness, dimensional stability and comfortable feel of the fabrics, increase the durability of the washing and the color is not easy to wash and remove.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004175102620000071
    Figure BDA0004175102620000071
  • Figure BDA0004175102620000081
    Figure BDA0004175102620000081
  • Figure BDA0004175102620000091
    Figure BDA0004175102620000091
Patent Text Reader

Abstract

The processing method of the durable and fresh cotton Tencel fabric garment disclosed in the present invention comprises the following steps: yarn-dyed fabric-singeing-de-sizing-singeing-liquid ammonia treatment-soap washing-drying-freshness and shaping-pre-shrinking-freshness and free ironing for garments; the freshness and free ironing process for garments comprises the following steps: pre-washing-drying-spraying free ironing finishing liquid-pre-drying-garment pressing-baking-cooling and moisture regain-freshness and water washing for garments-drying, and the freshness and water washing process for garments comprises the following steps: enzyme washing-clean water washing-deepening washing-color fixing washing. The processing method of the durable and fresh cotton Tencel fabric garment is scientifically and reasonably designed, and the process flow is simple. The fabric garment processed by the method of the present invention has a smooth surface, deep color, and excellent washing fastness, increases the washing durability of the free ironing fabric garment, and the color is not easy to wash off, has excellent durable freshness effect and appearance grade, and at the same time, the fabric garment processed by the method of the present invention has excellent appearance flatness, dimensional stability and comfortable hand feel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile printing and dyeing, and particularly relates to a method for processing durable and fresh cotton Tencel fabric garments. Background Art

[0002] As people's consumption level improves, they have higher demands on the comfort of fabrics. Tencel fabrics are loved by consumers due to their soft feel, excellent moisture absorption and breathability, drape and silk-like luster.

[0003] However, due to Tencel's unique fibril structure, it is easy to fibrillate due to mechanical friction during the dyeing and finishing process or wearing process, resulting in problems such as pilling, loss of luster, etc. During the washing process of household consumers, it is easy for the fabric to turn white and be scratched after washing, causing consumers to have a poor consumer experience and difficulty in daily care.

[0004] Therefore, it is of great significance to develop a cotton Tencel fabric with stable performance and durability. Summary of the invention

[0005] In order to solve the problem of cotton Tencel fabric turning white after washing, the present invention provides a method for processing durable and fresh cotton Tencel fabric garments. The processed fabric garments have excellent durable and fresh effect, appearance grade and washing fastness, can effectively improve the problems of cotton Tencel fabric turning white and scratching after repeated washing, and are durable, and have excellent appearance flatness, dimensional stability and comfortable hand feel.

[0006] The technical solution adopted by the present invention to solve the above technical problems is: a method for processing durable and fresh cotton Tencel fabric garments, comprising the following steps: yarn-dyed fabrics - singeing - desizing - singeing - liquid ammonia treatment - soaping - drying - freshness preservation and shaping - pre-shrinking - freshness preservation and ironing-free garments;

[0007] The garment freshness-free ironing process comprises the following steps: pre-washing - drying - spraying a freshness-free ironing finishing liquid - pre-drying - garment pressing - baking - cooling and regaining - garment freshness-free washing - drying. In the step of spraying a freshness-free ironing finishing liquid, the composition of the freshness-free ironing finishing liquid used is: formaldehyde-free resin WSF 300-400g / L, softener AQ-718 20-50g / L, softener UHS 10-40g / L, strong protective agent PSF 10-40g / L, fiber protective agent S-1 20-50g / L, catalyst MgCl 2 10-30g / L, penetrant A10582-5g / L, wear-resistant agent RPU 10-40g / L; among them, fiber protective agent S-1 can cross-link with cotton Tencel cellulose fibers, which has the function of protecting fibers and reducing damage, and can reduce fiber damage in the process of fresh-keeping and free-ironing finishing of ready-made clothes and the process of fresh-keeping washing;

[0008] In the step of spraying the non-ironing finishing liquid, the non-ironing finishing liquid is evenly sprayed onto the fabric by using a vapor phase spraying process technology, and the atomization spraying time is 60-90 minutes. After the pre-drying step, the moisture content of the fabric is 35-45%; the process conditions of the garment pressing step are: pressing temperature 150-170°C, pressing time 30-60s, so that the garment fabric and the non-ironing finishing liquid form uniform and stable moisture cross-linking after pressing;

[0009] The process conditions of the baking step are: baking temperature 120-140° C., baking time 8-15 min. After baking, the fabric fully reacts with the non-ironing finishing liquid to form a stable cross-linking layer to protect the fabric, greatly reducing fabric damage and color loss during subsequent garment freshness washing.

[0010] The garment freshness-keeping washing process comprises the following steps: enzyme washing - clean water washing - darkening washing - color fixing washing. The enzyme washing step adopts vat washing, and its process conditions are: immersing the fabric in the enzyme solution, the bath ratio is 1:10, the process temperature is 40-50°C, and the process time is 8-15min. The composition of the enzyme solution is: acid enzyme T50N 1-2g / L, glacial acetic acid 0.2-0.5g / L. The enzyme washing can fully wash away the fabric hairiness and the residual materials of the non-ironing finishing liquid, making the washed fabric smoother and reducing the subsequent washing wear of the fabric; the clean water washing step adopts vat washing, and its process conditions are: immersing the fabric in clean water, the bath ratio is 1:10, the process temperature is 30-40°C, and the process time is 3-6min. The clean water washing step adopts vat washing, and its process conditions are: immersing the fabric in darkening agent Y In a solution with a DA concentration of 2-5g / L, a bath ratio of 1:10, a process temperature of 35-45°C, and a process time of 8-15min, the fabric is given excellent softness, brightness, and smoothness through deepening washing, and has excellent color deepening performance; the color fixing washing step adopts a vat washing, and its process conditions are: the fabric is immersed in a solution with a color fixing agent WRF concentration of 2-5g / L, a bath ratio of 1:10, a process temperature of 35-45°C, and a process time of 8-15min. The color fixing washing can improve the washing fastness of the fabric and enhance the wet friction fastness of the fabric;

[0011] Among them, the formaldehyde-free resin WSF is produced by Shijiazhuang Federal Kote Chemical Co., Ltd., the softener AQ-718 is produced by Rihua Chemical (China) Co., Ltd., the softener UHS is produced by Huntsman Textile Dyeing (China) Co., Ltd., the strong protective agent PSF is produced by Huntsman Textile Dyeing (China) Co., Ltd., the fiber protection agent S-1 is produced by Guangzhou Youdao Biotechnology Co., Ltd., the penetrant A1058 is produced by Hangzhou Advanced Industrial Technology Co., Ltd., the wear-resistant agent RPU is produced by Anchroma Chemical (China) Co., Ltd., the acid enzyme T50N is produced by Kangdian Bio Group, the darkening agent YDA is produced by Hangzhou Advanced Industrial Technology Co., Ltd., and the fixing agent WRF is produced by Guangzhou Youdao Biotechnology Co., Ltd.

[0012] The processing method of the present invention comprises the following steps: firstly, singeing process is respectively performed before and after desizing, and the two singeing processes can effectively improve the smoothness of fabric and reduce the friction damage of fabric, especially remove the hairiness formed by the change of fabric tissue during desizing process and the internal movement of tissue during fiber swelling process, increase the surface smoothness of fabric and reduce the friction coefficient of fabric, and then treat the fabric with liquid ammonia after fully removing the surface hairiness, so that the fabric is smooth, has consistent orientation and smooth hand feeling, and reduces the friction damage of fabric; secondly, the fabric is treated with fiber protection agent S-1 to perform freshness preservation and shaping treatment, and the cotton Tencel fabric is protected once after cross-linking; in addition, in the process of making the fabric into a garment without ironing, the fiber protection agent S-1 is added to the ironing-free finishing liquid to perform freshness preservation and ironing-free finishing, and the cotton Tencel fabric is cross-linked with the fiber protection agent and then cross-linked with resin, so that the fabric is protected twice to achieve a double protection effect; finally, the garment is washed in the washing stage to make the fabric darker in color, better in fastness and more washable.

[0013] As preferred, the described freshness-preserving shaping process comprises the following steps: shaping 1—shaping 2—shaping 3—baking—washing—shaping 4, wherein the described shaping step 1 is to perform high-temperature shaping on the fabric after soaping and drying without adding an auxiliary agent, the described shaping step 2 is to add non-ionic penetrant MP-2 to the fabric after shaping 1 for shaping, the described shaping step 3 is to add fiber protective agent S-1 to the fabric after shaping 2 for shaping, the described baking step is to bake the fabric after shaping 3, and the described washing step is to place the baked fabric in a continuous The fabric is washed on an open-width washing machine, and the shaping step 4 is to add non-ionic penetrant MP-2 and a strong protective agent to the washed fabric at the same time to carry out finished product shaping treatment, and the strong protective agent is composed of organic silicon PE-208Z and organic acid AC; wherein, the non-ionic penetrant MP-2 is a product produced by Guangdong Demei Fine Chemical Group Co., Ltd., the organic silicon PE-208Z is a product produced by Zhejiang Rihua Chemical Co., Ltd., and the organic acid AC is a product produced by Huntsman Textile Dyeing (China) Co., Ltd.

[0014] As preferred, the process conditions of the shaping step 1 are: vehicle speed 10-30m / min, temperature 180-200℃; the process conditions of the shaping step 2 are: one dip and one roll, the fabric carries 60-70% of liquid after dipping and rolling, the vehicle speed is 40-60m / min, the temperature is 130-150℃, and the concentration of the non-ionic penetrant MP-2 is 1-5g / L; the process conditions of the shaping step 3 are: one dip and one roll, the fabric carries 60-70% of liquid after dipping and rolling, the vehicle speed is 30-50m / min, the temperature is 150-170℃, and the concentration of the fiber protective agent S-1 is 20-40g / L; the process conditions of the baking step are: one dip and one roll, the fabric carries 60-70% of liquid after dipping and rolling, the vehicle speed is 30-50m / min, the temperature is 150-170℃, and the concentration of the fiber protective agent S-1 is 20-40g / L. The conditions are: vehicle speed 20-40m / min, temperature 150-170℃; the process conditions of the washing step are: the temperatures of the first to sixth tanks on the continuous open-width washing machine are 50-60℃, 60-70℃, 70-80℃, 70-80℃, 50-60℃, 40-50℃ respectively, and the vehicle speed is 30m / min; the process conditions of the four shaping steps are: one dipping and one rolling, the fabric has 60-70% liquid after dipping and rolling, the vehicle speed is 40-60m / min, the temperature is 130-150℃, the concentration of the non-ionic penetrant MP-2 is 1-5g / L, and the composition of the strong protective agent is: organic silicon PE-208Z 10-20g / L, organic acid AC 1-2g / L.

[0015] The function of the above-mentioned shaping step 1 is to provide the fabric with a stable size, reduce the shrinkage of the fabric when it comes into contact with water, and reduce the disordered movement of the fibers in the subsequent shaping stage, providing a basis for the subsequent shaping step of adding an auxiliary agent, so that high temperature shaping is not required for the subsequent shaping of the auxiliary agent, thereby reducing the strong drop of the fabric and being more conducive to the non-ironing processing. The fabric after the shaping step 2 has excellent hydrophilicity and permeability, providing a better bonding environment for the subsequent shaping step 3 of adding the fiber protective agent S-1, and achieving a better absorption rate of the fabric for the fiber protective agent S-1, wherein the fiber protective agent S-1 can reduce the friction between the fabric fibers, reduce the damage to the fabric, and enhance the hydrophilicity and antistatic properties of the fabric. After the fabric is baked after shaping 3, the fiber protective agent S-1 is fully cross-linked with the fabric, which has a better effect of protecting the fibers. The washing step after baking can fully clean the residual auxiliary agent on the fabric and the odor generated after baking. The purpose of the 4 shaping steps is to provide excellent penetration performance and strong protection for the subsequent garment freshness and wrinkle-free process of the fabric, increase the washing rate of the fabric for the wrinkle-free finishing liquid and the uniformity of the combination of the fabric and the wrinkle-free finishing liquid during the garment freshness and wrinkle-free process, and at the same time reduce the strength loss of the fabric during the freshness and wrinkle-free process.

[0016] Preferably, the singeing process before and after desizing has a vehicle speed of 100 m / min and a firing angle of 75 degrees.

[0017] Preferably, the color-dyed fabric process is a process of weaving the dyed colored yarn into fabric according to a specific tissue structure.

[0018] Compared with the prior art, the present invention has the following advantages: the processing method of the durable and fresh cotton Tencel fabric garment of the present invention is scientifically and reasonably designed, and the process flow is simple; the fabric garment processed by the method of the present invention has a smooth surface, deep color, and excellent water washing fastness, increases the washing durability of the wrinkle-free fabric garment, and the color is not easy to wash away, has excellent durable and fresh effect and appearance grade, can effectively improve the whitening and scratches of the cotton Tencel fabric after repeated washing, and has durability; at the same time, the fabric garment processed by the method of the present invention has excellent appearance flatness, dimensional stability and comfortable feel. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in combination with the processing methods of Examples 1-6 of the present invention and the processing methods of conventional Comparative Examples 1-12.

[0020] The composition of the permanent-ironing finishing liquid used in the processing methods of Examples 1-6 is shown in Table 1.

[0021] Table 1: Composition of the permanent iron finishing liquid used in the processing methods of Examples 1-6

[0022] Amount of additives g / L Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Formaldehyde-free resin WSF 300 350 400 300 350 400 Softener AQ-718 20 30 40 30 40 50 Softener UHS 10 20 30 25 30 40 Strong protective agent PSF 15 25 30 15 30 40 Fiber Protective Agent S-1 30 35 40 35 25 45 <![CDATA[Catalyst MgCl 2 > 15 25 30 15 25 30 Penetrant A1058 2 3 3.5 2.5 4 5 Wear-resistant agent RPU 30 25 15 35 30 25

[0023] In each embodiment and comparative example, the formaldehyde-free resin WSF is a product produced by Shijiazhuang Lianbang Kete Chemical Co., Ltd., the softener AQ-718 is a product produced by Rihua Chemical (China) Co., Ltd., the softener UHS is a product produced by Huntsman Textile Dyeing (China) Co., Ltd., the strong protective agent PSF is a product produced by Huntsman Textile Dyeing (China) Co., Ltd., the fiber protective agent S-1 is a product produced by Guangzhou Youdao Biotechnology Co., Ltd., the penetrant A1058 is a product produced by Hangzhou Xianjin Industrial Technology Co., Ltd., the wear-resistant agent RPU is a product produced by Angko Chemical (China) Co., Ltd., and the acid enzyme T50N is a product produced by Kangdien Bio Group. Products, darkening agent YDA is produced by Hangzhou Xianjin Industrial Technology Co., Ltd., fixing agent WRF is produced by Guangzhou Youdao Biotechnology Co., Ltd., non-ionic penetrant MP-2 is produced by Guangdong Demei Fine Chemical Group Co., Ltd., silicone PE-208Z is produced by Zhejiang Rihua Chemical Co., Ltd., organic acid AC is produced by Huntsman Textile Dyeing (China) Co., Ltd., degreasing agent ELF is produced by Tona Trading (Shanghai) Co., Ltd., penetrant CWA is produced by Huntsman Textile Dyeing (China) Co., Ltd., and amylase DMA-260 is produced by Guangdong Demei Fine Chemical Co., Ltd.

[0024] Example 1

[0025] Fabric specification: CTN60 / 2*CPT60 / 2+DLB60 / 2+40D 126*90*53 / 54, 2 / 1 twill, color: black Fabric composition: 82% cotton 16% lyocell 2% spandex

[0026] For the above fabric, the durable freshness-keeping cotton Tencel fabric garment processing method of the present invention is used for processing, and the specific steps are: yarn-dyed fabric - singeing - desizing - singeing - liquid ammonia treatment - soaping - drying - freshness-keeping and shaping - pre-shrinking - garment freshness-keeping and free ironing, and the main process conditions are as follows:

[0027] (1) The process conditions for singeing are: machine speed 100 m / min, ignition angle 75 degrees, and singeing treatment is performed once before and after desizing.

[0028] (2) The desizing process is completed in a continuous desizing machine, which includes 8 water tanks and a steamer, and is composed of the following: the first tank - the second tank - the third tank - the fourth tank - the steamer - the fifth tank - the sixth tank - the seventh tank - the eighth tank - the dryer, wherein the temperatures of the first tank to the fourth tank are 95°C, 95°C, 60°C, and 60°C, respectively, and the temperatures of the fifth tank to the eighth tank are 80°C, 80°C, 80°C, and 80°C, respectively. The desizing finishing liquid is added to the third tank and the fourth tank, and the composition of the desizing finishing liquid is: degreasing agent ELF 5g / L, penetrant CWA 3g / L, and amylase DMA-260 5g / L. The process conditions for desizing are: vehicle speed 70m / min, enzyme treatment temperature 60°C, steamer stacking 50min, steamer stacking temperature 60°C, and washing temperature 80°C.

[0029] (3) The liquid ammonia treatment process uses liquid ammonia mercerization treatment, and the speed of the liquid ammonia mercerization treatment is 40m / min.

[0030] (4) The fabric treated with liquid ammonia was soaped in a continuous open-width washing machine. The temperatures from the first tank to the sixth tank of the continuous open-width washing machine were 85°C, 85°C, 85°C, 85°C, 60°C, and 50°C, respectively. The first tank to the fourth tank were soaping tanks, the fifth tank was a washing tank, and the sixth tank was a pH adjustment washing tank. The process conditions for soaping were: soaping agent 10 g / L, glacial acetic acid 2 g / L, and vehicle speed 40 m / min.

[0031] (5) The process of preserving and shaping includes the following steps: shaping 1—shaping 2—shaping 3—baking—washing—shaping 4, wherein:

[0032] Setting 1: High temperature setting without adding additives, process conditions: speed 20m / min, temperature 190℃;

[0033] Setting 2: Add non-ionic penetrant MP-2 for setting. The process conditions are: one dip and one padding. The fabric has 65% liquid after dipping and padding. The speed is 50m / min, the temperature is 140℃, and the concentration of non-ionic penetrant MP-2 is 3g / L.

[0034] Setting 3: Add fiber protection agent S-1 for setting, the process conditions are: one dip and one pad, the fabric has 65% liquid after dipping and padding, the speed is 40m / min, the temperature is 160℃, and the concentration of fiber protection agent S-1 is 30g / L;

[0035] Baking: process conditions are: speed 30m / min, temperature 160℃;

[0036] Washing: It is done on a continuous open-width washing machine. The process conditions are as follows: the temperatures of the first to sixth tanks on the continuous open-width washing machine are 55°C, 65°C, 75°C, 75°C, 55°C, and 45°C respectively, and the machine speed is 30m / min.

[0037] Setting 4: Add non-ionic penetrant MP-2 and strong protective agent at the same time to set the finished product. The process conditions are: one dip and one rolling, the fabric has 65% liquid after dipping and rolling, the speed is 50m / min, the temperature is 140℃, the concentration of non-ionic penetrant MP-2 is 3g / L, and the composition of the strong protective agent is: organic silicon PE-208Z 15g / L, organic acid AC 1.5g / L.

[0038] (6) Pre-shrinkage process conditions: speed 60m / min, temperature 95℃.

[0039] (7) The garment freshness-preserving and non-ironing process comprises the following steps: pre-washing - drying - spraying non-ironing finishing liquid - pre-drying - garment pressing - baking - cooling and moisture regain - garment freshness-preserving washing - drying, wherein:

[0040] Spraying non-ironing finishing liquid: Use gas phase spraying processing technology to spray the non-ironing finishing liquid evenly onto the fabric, and the atomization spraying time is 75 minutes;

[0041] Pre-drying: After pre-drying, the moisture content of the fabric is 40%;

[0042] Garment pressing: pressing temperature 160℃, pressing time 45s;

[0043] Baking: Baking temperature 135℃, baking time 12min;

[0044] The garment freshness-keeping washing process includes the following steps: enzyme washing - clean water washing - darkening washing - color fixing washing, among which:

[0045] Enzyme washing: adopt tank washing, the process conditions are: soak the fabric in the enzyme solution, the bath ratio is 1:10, the process temperature is 45℃, the process time is 12min, and the composition of the enzyme solution is: acid enzyme T50N 1.5g / L, glacial acetic acid 0.3g / L;

[0046] Clean water washing: adopt tank washing, the process conditions are: soak the fabric in clean water, the bath ratio is 1:10 clean water, the process temperature is 35℃, and the process time is 5min;

[0047] Deepening washing: adopt tank washing, the process conditions are: soak the fabric in a solution with a concentration of 3g / L of the darkening agent YDA, the bath ratio is 1:10, the process temperature is 40℃, and the process time is 12min;

[0048] Color fixing washing: adopt cylinder washing, the process conditions are: soak the fabric in a solution with a color fixing agent WRF concentration of 3g / L, bath ratio 1:10, process temperature 40℃, process time 12min.

[0049] The ready-made non-ironing trousers processed by the method of the present invention have excellent appearance flatness, stable size, comfortable hand feel, and durable washing performance. The main reasons are:

[0050] 1) The cotton Tencel ready-made iron-free trousers processed by the method of the present invention are subjected to two singeing and liquid ammonia treatments in the fabric finishing process to fully remove the fabric hairiness, give the fabric a smooth feel, and reduce the risk of fabric scratches.

[0051] 2) The fiber protective agent added to the cotton Tencel ready-made ironing trousers processed by the method of the present invention cross-links with the fibers during the fabric shaping stage, protects the fabric, reduces the friction between the fibers, and reduces the friction damage of the fabric.

[0052] 3) The cotton Tencel ready-made wrinkle-free trousers processed by the method of the present invention have a fiber protective agent added to the composition of the wrinkle-free finishing liquid. The cotton Tencel fabric is cross-linked with the fiber protective agent and then cross-linked with the resin to achieve a double protection effect. Due to the double cross-linking effect, the processed cotton Tencel fabric has excellent dimensional stability. At the same time, before the resin layer is destroyed, the fabric fibers are not easily damaged. After multiple washings and the resin layer is damaged, the fiber protective agent continues to protect the fibers, which greatly increases the wash resistance of the fabric. In addition, in the garment washing stage, after multiple washings such as enzyme washing, clear water washing, darkening washing, and color fixing washing, the processed ready-made wrinkle-free trousers have a smoother surface, a deeper color, and a better washing fastness, thereby increasing the washing durability of the cotton Tencel fabric and preventing the color from fading away.

[0053] After the ready-made non-ironing trousers processed by the process of Example 1 were washed and dried 20 times, the fabric still had excellent appearance smoothness, stable size, soft and comfortable feel, and the trousers had no whitening or scratches after 20 washes. Therefore, the trousers processed by the process of Example 1 had excellent appearance smoothness, stable size, comfortable feel, and durable washing performance.

[0054] Comparative Example 1: The difference from Example 1 is that after the desizing of the fabric post-finishing process is completed, the second singeing treatment is not performed, the shaping is performed only once, the finished product is high-temperature shaped, no fiber protective agent is added during the shaping process, no fiber protective agent is added to the composition of the non-ironing finishing liquid, and the washing stage does not undergo enzyme washing and deepening washing steps, that is, the fabric processing method in Comparative Example 1 does not undergo the second singeing treatment, the freshness-preserving shaping treatment, and the freshness-preserving non-ironing treatment of the finished garment. The ready-made non-ironing trousers processed by the process of Comparative Example 1 have whitening and scratches after washing and drying 5 times. After washing and drying 20 times, the ready-made non-ironing trousers have whitening and serious scratches, and do not have a durable freshness-preserving effect.

[0055] Comparative Example 2: The difference from Comparative Example 1 is that the trousers processed by the process of Comparative Example 2 are not treated with wrinkle-free treatment. After washing and drying for 5 times, they turn white and have serious scratches. After washing and drying for 20 times, the whitening and scratches are further aggravated, and they do not have the effect of durable newness preservation.

[0056] The relevant properties of the fabrics processed by the processes of Example 1, Comparative Example 1 and Comparative Example 2 were tested according to the following methods: GB / T18863-2002 "Wrinkle-free Textiles" and GB / T 21294-2014 "Test Methods for Physical and Chemical Properties of Clothing". The specific test results are shown in Tables 2 and 3.

[0057] Table 2: Test data of the non-ironing performance of the trousers processed in Example 1, Comparative Example 1 and Comparative Example 2

[0058]

[0059] Table 3: Appearance test data of the trousers processed in Example 1, Comparative Example 1 and Comparative Example 2 after washing

[0060]

[0061] Example 2

[0062] Fabric specifications: CTN60 / 2*CPT60 / 2+DLB60 / 2+40D 126*90*53 / 54, 2 / 1 twill, color: navy blue Fabric composition: 82% cotton 16% lyocell 2% spandex

[0063] The difference from the fabric processing method of Example 1 is that the composition of the non-ironing finishing liquid is different.

[0064] The ready-made non-ironing trousers processed by the process of Example 2 have excellent appearance smoothness, stable size, comfortable hand feel, and durable washing performance.

[0065] Comparative Example 3: The difference from Example 2 is that after the desizing of the fabric post-finishing process is completed, the second singeing treatment is not performed, the shaping is only performed once, the finished product is high-temperature shaped, no fiber protective agent is added during the shaping process, no fiber protective agent is added to the composition of the non-ironing finishing liquid, and the water washing stage does not undergo enzyme washing and deepening washing steps, that is, the fabric processing method in Comparative Example 3 does not undergo the second singeing treatment, does not undergo the freshness-preserving shaping treatment, and does not undergo the freshness-preserving non-ironing treatment of the finished garment. The ready-made non-ironing trousers processed by the process of Comparative Example 3 have whitening and scratches after washing and drying 5 times. After washing and drying 20 times, the ready-made non-ironing trousers have whitening and serious scratches, and do not have a durable freshness-preserving effect.

[0066] Comparative Example 4: The difference from Comparative Example 3 is that the trousers processed by the process of Comparative Example 4 are not treated with wrinkle-free treatment. After washing and drying for 5 times, they turn white and have serious scratches. After washing and drying for 20 times, the whitening and scratches are further aggravated, and they do not have the effect of durable newness preservation.

[0067] The relevant properties of the trousers processed by the process of Example 2, Comparative Example 3 and Comparative Example 4 were tested according to the following methods: GB / T18863-2002 "Wrinkle-free textiles" and GB / T 21294-2014 "Test methods for physical and chemical properties of clothing". The specific test results are shown in Tables 4 and 5.

[0068] Table 4: Test data of the non-ironing performance of the trousers processed in Example 2, Comparative Example 3 and Comparative Example 4

[0069]

[0070] Table 5: Appearance test data of the trousers processed in Example 2, Comparative Example 3 and Comparative Example 4 after washing

[0071]

[0072] Example 3

[0073] Fabric specifications: CTN60 / 2*CPT60 / 2+DLB60 / 2+40D 126*90*53 / 54, 2 / 1 twill, color: dark gray Fabric composition: 82% cotton 16% lyocell 2% spandex

[0074] The difference from the fabric processing method of Example 1 is that the composition of the finishing liquid is different.

[0075] The ready-made non-ironing trousers processed by the process of Example 3 have excellent appearance smoothness, stable size, comfortable hand feel, and durable washing performance.

[0076] Comparative Example 5: The difference from Example 3 is that after the desizing of the fabric post-finishing process is completed, the second singeing treatment is not performed, the shaping is performed only once, the finished product is high-temperature shaped, no fiber protective agent is added during the shaping process, no fiber protective agent is added to the composition of the non-ironing finishing liquid, and the washing stage does not undergo enzyme washing and deepening washing steps, that is, the fabric processing method in Comparative Example 5 does not undergo the second singeing treatment, the freshness-preserving shaping treatment, and the freshness-preserving non-ironing treatment of the finished garment. The ready-made non-ironing trousers processed by the process of Comparative Example 5 have whitening and scratches after washing and drying 5 times. After washing and drying 20 times, the ready-made non-ironing trousers are white and severely scratched, and do not have a durable freshness-preserving effect.

[0077] Comparative Example 6: The difference from Comparative Example 5 is that the trousers processed by the process of Comparative Example 6 are not treated with wrinkle-free treatment. After washing and drying for 5 times, they turn white and have serious scratches. After washing and drying for 20 times, the whitening and scratches are further aggravated, and they do not have the effect of durable newness preservation.

[0078] The relevant properties of Example 3, Comparative Example 5 and Comparative Example 6 were tested according to the following methods: GB / T 18863-2002 "Wrinkle-free Textiles" and GB / T 21294-2014 "Test Methods for Physical and Chemical Properties of Clothing". The specific test results are shown in Tables 6 and 7.

[0079] Table 6: Test data of the non-ironing performance of the trousers processed in Example 3, Comparative Example 5 and Comparative Example 6

[0080]

[0081] Table 7: Appearance test data of the trousers processed in Example 3, Comparative Example 5 and Comparative Example 6 after washing

[0082]

[0083] Example 4

[0084] Fabric specification: 60 / 2*TN108D / 72F+JLB60 / 2+40D 124*90*55 / 56, weave 2 / 1 twill, color: black Fabric composition: 81% cotton 17% lyocell 2% spandex

[0085] The difference between the fabric processing method of Example 1 and that of Example 1 is that the composition of the finishing liquid is different and the fabric is selected differently.

[0086] The ready-made non-iron trousers processed by the process of Example 4 have excellent appearance smoothness, stable size, comfortable hand feel, and durable washing performance.

[0087] Comparative Example 7: The difference from Example 4 is that after the desizing of the fabric post-finishing process is completed, the second singeing treatment is not performed, the shaping is only performed once, the finished product is high-temperature shaped, no fiber protective agent is added during the shaping process, no fiber protective agent is added to the composition of the non-ironing finishing liquid, and the water washing stage does not undergo enzyme washing and deepening washing steps, that is, the fabric processing method in Comparative Example 7 does not undergo the second singeing treatment, the freshness-preserving shaping treatment, and the freshness-preserving non-ironing treatment of the finished garment. The ready-made non-ironing trousers processed by the process of Comparative Example 7 have whitening and scratches after washing and drying 5 times. After washing and drying 20 times, the ready-made non-ironing trousers are white and severely scratched, and do not have a durable freshness-preserving effect.

[0088] Comparative Example 8: The difference from Comparative Example 7 is that the trousers processed by the process of Comparative Example 8, without the ready-made garment wrinkle-free treatment, turned white and had serious scratches after washing and drying for 5 times. The whitening and scratches were further aggravated after washing and drying for 20 times, and the trousers did not have the effect of durable newness preservation.

[0089] The relevant properties of the trousers processed by the process of Example 4, Comparative Example 7 and Comparative Example 8 were tested according to the following methods: GB / T18863-2002 "Wrinkle-free textiles" and GB / T 21294-2014 "Test methods for physical and chemical properties of clothing". The specific test results are shown in Tables 8 to 9.

[0090] Table 8: Test data of the non-ironing performance of the trousers processed in Example 4, Comparative Example 7 and Comparative Example 8

[0091]

[0092] Table 9: Appearance test data of the trousers processed in Example 4, Comparative Example 7 and Comparative Example 8 after washing

[0093]

[0094] Example 5

[0095] Fabric specification: 60 / 2*TN108D / 72F+JLB60 / 2+40D 124*90*55 / 56, weave 2 / 1 twill, color: navy blue Fabric composition: 82% cotton 16% lyocell 2% spandex

[0096] The difference between the fabric processing method of Example 1 and that of Example 1 is that the composition of the finishing liquid is different and the fabric is selected differently.

[0097] The ready-made non-iron trousers processed by the process of Example 5 have excellent appearance smoothness, stable size, comfortable hand feel, and durable washing performance.

[0098] Comparative Example 9: The difference from Example 5 is that after the desizing of the fabric post-finishing process is completed, the second singeing treatment is not performed, the shaping is performed only once, the finished product is high-temperature shaped, no fiber protective agent is added during the shaping process, no fiber protective agent is added to the composition of the non-ironing finishing liquid, and the washing stage does not undergo enzyme washing and deepening washing steps, that is, the fabric processing method in Comparative Example 9 does not undergo the second singeing treatment, the freshness-preserving shaping treatment, and the freshness-preserving non-ironing treatment of the finished garment. The ready-made non-ironing trousers processed by the process of Comparative Example 9 have whitening and scratches after washing and drying 5 times. After washing and drying 20 times, the ready-made non-ironing trousers are white and severely scratched, and do not have a durable freshness-preserving effect.

[0099] Comparative Example 10: The difference from Comparative Example 9 is that the trousers processed by the process of Comparative Example 10 are not treated with wrinkle-free treatment. After washing and drying for 5 times, they turn white and have serious scratches. After washing and drying for 20 times, the whitening and scratches are further aggravated, and they do not have the effect of durable newness preservation.

[0100] The relevant properties of the trousers processed by the process of Example 5, Comparative Example 9 and Comparative Example 10 were tested according to the following methods: GB / T18863-2002 "Wrinkle-free textiles" and GB / T 21294-2014 "Test methods for physical and chemical properties of clothing". The specific test results are shown in Tables 10 and 11.

[0101] Table 10: Test data of the non-ironing performance of the trousers processed in Example 5, Comparative Example 9 and Comparative Example 10

[0102]

[0103] Table 11: Appearance test data of the trousers processed in Example 5, Comparative Example 9 and Comparative Example 10 after washing

[0104]

[0105] Example 6

[0106] Fabric specification: 60 / 2*TN108D / 72F+JLB60 / 2+40D 124*90*55 / 56, 2 / 1 twill, color: dark gray Fabric composition: 82% cotton 16% lyocell 2% spandex

[0107] The difference between the fabric processing method of Example 1 and that of Example 1 is that the composition of the finishing liquid is different and the fabric is selected differently.

[0108] The ready-made non-ironing trousers processed by the process of Example 6 have excellent appearance smoothness, stable size, comfortable hand feel, and durable washing performance.

[0109] Comparative Example 11: The difference from Example 6 is that after the desizing of the fabric post-finishing process is completed, the second singeing treatment is not performed, the shaping is performed only once, the finished product is high-temperature shaped, no fiber protective agent is added during the shaping process, no fiber protective agent is added to the composition of the non-ironing finishing liquid, and the washing stage does not undergo enzyme washing and deepening washing steps, that is, the fabric processing method in Comparative Example 11 does not undergo the second singeing treatment, the freshness-preserving shaping treatment, and the freshness-preserving non-ironing treatment of the finished garment. The ready-made non-ironing trousers processed by the process of Comparative Example 11 have whitening and scratches after washing and drying 5 times. After washing and drying 20 times, the ready-made non-ironing trousers are white and severely scratched, and do not have a durable freshness-preserving effect.

[0110] Comparative Example 12: The difference from Comparative Example 11 is that the trousers processed by the process of Comparative Example 12 are not treated with wrinkle-free treatment. After washing and drying for 5 times, they turn white and have serious scratches. After washing and drying for 20 times, the whitening and scratches are further aggravated, and they do not have the effect of durable newness preservation.

[0111] The relevant properties of the trousers processed by the process of Example 6, Comparative Example 11 and Comparative Example 12 were tested according to the following methods: GB / T18863-2002 "Wrinkle-free textiles" and GB / T 21294-2014 "Test methods for physical and chemical properties of clothing". The specific test results are shown in Tables 12 and 13.

[0112] Table 12: Test data of the non-ironing performance of the trousers processed in Example 6, Comparative Example 11 and Comparative Example 12

[0113]

[0114] Table 13: Appearance test data of the trousers processed in Example 6, Comparative Example 11 and Comparative Example 12 after washing

[0115]

[0116] The above embodiments and comparative examples take trouser fabrics as an example. For shirts, jackets, windbreakers and other clothing categories with cotton Tencel as the main component, after being processed by the processing method of the present invention, they also have excellent appearance smoothness, stable size, comfortable feel and durable washing performance.

Claims

1. A method for processing durable and fresh cotton Tencel fabric garments, characterized in that: It includes the following processes: yarn-dyed fabrics - singeing - desizing - singeing - liquid ammonia treatment - soaping - drying - freshening and shaping - pre-shrinking - freshening and ironing of finished garments; The garment freshness-free ironing process comprises the following steps: pre-washing - drying - spraying a freshness-free ironing finishing liquid - pre-drying - garment pressing - baking - cooling and regaining - garment freshness-free washing - drying. In the step of spraying a freshness-free ironing finishing liquid, the composition of the freshness-free ironing finishing liquid used is: formaldehyde-free resin WSF 300-400g / L, softener AQ-718 20-50g / L, softener UHS 10-40g / L, strong protective agent PSF 10-40g / L, fiber protective agent S-1 20-50g / L, catalyst MgCl2 10-30g / L, penetrant A10582-5g / L, wear-resistant agent RPU 10-40g / L; In the step of spraying the non-ironing finishing liquid, the non-ironing finishing liquid is evenly sprayed onto the fabric by using the gas phase spraying processing technology, the atomization spraying time is 60-90 minutes, and after the pre-drying step, the moisture content of the fabric is 35-45%; the process conditions of the garment pressing step are: pressing temperature 150-170°C, pressing time 30-60s; the process conditions of the baking step are: baking temperature 120-140°C, baking time 8-15min; the garment freshness preservation washing process includes the following steps: enzyme washing - clean water washing - darkening washing - color fixing washing, the enzyme washing step adopts cylinder washing, and its process conditions are: immersing the fabric in the enzyme solution, the bath ratio is 1:10, the process temperature is 40-50°C, the process time is 8-15min, and the composition of the enzyme solution is: acid enzyme enzyme T50N 1-2g / L, glacial acetic acid 0.2-0.5g / L; the clean water washing step adopts vat washing, and its process conditions are: soaking the fabric in clean water, bath ratio 1:10 clean water, process temperature 30-40℃, process time 3-6min; the darkening washing step adopts vat washing, and its process conditions are: soaking the fabric in a solution with a darkening agent YDA concentration of 2-5g / L, bath ratio 1:10, process temperature 35-45℃, process time 8-15min; the color fixing washing step adopts vat washing, and its process conditions are: soaking the fabric in a solution with a color fixing agent WRF concentration of 2-5g / L, bath ratio 1:10, process temperature 35-45℃, process time 8-15min; The described newness-preserving shaping process comprises the following steps: shaping 1—shaping 2—shaping 3—baking—washing—shaping 4, wherein the described shaping step 1 is to perform high-temperature shaping on the fabric after soaping and drying without adding an auxiliary agent, the described shaping step 2 is to add non-ionic penetrant MP-2 to the fabric after shaping 1 for shaping, the described shaping step 3 is to add fiber protective agent S-1 to the fabric after shaping 2 for shaping, the described baking step is to bake the fabric after shaping 3, and the described washing step is to place the baked fabric on a continuous flat The fabric is washed in a washing machine, and the shaping step 4 is to add non-ionic penetrant MP-2 and strong protective agent to the washed fabric at the same time to shape the finished product, and the strong protective agent is composed of organic silicon PE-208Z and organic acid AC; wherein the non-ionic penetrant MP-2 is a product produced by Guangdong Demei Fine Chemical Group Co., Ltd., the organic silicon PE-208Z is a product produced by Zhejiang Rihua Chemical Co., Ltd., and the organic acid AC is a product produced by Huntsman Textile Dyeing (China) Co., Ltd.; The process conditions of the step 1 of setting are: vehicle speed 10-30m / min, temperature 180-200℃; the process conditions of the step 2 of setting are: one dip and one roll, the fabric has 60-70% liquid after dipping and rolling, the vehicle speed is 40-60m / min, the temperature is 130-150℃, and the concentration of the non-ionic penetrant MP-2 is 1-5g / L; the process conditions of the step 3 of setting are: one dip and one roll, the fabric has 60-70% liquid after dipping and rolling, the vehicle speed is 30-50m / min, the temperature is 150-170℃, and the concentration of the fiber protective agent S-1 is 20-40g / L; the process conditions of the baking step are: : speed 20-40m / min, temperature 150-170℃; the process conditions of the washing step are: the temperatures of the first to sixth tanks on the continuous open-width washing machine are 50-60℃, 60-70℃, 70-80℃, 70-80℃, 50-60℃, 40-50℃ respectively, and the speed is 30m / min; the process conditions of the 4 shaping steps are: one dip and one padding, the fabric has 60-70% liquid after dipping and padding, the speed is 40-60m / min, the temperature is 130-150℃, the concentration of non-ionic penetrant MP-2 is 1-5g / L, and the composition of the strong protective agent is: organic silicon PE-208Z 10-20g / L, organic acid AC 1-2g / L; Among them, the formaldehyde-free resin WSF is produced by Shijiazhuang Federal Kote Chemical Co., Ltd., the softener AQ-718 is produced by Rihua Chemical (China) Co., Ltd., the softener UHS is produced by Huntsman Textile Dyeing (China) Co., Ltd., the strong protective agent PSF is produced by Huntsman Textile Dyeing (China) Co., Ltd., the fiber protection agent S-1 is produced by Guangzhou Youdao Biotechnology Co., Ltd., the penetrant A1058 is produced by Hangzhou Advanced Industrial Technology Co., Ltd., the wear-resistant agent RPU is produced by Anchroma Chemical (China) Co., Ltd., the acid enzyme T50N is produced by Kangdian Bio Group, the darkening agent YDA is produced by Hangzhou Advanced Industrial Technology Co., Ltd., and the fixing agent WRF is produced by Guangzhou Youdao Biotechnology Co., Ltd.

2. The method for processing a durable and fresh cotton Tencel fabric garment according to claim 1, characterized in that: The singeing process before and after desizing has a vehicle speed of 100 m / min and a firing angle of 75 degrees.

3. The method for processing a durable and fresh cotton Tencel fabric garment according to claim 1, characterized in that: The process of making the color-dyed fabric is a process of weaving the dyed colored yarn into the fabric according to a specific tissue structure.

Citation Information

Patent Citations

  • Processing method of wash-and-wear shirt containing bast fiber or regenerated cellulose fiber

    CN109577004A

  • Processing method for improving antistatic performance of garment non-ironing trousers fabric