A method for improving the sizing performance of surface starch prepared by bio-enzyme hydrolysis and its application

By wet heat treatment, the ratio of straight chain to branch chain and enzyme action is adjusted, and the surface glue-sizing starch with low viscosity and high stability is prepared, which solves the problem of insufficient performance in preparing surface glue-sized starch by biological enzyme hydrolysis and improves the paper Mechanical properties and printing quality.

CN116427197BActive Publication Date: 2024-11-19ZHEJIANG JINGXING PAPER
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310291308.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-11-19
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

The surface glue starch gel prepared by the existing biological enzyme hydrolysis method is insufficient in the performance, resulting in low surface strength of the paper, poor printing quality, and problems with enzyme activity and storage stability, which limits its application in the papermaking industry.

Method used

The starch is treated with moisture heat, and physical modification is carried out by adjusting the moisture content, temperature and treatment time, adjusting the linear and branched chain ratio of the starch, enhancing the role of starch and enzymes, and preparing low viscosity and high stability surface glue-sizing starch .

Benefits of technology

It significantly improves the mechanical enhancement performance of surface glue starch, reduces viscosity, and enhances stability. It is suitable for industrial production, and solves the problems of poor rheological characteristics and insufficient storage stability of the glue solution in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116427197B_ABST
    Figure CN116427197B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for improving the sizing performance of surface starch prepared by bio-enzyme hydrolysis, comprising the following steps: wet heat treatment of starch: weighing the original starch, adjusting the water content, treatment temperature, treatment time, drying, grinding and sieving of the starch in sequence; preparing starch slurry, adding α-amylase, stirring, heating, and inactivating the enzyme; preparing surface sizing liquid, and surface sizing, drying, and calendering the corrugated base paper. The method of the present invention is based on an environmentally friendly and simple wet heat treatment method to physically modify the original starch. The operation process has low requirements for moisture content, which is conducive to greatly reducing the energy consumption of drying wet heat treated starch, improving production efficiency, and can improve the sizing performance of surface starch prepared by bio-enzyme hydrolysis. The method of the present invention does not add any chemicals in the pretreatment process of starch, and takes into account the green and low-carbon environmental protection concepts while ensuring safety. The prepared surface starch has excellent sizing performance and can be used for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pulping and papermaking, in particular to a method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method and its application. Background Art

[0002] The awareness of protecting forest resources is becoming increasingly prominent, and the high-quality papermaking fiber raw materials needed by my country's pulp and paper industry are scarce. To solve this problem, in addition to vigorously developing fast-growing artificial papermaking forests, the rational use of grass fibers and recycled waste paper are currently particularly effective ways. More than 90% of my country's papermaking raw materials are straw pulp or secondary and multiple fibers, which leads to low surface strength of paper after papermaking, and problems such as hair loss and powder loss during printing, affecting the mechanical properties and printing quality of the paper. Judging from my country's current basic national conditions, for a long time, grass fibers and recycled waste paper will remain an indispensable part of China's papermaking industry, and the requirements for paper mechanical properties and printing quality have also become issues that the industry cannot ignore.

[0003] However, due to the low mechanical strength of paper made from recycled waste paper raw materials, domestic corrugated boxboard paper manufacturers currently use methods to make up for the deficiencies in the mechanical properties of waste paper pulp. Currently, the main methods used are adding inorganic fillers, adding polymers to the pulp, surface sizing, surface dissolution, nanofiber coating, etc. Among them, surface sizing is a more convenient method and is more common in actual production. Starch, as a product with a wide range of sources and relatively friendly prices, plays an indispensable role in surface sizing. Increasing the concentration of starch-based surface sizing liquid can increase the amount of sizing, significantly improve the surface strength of paper, and improve its poor printing quality. However, while increasing the concentration of the sizing liquid, it is also accompanied by an increase in the viscosity of the sizing liquid, which will cause a series of problems during the operation of the paper machine, especially in the deterioration of the rheological properties of the sizing liquid, easy bubbling in the sizing machine, and uneven sizing on the paper surface. Therefore, it has become a new trend to find a product that can take into account the increase in the amount of sizing without increasing the viscosity of the sizing liquid. As a modification method, enzymatic starch hydrolysis uses α-amylase to cut the α-1,4 glycosidic bonds of native starch to obtain a high-solid content, low-viscosity starch sizing solution. However, data show that enzymatic starch sizing solutions with enzyme activity are more likely to breed bacteria and have poor storage stability, which to a certain extent limits the application of enzymatic starch in surface sizing.

[0004] Patent publication number CN111303307A discloses a modified sizing starch, a surface sizing solution, and a preparation method and application thereof. In the method, a prehydrolysis solution and starch are mixed under a pH of 3-6 to obtain material A; material A, a catalyst and an aqueous hydrogen peroxide solution are mixed and kept warm to obtain material B; material B is mixed with a reducing agent to obtain a modified sizing starch. In the method, the raw material of the modified sizing starch uses a prehydrolysis solution to replace part of the starch, which saves costs. The surface sizing solution is applied to paper to effectively improve the water resistance of the paper and reduce the Cobb value of the paper. However, the method requires more raw material ratios in the process, more catalysts are required in the process, and the process is complicated, which is not conducive to actual production. Patent publication number CN115210426A discloses the use of cellulose derivatives and a method for surface sizing, wherein one or more cellulose derivatives are combined and applied to paper surface sizing, and the compressive strength characteristics and moisture resistance obtained by using cellulose ethers provide a wide range of possible end uses and applications, and reduce moisture-related damage to paper, paperboard, etc. in geographical areas with high humidity levels and high temperatures. In addition, the improvement of compressive strength characteristics can make lighter structures possible, thereby making fiber webs such as paperboard a more sustainable packaging option, but the source of cellulose derivatives used in this method is not as extensive as starch, and the price is not suitable for large-scale production by enterprises. The patent publication document with patent publication number CN 111101399A discloses a corn starch surface sizing solution and a preparation method thereof, wherein the method comprises mixing corn starch and amylopectin into a starch slurry; adding a protein inhibitor and an amylase into the starch slurry; and subjecting the starch slurry after the addition to a heating and insulation process to obtain the corn starch surface sizing solution, thereby improving the stability and anti-aging properties of the corn starch sizing solution and making the sizing solution have a lower viscosity and a higher bonding strength. However, the method has problems in controlling the proportion of corn starch and amylopectin, and the addition of the protein inhibitor makes the process complicated, and the addition of the protein inhibitor makes the sizing solution have certain safety hazards.

[0005] It can be seen from this that the existing materials and methods are not sufficient to meet the production needs of the factory. Therefore, under the constraints of carbon emission policies, it is necessary to develop a safe, environmentally friendly and low-cost method to optimize the performance of surface starch sizing prepared by bio-enzyme hydrolysis, and to ensure that the treatment process is clean and easy to operate, so as to ensure environmental safety while taking into account the improvement of the performance of surface starch.

[0006] In view of this, the present invention proposes a method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method. The surface sizing starch is prepared by a biological enzyme hydrolysis method using wet heat treated starch as a raw material. Since wet heat treatment refers to a heat treatment process in which the moisture content of the starch is less than 35% and the temperature is set above the gelatinization temperature of the starch, the wet heat treatment is a physical and environmentally friendly heat treatment process. In addition, the properties of the wet heat treated starch greatly depend on two main factors, namely, the treatment conditions (i.e., moisture content, temperature, and duration) and the type of starch (i.e., the physicochemical properties of the starch). In addition, the wet heat treatment process can also adjust the ratio of straight chain starch to amylopectin in the original starch granules, and the effect of the starch granules and the amylase will be further enhanced, which is beneficial to improving the enzymatic hydrolysis behavior of the starch, thereby reducing the viscosity of the starch slurry while giving the surface sizing starch slurry excellent mechanical reinforcement properties for the paperboard. Summary of the invention

[0007] The purpose of the present invention is to overcome the existing technical shortcomings of the existing bio-enzyme hydrolysis method for preparing surface sizing starch, that is, the low reinforcing performance of the surface sizing starch on paperboard, and to provide a method and application for improving the sizing performance of the surface sizing starch prepared by the bio-enzyme hydrolysis method.

[0008] The technical solution adopted by the present invention to solve its technical problem is:

[0009] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0010] Step 1: Moisture heat treatment of starch: Weigh the original starch with a dryness of 92.47%, adjust the moisture content of the starch to 15-30%, the treatment temperature to 100-120°C, and the treatment time to 6-16h, and number the treated sample as C. X T X H X , where C represents moisture content, T represents treatment temperature, H represents treatment time, and the subscript X is the corresponding treatment condition; after the wet heat treatment is completed, the wet heat treated starch sample is placed in a 30-50°C forced air oven for drying for 10-24 hours, and the wet heat treated starch is obtained after grinding and sieving, and retained for later use;

[0011] Step 2: Take the wet heat treated starch obtained in step 1 and add distilled water to prepare a starch slurry with a mass concentration of 10-25%, place it in a constant temperature water bath at 37-40°C and stir for 5 minutes at a stirring speed of 300 rpm, transfer α-amylase to the starch slurry, the amount of amylase is 2.0-18.5 U / g, the enzyme activity is 45600 U / ml, and keep stirring in a constant temperature water bath at 37-40°C for 5-10 minutes at a speed of 300 rpm. After the end, heat it to 85-90°C while stirring at a heating rate of 1°C / min, keep warm for 20-40 minutes, place it in a 120°C oil bath to inactivate the enzyme for 5 minutes, obtain surface sizing starch, and place it in a water bath at 80-85°C for constant temperature storage for standby use;

[0012] Step 3: Add distilled water at the same constant temperature storage temperature to prepare a surface sizing solution with a mass fraction of 10% to 25%, and apply it to the coating machine to apply surface sizing to the corrugated base paper. The surface sizing amount is 1 to 4 g / m 2 The coated paper is immediately placed in a 105°C forced air oven to dry for 2 to 5 minutes, and the paper is calendered.

[0013] Furthermore, in step 1, the native starch is one or any combination of potato native starch, cassava native starch, and corn native starch.

[0014] Furthermore, in step 1, the wet heat treated starch sample is placed in a 30° C. forced air oven and dried for 12 hours.

[0015] Furthermore, in step 2, the wet heat treated starch obtained in step 1 is added with distilled water to prepare a starch slurry with a mass concentration of 25%, the amount of amylase used is 6.8U / g, the enzyme activity is 45600U / ml, and stirring is maintained in a 38°C constant temperature water bath for 5 to 10 minutes at a speed of 300rpm. After the end, the temperature is raised to 85°C while stirring at a heating rate of 1°C / min and kept warm for 30 minutes.

[0016] Furthermore, the conditions for the wet heat treatment of starch in step 1 are: adjusting the moisture content of the treated starch to 25%, the temperature to 100° C., and the time to 16 hours.

[0017] Furthermore, in step 3, distilled water having the same constant temperature storage temperature is added to prepare a surface sizing solution having a mass fraction of 10%;

[0018] Alternatively, the surface sizing amount in step 3 is 3 g / m 2 The paper is placed in a blast oven and dried for 1 minute.

[0019] Furthermore, in step 3, the basis weight of the corrugated paper is 160±2 g / m 2The conditions for paper calendering treatment are: the upper roller is a rubber roller, the line pressure is 25N / mm, the creeping speed is 5m / min, and the steel roll temperature is 60℃.

[0020] Furthermore, the step 1 is specifically as follows: weigh the original starch with a dryness of 92.47%, numbered C X T X H X , where C represents moisture content, T represents treatment temperature, H represents treatment time, and the subscripts represent corresponding treatment conditions. ①C X T 100 H 16 Group: fixed heat treatment temperature at 100℃, treatment time at 16h, and starch moisture content at 15%, 20%, 25%, and 30%; ②C 30 T X H 16 Group: fixed moisture content of starch in heat treatment was 30%, treatment time was 16h, and design treatment temperature was 100℃, 110℃, 120℃; ③C 30 T 100 H X Group: The moisture content of the starch treated with wet heat was fixed at 30%, the treatment temperature was 100°C, and the designed treatment time was 6h, 10h, and 16h; after the wet heat treatment was completed, the wet heat treated starch sample was placed in a 30-50°C forced air oven and dried for 10-24h and retained.

[0021] The method as described above is used to improve the sizing performance of surface starch prepared by bio-enzyme hydrolysis.

[0022] The advantages and positive effects achieved by the present invention are:

[0023] 1. The method of the present invention is based on an environmentally friendly and simple wet heat treatment method to physically modify the original starch. The operation process has low requirements for moisture content, which is conducive to significantly reducing the energy consumption of drying wet heat treated starch, improving production efficiency, and can improve the sizing performance of the surface starch prepared by the bio-enzyme hydrolysis method. The method of the present invention is a method for further enhancing the sizing performance of the surface starch prepared by the bio-enzyme hydrolysis method. This method does not add any chemicals during the starch pretreatment process, and while ensuring safety, it also takes into account the green and low-carbon environmental protection concept. The surface starch prepared has excellent sizing performance and can be used for industrial production.

[0024] 2. The method of the present invention is based on a simple and easy-to-operate wet heat treatment to physically modify the native starch, and through the synergistic effect of α-amylase, surface sizing starch is obtained under a continuous cooking process. The preparation method is highly operable, and the preparation process does not add any ingredients harmful to the environment. It is green and environmentally friendly, and complies with the national low-carbon emission reduction strategic deployment. In addition, the preparation process is simple, the reaction conditions are mild and controllable, and it is suitable for large-scale manufacturing, and has broad application prospects in the field of papermaking technology.

[0025] 3. The method of the present invention uses starch treated with wet heat. Compared with native starch, the starch treated with wet heat has increased amylose content, increased solubility and reduced swelling, which will help to increase the initial concentration of cooked starch and reduce the viscosity of the surface starch.

[0026] 4. Compared with the original starch, the peak viscosity, trough viscosity and final viscosity of the wet heat treated starch used in the method of the present invention are significantly reduced, which effectively inhibits the retrogradation of starch, improves the stability of starch slurry, and ensures the performance stability of surface sizing starch during use.

[0027] 5. Compared with native starch, the ratio of amylose to amylopectin in the wet heat-treated starch used in the method of the present invention can be adjusted, which is beneficial to improving the reinforcing efficiency of the surface sizing starch, resulting in a significant improvement in the folding endurance, bursting index and ring crush index of the corrugated board.

[0028] 6. Compared with native starch, the wet heat-treated starch used in the method of the present invention further enhances the interaction between starch granules and amylase, which is beneficial to improving the enzymatic hydrolysis behavior of starch, thereby directly affecting the rheological behavior and enhanced performance of the surface starch prepared by enzymatic hydrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a graph showing the effect of enzyme dosage on the viscosity of surface sizing starch in the present invention;

[0030] Figure 2 This is a graph showing the effect of the initial concentration of the starch slurry on the mechanical properties of the surface sizing starch in the present invention;

[0031] Figure 3 This is a graph showing the effect of the termination temperature of starch cooking on the viscosity of the surface sizing starch in the present invention;

[0032] Figure 4 This is a graph showing the effect of the holding time after the end point of cooking on the viscosity of the surface sizing starch in the present invention;

[0033] Figure 5 This is a graph showing the effect of the amount of surface sizing starch on the mechanical properties of corrugated base paper in the present invention;

[0034] Figure 6This is a graph showing the amylose content of starch under different heat-moisture treatment conditions in the present invention;

[0035] Figure 7 It is the solubility diagram of starch under different wet heat treatment conditions in the present invention;

[0036] Figure 8 This is a diagram of the swelling degree of starch under different wet heat treatment conditions in the present invention;

[0037] Fig. 9 The figure is the effect of the wet heat treatment conditions of starch on the viscosity of the surface starch slurry in the present invention;

[0038] Fig.10 This is a graph showing the influence of the wet heat treatment conditions of starch in the present invention on the mechanical properties (folding endurance, ring crush index, bursting index and longitudinal tensile index) of corrugated paperboard glued with surface starch.

[0039] Fig.11 The best embodiment 3 of the present invention is the wet heat treatment starch C 25 T 100 H 16 SEM image of native starch. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with the embodiments. The following embodiments are descriptive rather than restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.

[0041] The various experimental operations involved in the specific embodiments are all routine techniques in the art. For parts not specially annotated in this document, ordinary technicians in the art can implement them by referring to various commonly used reference books, scientific and technological literature or related instructions, manuals, etc. before the filing date of this invention.

[0042] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0043] Step 1: Moisture heat treatment of starch: Weigh the original starch with a dryness of 92.47%, adjust the moisture content of the starch to 15-30%, the treatment temperature to 100-120°C, and the treatment time to 6-16h, and number the treated sample as C. X T X H X , where C represents moisture content, T represents treatment temperature, H represents treatment time, and the subscript X is the corresponding treatment condition; after the wet heat treatment is completed, the wet heat treated starch sample is placed in a 30-50°C forced air oven for drying for 10-24 hours, and the wet heat treated starch is obtained after grinding and sieving, and retained for later use;

[0044] Step 2: Take the wet heat treated starch obtained in step 1 and add distilled water to prepare a starch slurry with a mass concentration of 10-25%, place it in a constant temperature water bath at 37-40°C and stir for 5 minutes at a stirring speed of 300 rpm, transfer α-amylase to the starch slurry, the amount of amylase is 2.0-18.5 U / g, the enzyme activity is 45600 U / ml, and keep stirring in a constant temperature water bath at 37-40°C for 5-10 minutes at a speed of 300 rpm. After the end, heat it to 85-90°C while stirring at a heating rate of 1°C / min, keep warm for 20-40 minutes, place it in a 120°C oil bath to inactivate the enzyme for 5 minutes, obtain surface sizing starch, and place it in a water bath at 80-85°C for constant temperature storage for standby use;

[0045] Step 3: Add distilled water at the same constant temperature storage temperature to prepare a surface sizing solution with a mass fraction of 10% to 25%, and apply it to the coating machine to apply surface sizing to the corrugated base paper. The surface sizing amount is 1 to 4 g / m 2 The coated paper is immediately placed in a 105°C forced air oven to dry for 2 to 5 minutes, and the paper is calendered.

[0046] Preferably, the native starch in step 1 is one or any combination of potato native starch, cassava native starch, and corn native starch.

[0047] Preferably, in step 1, the wet heat treated starch sample is placed in a 30° C. forced air oven and dried for 12 hours.

[0048] Preferably, in step 2, the heat-treated starch obtained in step 1 is added with distilled water to prepare a starch slurry with a mass concentration of 25%, the amount of amylase used is 6.8U / g, the enzyme activity is 45600U / ml, and stirring is maintained in a constant temperature water bath at 38°C for 5 to 10 minutes at a speed of 300rpm. After the end, the temperature is raised to 85°C while stirring at a heating rate of 1°C / min and kept warm for 30 minutes.

[0049] Preferably, the conditions for the wet heat treatment of starch in step 1 are: adjusting the moisture content of the treated starch to 25%, the temperature to 100° C., and the time to 16 hours.

[0050] Preferably, in step 3, distilled water having the same constant temperature storage temperature is added to prepare a surface sizing solution having a mass fraction of 10%;

[0051] Alternatively, the surface sizing amount in step 3 is 3 g / m 2 The paper is placed in a blast oven and dried for 1 minute.

[0052] Preferably, the basis weight of the corrugated paper in step 3 is 160±2g / m 2The conditions for paper calendering treatment are: the upper roller is a rubber roller, the line pressure is 25N / mm, the creeping speed is 5m / min, and the steel roll temperature is 60℃.

[0053] Preferably, the step 1 is specifically as follows: weigh the original starch with a dryness of 92.47%, numbered C X T X H X , where C represents moisture content, T represents treatment temperature, H represents treatment time, and the subscripts represent corresponding treatment conditions. ①C X T 100 H 16 Group: fixed heat treatment temperature at 100℃, treatment time at 16h, and starch moisture content at 15%, 20%, 25%, and 30%; ②C 30 T X H 16 Group: fixed moisture content of starch in heat treatment was 30%, treatment time was 16h, and design treatment temperature was 100℃, 110℃, 120℃; ③C 30 T 100 H X Group: The moisture content of the starch treated with wet heat was fixed at 30%, the treatment temperature was 100°C, and the designed treatment time was 6h, 10h, and 16h; after the wet heat treatment was completed, the wet heat treated starch sample was placed in a 30-50°C forced air oven and dried for 10-24h and retained.

[0054] The method as described above is used to improve the sizing performance of surface starch prepared by bio-enzyme hydrolysis.

[0055] The native starch in the present invention was purchased from Tianjin Jiangtian Chemical Technology Co., Ltd. with the item number S818265; the α-amylase in the present invention was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. with the item number A834632; the raw materials used in the present invention, unless otherwise specified, are conventional commercial products, and the methods used in the present invention, unless otherwise specified, are conventional methods in the art.

[0056] In the following examples, the best cooking process scheme for surface sizing starch is:

[0057] A starch slurry with a mass fraction of 24% is prepared with deionized water, and then it is placed in a 38°C water bath and stirred for 5 minutes at a stirring speed of 300 rpm. 6.8 U / g of α-amylase is added to the slurry and stirred in a constant temperature water bath at 37-40°C for 10 minutes to make it evenly mixed. The enzyme activity is 45600 U / ml, and the rotation speed is 300 rpm. Then the temperature is continuously raised to a termination temperature of 85°C at a heating rate of 1°C / min, and it is kept at 85°C for 30 minutes. The starch slurry is placed in a 120°C oil bath to inactivate the enzyme for 5 minutes, and the slurry temperature is naturally cooled to 80°C. Deionized water with a temperature of 80°C is added to dilute the surface sizing starch slurry concentration to 10%, and the diluted surface sizing starch slurry is placed in a water bath with a temperature of 80°C for constant temperature storage for standby use.

[0058] The best cooking process of surface sizing starch adopted in the present invention is obtained based on the conditions that can be further optimized in the actual production process of the factory cooking workshop, while ensuring that the surface sizing starch has the best rheological behavior conducive to production needs and the best mechanical properties of the corrugated board. Figure 1 The data show that with the increase of amylase concentration, the viscosity value of the surface sizing starch slurry shows a significant downward trend. When the dosage of α-amylase is 4U / g, the viscosity value of the starch slurry drops sharply to 578cp. When the enzyme dosage is increased to 6.8U / g, the viscosity of the starch slurry tends to be stable, and the viscosity value is about 144cp. Therefore, the enzyme dosage selected for enzymatic starch hydrolysis in the present invention is 6.8U / g to meet the viscosity requirements of the sizing machine while taking into account the economic benefits of production. Figure 2 The data show that the initial cooking of starch slurry has little effect on the mechanical properties of sizing corrugated board, and the overall mechanical properties do not change much. From the perspective of production efficiency and economy, the higher the initial concentration of starch slurry, the more advantageous it is. For this reason, the initial cooking concentration of starch slurry is preferably set to 24%. Figure 3 The data show that the viscosity of the system decreases significantly after the termination temperature of starch cooking is 85°C. This may be because when the cooking temperature is greater than 85°C, the free glucan molecules in the starch slurry are partially degraded, which reduces the average molecular weight of the system and thus reduces the viscosity; when the termination temperature increases from 70°C to 85°C, the viscosity of the starch slurry increases slightly. This may be because before 85°C, the starch granules are not fully swollen and the glucan molecules are not fully free in the aqueous solution. Therefore, the optimal termination temperature for cooking starch in the present invention is 85°C. Figure 4 The data show that the final viscosity of the cooked starch decreases with the increase of the holding time. When the holding time reaches 30 minutes, the viscosity of the surface sizing starch slurry tends to be stable. Therefore, the optimal holding time for the cooked starch in the present invention is 30 minutes. The surface sizing starch obtained under the optimal cooking process conditions is applied to the surface of the corrugated paper (the basis weight of the corrugated paper is 160±2g / m 2), change the amount of surface glue, and measure the mechanical properties of corrugated board such as Figure 5 As shown in the data, the folding resistance of the corrugated board increases and then decreases with the increase of the glue application amount, and the ring crush index, burst index and tensile index (longitudinal) gradually increase. Therefore, the optimal glue application amount selected in the present invention is 3g / m 2 .

[0059] Specifically, the relevant preparation and detection are as follows:

[0060] Example 1

[0061] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0062] Step 1: Wet heat treatment of corn starch (in other embodiments, the raw starch is one or any combination of corn starch, tapioca starch, and potato starch), weigh 64.89 g of raw starch (dryness is 92.47%), add distilled water to make a sample with a moisture content of 15%, treat it in a 100° C. blast oven for 16 h, take out the sample, cool it to room temperature, place it in a 30° C. blast oven for 12 h, grind and sieve to obtain wet heat treated starch C 15 T 100 H 16 , keep for future use.

[0063] Step 2: Moist heat treatment of starch C 15 T 100 H 16 Determination of amylose content, solubility and swelling rate.

[0064] Step 3: Preparation of surface sizing starch: weigh 15.24g of heat-treated starch, add distilled water to prepare a starch slurry with a solid content of 24%, stir in a constant temperature water bath at 38°C for 5 minutes to mix evenly, then add 6.8U / g of α-amylase to the starch slurry and stir continuously for 10 minutes at 38°C at a speed of 300rpm. Keep stirring and continue to heat to 85°C, keep warm for 30 minutes, place in a 120°C oil bath to inactivate the enzyme for 5 minutes to obtain surface sizing starch, and measure the viscosity of the surface sizing starch slurry at this temperature and its viscosity when cooled to 25°C.

[0065] Step 4: Glue the corrugated board surface. Take the surface glue starch in step 3 and add a certain amount of 85°C deionized water to dilute the surface glue starch solution to a solid content of 10%. Then use a semi-automatic coating machine to glue the corrugated board surface. The surface glue amount is 3g / m 2After sizing, the paper was placed in a 105℃ forced air oven to dry for 5 minutes, and then the paper was calendered. Finally, the paper sample was placed in a constant temperature and humidity laboratory at 23±1℃ and 50±2%RH for 24 hours to balance, and then the physical properties of the paper were measured.

[0066] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C 15 T 100 H 16 The straight chain starch content is 33.26%, the solubility is 9.8%, and the swelling ratio is 9.1; the starch C 15 T 100 H 16 The viscosity of the prepared surface sizing starch was 2628cp at 85°C, and the viscosity increased to 3175cp after cooling to room temperature, an increase of 20.8%. Compared with the viscosity of the surface sizing starch prepared from the original starch in Comparative Example 1 under the same conditions, the increase was about 3.5 times (from 4633cp to 16346cp), indicating that the stability of the surface sizing starch under the wet heat treatment condition was good; at the same time, the corrugated board was sizing at 85°C, and the folding endurance of the board after drying was 12.5±4.3 times, and the bursting index was 2.09±0.23Kpa·m 2 / g, the ring compression index is 12.3±0.1N·m / g, and the longitudinal tensile index is 46.1±2.0N·m / g. Compared with the native starch Nst of comparative example 1 and the surface starch prepared in comparative example 2, except for the folding endurance, all other properties are significantly improved.

[0067] Example 2

[0068] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0069] Step 1: The conditions for wet heat treatment of starch are the same as those described in Example 1 except that the moisture content of the starch slurry is controlled to be 20%. The wet heat treated starch obtained after grinding and sieving is C 20 T 100 H 16 , to be kept for future use.

[0070] Step 2: Moist heat treatment of starch C 20 T 100 H 16 Determination of amylose content, solubility and swelling rate.

[0071] Step 3: Same as step 3 in Example 1.

[0072] Step 4: Same as step 4 in Example 1.

[0073] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C20 T 100 H 16 The straight chain starch content is 33.63%, the solubility is 8.4%, and the swelling rate is 8.8; the starch C 20 T 100 H 16 The viscosity of the prepared surface sizing starch slurry at 85°C was 2652cp, and the viscosity decreased to 2291cp after cooling to room temperature, which was opposite to the viscosity change trend of Comparative Example 1 and Example 1. This may be because the degree of crystallization of the starch was high under the treatment conditions, the viscosity of the system after enzymatic hydrolysis was low, and the recrystallized starch was easily precipitated from the system during the cooling process, thereby further reducing the viscosity of the system; at the same time, the corrugated board was sizing at 85°C, and the folding endurance of the board after drying was 14.2±3.8 times, and the bursting index was 2.18±0.11Kpa·m 2 / g, the ring compression index is 12.1±0.2N·m / g, and the longitudinal tensile index is 47.3±1.2N·m / g. Compared with Comparative Examples 1, 2 and 4, the comprehensive performance is the best. It can be seen that the water content of the wet-heat treated starch has a great influence on the enzymatic hydrolysis performance of the starch.

[0074] Example 3

[0075] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0076] Step 1: The conditions for wet heat treatment of starch are the same as those described in Example 1 except that the moisture content of the starch slurry is controlled to be 25%. The wet heat treated starch obtained after grinding and sieving is C 25 T 100 H 16 , to be kept for future use.

[0077] Step 2: Moist heat treatment of starch C 25 T 100 H 16 Determination of amylose content, solubility and swelling rate.

[0078] Step 3: Same as step 3 in Example 1.

[0079] Step 4: Same as step 4 in Example 1.

[0080] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C 25 T 100 H 16 The straight chain starch content is 33.99%, the solubility is 9.2%, and the swelling ratio is 7.0; the starch C 25 T 100 H 16The viscosity of the prepared surface sizing starch was 623cp at 85℃, and the viscosity increased to 2312cp after cooling to room temperature, with high stability. 25 T 100 H 16 and the surface morphology of native starch granules, Fig.11 The results showed that the surface of starch granules was no longer smooth under this condition, but became more irregular compared with the original starch, with obvious peeling layers and depressions on the surface, indicating that C 25 T 100 H 16 Starch is more conducive to enzymatic hydrolysis than native starch, thus changing the composition and properties of the enzymatic hydrolysate; at the same time, starch C is treated with wet heat at 85°C. 25 T 100 H 16 The prepared sizing solution was used to glue the corrugated board. After drying, the folding endurance of the board was 19.4±7.5 times, and the bursting index was 2.32±0.14Kpa·m. 2 / g, the ring crush index is 12.8±0.4N·m / g, and the longitudinal tensile index is 54.6±2.1N·m / g. Compared with the performance of the original starch enzymatic sizing solution applied to the surface of the corrugated paper in the comparative example, the folding endurance is increased by 29.3%, the bursting index is increased by 32.6%, the ring crush index is increased by 42.2%, and the longitudinal tensile index is increased by 50.0%. Compared with comparative examples 1, 2, 3 and 4, the comprehensive performance of the paper under this condition is significantly improved. It can be seen that the moisture, temperature and treatment time of the wet heat treated starch have a great influence on the performance of the enzymatic starch.

[0081] Example 4

[0082] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0083] Step 1: The conditions for wet heat treatment of starch are the same as those described in Example 1 except that the moisture content of the starch slurry is controlled to be 30%. The wet heat treated starch obtained after grinding and sieving is C 30 T 100 H 16 , to be kept for future use.

[0084] Step 2: Moist heat treatment of starch C 30 T 100 H 16 Determination of amylose content, solubility and swelling rate.

[0085] Step 3: Same as step 3 in Example 1.

[0086] Step 4: Same as step 4 in Example 1.

[0087] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C 30 T 100 H 16 The straight chain starch content is 38.37%, the solubility is 7.1%, and the swelling ratio is 6.8; the starch C 30 T 100 H 16 The viscosity of the prepared surface sizing starch was 493cp at 85℃, and the viscosity increased to 826cp after cooling to room temperature. At the same time, the corrugated cardboard was sizing at 85℃, and the folding endurance of the cardboard after drying was 12.5±7.3 times, and the bursting index was 2.19±0.14Kpa·m 2 / g, the ring compression index is 12.1±0.3N·m / g, and the longitudinal tensile index is 43.2±6.2N·m / g. Compared with Comparative Example 1 and Comparative Example 2, the content of amylose is the highest and the performance is greatly improved; this once again proves that the moisture content of wet-heat treated starch has the greatest influence on the physicochemical properties of starch and the performance of its sizing solution.

[0088] Example 5

[0089] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0090] Step 1: Wet heat treatment of corn starch (in other embodiments, the raw starch is one or any combination of corn starch, tapioca starch, and potato starch), weigh 64.89 g of raw starch (dryness 92.47%), add distilled water to make a sample with a moisture content of 30%, treat it in a 110° C. blast oven for 16 h, take out the sample, cool it to room temperature, place it in a 30° C. blast oven to dry for 12 h, grind and sieve to obtain wet heat treated starch C 30 T 110 H 16 , keep for future use.

[0091] Step 2: Moist heat treatment of starch C 30 T 110 H 16 Determination of amylose content, solubility and swelling rate.

[0092] Step 3: Same as step 3 in Example 1.

[0093] Step 4: Same as step 4 in Example 1.

[0094] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C 30 T 110 H 16 The straight chain starch content is 32.83%, the solubility is 4.5%, and the swelling ratio is 6.6; the starch C 30T 110 H 16 The viscosity of the prepared surface sizing starch was 83cp at 85℃, and the viscosity increased to 321cp after cooling to room temperature. At the same time, the corrugated cardboard was sizing at 85℃, and the folding endurance of the cardboard after drying was 14.6±4.9 times, and the bursting index was 2.25±0.21Kpa·m 2 / g, the ring compression index is 12.0±0.3N·m / g, and the longitudinal tensile index is 41.1±7.5N·m / g. The various properties are significantly better than those of Comparative Example 1. Compared with Example 4, the increase of temperature from 100°C to 110°C significantly reduces the content and solubility of amylose, and greatly reduces the viscosity of the enzymatic starch slurry, which is beneficial to surface sizing, but at the same time, the various mechanical properties of the sizing solution are improved to varying degrees.

[0095] Example 6

[0096] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0097] Step 1: The conditions for wet heat treatment of starch are the same as those of step 1 of Example 4 except that the temperature is controlled to be 120° C., and the wet heat treated starch obtained after grinding and sieving is C 30 T 120 H 16 , to be kept for future use.

[0098] Step 2: Moist heat treatment of starch C 30 T 120 H 16 Determination of amylose content, solubility and swelling rate.

[0099] Step 3: Same as step 3 in Example 1.

[0100] Step 4: Same as step 4 in Example 1.

[0101] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C 30 T 120 H 16 The straight chain starch content is 30.87%, the solubility is 8.9%, and the swelling ratio is 6.9; the starch C 30 T 120 H 16 The viscosity of the prepared surface sizing starch was 98cp at 85℃, and the viscosity dropped to 46cp after cooling to room temperature. At the same time, the corrugated cardboard was sizing at 85℃, and the folding endurance of the cardboard after drying was 18.2±7.5 times, and the bursting index was 2.29±0.18Kpa·m 2 / g, the ring crush index is 12.8±0.2N·m / g, and the longitudinal tensile index is 39.3±4.5N·m / g; compared with Example 4 and Example 5, under this condition, the straight chain content of starch is the lowest, the viscosity of the sizing solution is the lowest, and the folding endurance, ring crush index and bursting index of the paper after sizing are the best, but the tensile strength is slightly reduced, but far lower than the various properties of the paper in Example 3.

[0102] Example 7

[0103] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0104] Step 1: Wet heat treatment of corn starch (in other embodiments, the raw starch is one or any combination of corn starch, tapioca starch, and potato starch), weigh 64.89 g of raw starch (dryness 92.47%), add distilled water to make a sample with a moisture content of 30%, treat it in a 100° C. blast oven for 10 h, take out the sample, cool it to room temperature, place it in a 30° C. blast oven for 12 h, grind and sieve to obtain wet heat treated starch C 30 T 100 H 10 , keep for future use.

[0105] Step 2: Moist heat treatment of starch C 30 T 100 H 10 Determination of amylose content, solubility and swelling rate.

[0106] Step 3: Same as step 3 in Example 1.

[0107] Step 4: Same as step 4 in Example 1.

[0108] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C 30 T 100 H 10 The straight chain starch content is 29.50%, the solubility is 4.1%, and the swelling rate is 7.8; the starch C 30 T 100 H 10 The viscosity of the prepared surface sizing starch was 652cp at 85℃, and the viscosity increased to 1235cp after cooling to room temperature. At the same time, the corrugated cardboard was sizing at 85℃, and the folding endurance of the cardboard after drying was 15.8±4.6 times, and the bursting index was 2.29±0.08Kpa·m 2 / g, the ring crush index is 13.2±0.1N·m / g, and the longitudinal tensile index is 40.3±5.3N·m / g; compared with Example 4, the wet heat treatment time is adjusted to 10 hours, the amylose content is significantly reduced, and the viscosity of the surface sizing solution is significantly increased, so that the folding endurance, bursting index and ring crush index of the paper are slightly increased, and the tensile index is slightly decreased. This may be because the wet heat treatment time is shortened, which weakens the degree of directional reorganization of the starch structure, and the molecular weight of the starch is larger, thereby giving the paper better mechanical properties.

[0109] Example 8

[0110] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0111] Step 1: The conditions for the wet heat treatment of starch are the same as those of step 1 of Example 7 except that the time is controlled to be 6 hours, and the wet heat treated starch obtained after grinding and sieving is C 30 T 100 H6, to be kept for future use.

[0112] Step 2: Moist heat treatment of starch C 30 T 100 H6 Determination of amylose content, solubility and swelling rate.

[0113] Step 3: Same as step 3 in Example 1.

[0114] Step 4: Same as step 4 in Example 1.

[0115] The results of the test are as follows Figures 6 to 10 It shows that heat-moisture treated starch C 30 T 100 The amylose content of H6 was 28.88%, the solubility was 7.1%, and the swelling ratio was 7.8; 30 T 100 The surface sizing starch prepared by H6 has a slurry viscosity of 652cp at 85℃, and the viscosity increases to 1235cp after cooling to room temperature. At the same time, the corrugated cardboard is sizing at 85℃. After drying, the folding endurance of the cardboard is 13.2±2.7 times, and the bursting index is 2.31±0.19Kpa·m. 2 / g, the ring crush index is 15.2±0.1N·m / g, and the longitudinal tensile index is 37.3±8.4N·m / g. Compared with Example 4 and Example 7, as the wet heat treatment time increases, the amylose content increases, the viscosity of the surface starch decreases, and the bursting resistance index of the paperboard is the best; but except that the folding endurance is significantly lower than that of Comparative Example 1, the other properties are better than those of Comparative Example 1.

[0116] Comparative Example 1

[0117] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0118] Step 1: Except that the starch raw material is corn starch that has not been subjected to heat and moisture treatment, the rest is the same as Step 1 of Example 1.

[0119] Step 2: Determination of the amylose content, solubility and swelling rate of corn native starch NSt.

[0120] Step 3: Same as step 3 in Example 1.

[0121] Step 4: Same as step 4 in Example 1.

[0122] The results of the test are as follows Figures 6 to 10 The results showed that the straight chain starch content of corn starch was 23.92%, the solubility was 4.2%, and the expansion ratio was 9.3. The surface sizing starch prepared from the original starch had a slurry viscosity of 4633cp at 85°C, and the viscosity increased to 16346cp after cooling to room temperature. At the same time, the corrugated cardboard was sizing at 85°C, and the folding endurance of the cardboard after drying was 14.8±7.2 times, and the bursting index was 1.75±0.12Kpa·m. 2 / g, the ring compression index is 9.1±0.2N·m / g, and the longitudinal tensile index is 36.4±9.2N·m / g.

[0123] Comparative Example 2

[0124] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0125] Step 1: The conditions for wet heat treatment of starch are the same as those described in Example 3 except that the moisture content of starch is controlled to be 10%. The wet heat treated starch obtained after grinding and sieving is C 10 T 100 H 16 , to be kept for future use.

[0126] Step 2: Moist heat treatment of starch C 10 T 100 H 16 Determination of amylose content, solubility and swelling rate.

[0127] Step 3: Except for not measuring the viscosity of the surface starch, the rest is the same as described in Step 3 of Example 1.

[0128] Step 4: Same as step 4 in Example 1.

[0129] The results showed that the heat-moisture treated starch C 10 T 100 H 16The straight chain starch content is 23.91%, the solubility is 8.9%, and the swelling ratio is 6.9; the starch C 10 T 100 H 16 The prepared surface sizing starch slurry, after sizing the corrugated board, has very close performances in folding endurance, bursting index, ring crush index and longitudinal tensile index of the paper and the surface sizing starch prepared from the native starch NSt in Comparative Example 1, as shown in Table 1. This is because when the moisture content of the wet heat treated starch is 10%, the moisture content is extremely low, which is not enough to change the hydrogen bonding between the straight chain starch molecules in the starch granules, and the double helix microcrystalline structure is not moved or destroyed, so that the enzymatic hydrolysis characteristics of the starch and its sizing performance will not be changed.

[0130] Comparative Example 3

[0131] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0132] Step 1: The conditions for wet heat treatment of starch are the same as those described in Comparative Example 1 except that the temperature of the starch slurry is controlled to be 150°C, and the wet heat treated starch obtained after grinding and sieving is C 25 T 150 H 16 , to be kept for future use.

[0133] Step 2: Moist heat treatment of starch C 25 T 150 H 16 Determination of amylose content, solubility and swelling rate.

[0134] Step 3: Except for not measuring the viscosity of the surface starch, the rest is the same as Step 3 of Example 1.

[0135] Step 4: Same as step 4 in Example 1.

[0136] The results showed that the heat-moisture treated starch C 25 T 150 H 16 The straight chain starch content is 24.12%, the solubility is 10.1%, and the swelling ratio is 6.7; the starch C 25 T 150 H 16 The prepared surface sizing starch slurry, after sizing the corrugated board, has a folding endurance of 15.4±5.8 times and a bursting index of 1.83±0.21 Kpa·m 2 / g, the ring compression index is 12.1±0.1N·m / g, and the longitudinal tensile index is 43.6±3.2N·m / g, as shown in Table 1. This is because when the temperature of the wet heat treatment starch is 150°C, the molecular chains of the straight-chain starch or branched-chain starch molecules in the amorphous region of the starch molecules are cleaved due to the high temperature, and the microcrystalline structure of the starch moves under the dual effects of high heat and moisture. The microcrystalline region formed by the hydrate water bridge connection in the adjacent double helix structure is broken due to the high temperature, so that the hydrate water bridge is destroyed and reoriented, and the helical structure molecules are directly bonded by hydrogen bonds, the helical structure is more compact, and the crystallinity of the starch molecules is increased; thus, the straight-chain starch content, solubility and swelling rate are significantly lower than those in Example 3; thus, its sensitivity to enzymes is affected, the enzymolysis efficiency is reduced, and the reinforcing properties of the surface sizing starch slurry are changed, and its sizing properties are significantly lower than those in Example 3.

[0137] Comparative Example 4

[0138] A method for improving the sizing performance of surface starch prepared by a biological enzyme hydrolysis method, the method comprising the following steps:

[0139] Step 1: The conditions for wet heat treatment of starch are the same as those described in Comparative Example 1 except that the treatment time of starch is controlled to be 3 hours, and the wet heat treated starch obtained after grinding and sieving is C 25 T 100 H3, to be retained for future use.

[0140] Step 2: Moist heat treatment of starch C 25 T 100 H3 Determination of amylose content, solubility and swelling rate.

[0141] Step 3: Except for not measuring the viscosity of the surface starch, the rest is the same as Step 3 of Example 1.

[0142] Step 4: Same as step 4 in Example 1.

[0143] The results showed that the heat-moisture treated starch C 25 T 100 The amylose content, solubility and swelling rate of H3 are similar to those of native starch, which are 23.87%, 4.05% and 9.16 respectively. 25 T 100 The mechanical properties of the corrugated board prepared by the surface sizing starch slurry H3 under the same sizing parameters as those in Example 3 are shown in Table 1, with a folding endurance of 15.2±5.3 times and a bursting index of 1.76±0.22 Kpa·m 2 / g, ring crush index is 9.3±0.8N·m / g, and longitudinal tensile index is 35.7±1.9N·m / g. This is because even at the optimal heat treatment temperature and moisture content, the heat treatment time (3h) is too short, and the molecular structure inside the starch granules is not destroyed and rearranged in time, so that the microcrystalline structure of the starch does not change much compared with the original starch, making its enzymatic hydrolysis characteristics and the performance of the sizing solution almost close to those of the original starch.

[0144] At the same time, it can also be seen that there is a synergistic effect between the three conditions of 15-30% moisture content of starch, 100-120°C treatment temperature and 6-16h treatment time when the starch is subjected to wet heat treatment in the present invention. The three conditions can synergistically promote the regulation of related properties such as the solubility of starch after wet heat treatment, the content of amylose and the sensitivity to enzymes, thereby improving the sizing performance of the corrugated board surface starch.

[0145] In addition, by combining the best embodiment 3 with comparative examples 2, 3 and 4, it can be seen that the wet heat treatment conditions of starch are highly dependent on temperature and time at the optimal moisture content, and both are indispensable. Only when both are satisfied at the same time can the structure of starch molecules be changed, thereby adjusting the hydrolysis behavior of starch. It is further proved that there is a synergistic effect between the three conditions of 15-30% moisture content of starch, 100-120°C treatment temperature and 6-16h treatment time when the starch is wet-heat treated in the present invention, and the three conditions can synergistically promote the relevant properties of the starch after wet-heat treatment, thereby improving the sizing performance of the corrugated board surface starch.

[0146] Table 1 Physical properties of cardboard after comparative samples were applied on the surface of corrugated paper

[0147]

[0148] The relevant tests are as follows:

[0149] Characterization performance test:

[0150] Mechanical properties test: The bursting strength test refers to GB / T6545-1998 "Determination method of bursting strength of corrugated board", the folding endurance test refers to GB / T457-2008 "Standard for determination of folding endurance of paper and board", and the ring crush strength test refers to GB / T2679.8-1995- "Determination method of ring crush strength of paperboard".

[0151] Solubility (SA) and swelling (SP) test: Weigh 0.5g of the sample to be tested, put it into a 45mL centrifuge tube, add 40mL of distilled water, place it in an 85℃ water bath oscillator for 30min, take it out and cool it to room temperature, centrifuge it at 4000r / min for 15min. Pour out the supernatant, dry it at 130℃ to constant weight, and calculate the solubility and swelling according to the following formula 1 and formula 2 respectively.

[0152]

[0153] Where A is the mass of the dissolved substance in the supernatant in g; W is the dry weight of the sample in g; P is the mass of the sediment in the centrifuge tube in g.

[0154] Test of amylose content: Determination by iodine colorimetry

[0155] 1. Drawing of the standard curve of amylose

[0156] Accurately weigh 50 mg of amylose and amylopectin standards, place them in 50 mL volumetric flasks, moisten with 1 mL of ethanol, add 9 mL of 0.5 mol / L NaOH solution, heat and dissolve in a boiling water bath for 15 min, cool, dilute to volume with distilled water, mix well, and obtain 1 mg / mL amylose and amylopectin standard solutions, i.e., mother solutions.

[0157] The mother solution was taken into 50mL volumetric flasks according to the volume ratio of amylose standard solution: amylopectin standard solution of 0.2:2.3, 0.3:2.2, 0.4:2.1, 0.5:2.0, 0.6:1.9, 0.7:1.8, 0.8:1.7, and 20mL of distilled water was added to each flask. The pH was adjusted to 3 with 0.1mol / L HCl solution, and 0.5mol / L iodine reagent (2mg / mL) was added, and the volume was fixed with distilled water. After standing for 20min, the absorbance was measured at 620nm with a 1cm cuvette. The mass fraction of amylose in the mixed solution was used as the horizontal axis and the absorbance was used as the vertical axis. The standard curve was drawn to obtain the linear regression equation between absorbance and amylose content y=0.00562x+0.12711(R 2 =0.9937) and used it for the determination of amylose content.

[0158] 2. The content of amylose in the sample to be tested

[0159] Accurately weigh 50 mg of corn starch or toughened corn starch, place it in a 50 mL volumetric flask, moisten it with 1 mL of ethanol, then add 9 mL of 0.5 mol / L NaOH solution, heat and dissolve it in a boiling water bath for 15 min, and cool it. Make up to volume with distilled water, mix well, and get 1 mg / mL starch test solution. Pipette 2.5 mL of starch test solution into a 50 mL volumetric flask, add 20 mL of distilled water, adjust the pH to 3 with 0.1 mol / L HCl solution, add 0.5 mol / L iodine reagent (2 mg / mL), and make up to volume with distilled water. Let it stand for 20 minutes, and measure its absorbance at a wavelength of 620 nm. According to the absorbance value, the content of amylose in the sample to be tested is calculated by the standard curve equation. Each sample is measured three times in parallel, and the average value is calculated as the amylose content of the sample.

[0160] Test of gelatinization characteristics:

[0161] The gelatinization properties of starch samples were measured using a rapid viscosity analyzer RVA-4. Weigh 3 g of the starch sample to be tested and add deionized water to a total mass of 28 g. The rapid viscosity analyzer measurement parameters were set to balance the sample from 50 ° C for 1 min, heat it to 95 ° C at a rate of 120 ° C / min, and keep it warm for 2.5 min; then cool it to 50 ° C at a rate of 12 ° C / min and keep it warm for 2 min. The stirring bar was initially rotated at 960 r / min, stirred for 10 s to mix the material, and then the speed was set to 160 r / min.

[0162] Table 2 Gelatinization characteristics of starch under different heat and humidity treatment conditions

[0163] sample Gelatinization temperature / ℃ Peak viscosity / cp Low viscosity / cp Final viscosity / cp Regeneration value Peak time / s Corn starch 83.15 1896 1399 1973 574 336 <![CDATA[C 15 T 100 H 16 ]]> 84.75 1594 1159 1661 502 336 <![CDATA[C 20 T 100 H 16 ]]> 88.00 1368 1111 1525 414 352 <![CDATA[C 25 T 100 H 16 ]]> 92.10 1036 973 1105 132 408 <![CDATA[C 30 T 100 H 16 ]]> 94.55 953 907 1026 62 416 <![CDATA[C 30 T 110 H 16 ]]> 91.25 646 605 667 119 412 <![CDATA[C 30 T 120 H 16 ]]> 88.8 573 529 662 133 364 <![CDATA[C 30 T 100 H 10 ]]> 93.65 748 680 779 99 420 <![CDATA[C 30 T 100 H6]]> 92.85 876 812 912 100 420

[0164] In order to fully understand the effect of surface starch prepared by wet heat treatment on the mechanical properties of corrugated board, the present invention explores the effect of wet heat treatment conditions on the physicochemical properties of starch. Figure 6 , Figure 7 , Figure 8 And as shown in Table 2. Figure 6 The results showed that the amylose content of the wet-heat treated starch was higher than that of the native starch, and increased with the increase of moisture content. Figure 7 and Figure 8 The solubility and swelling data show that compared with native starch, the solubility of wet-heat treated starch increases to varying degrees, while the swelling tends to decrease. This is because wet-heat treatment can break some amylopectin branches inside the starch molecules. As the water content increases, the number of free starch chains increases, and the breakage of amylopectin directly changes the straight chain / amylopectin content ratio inside the starch molecules, increasing the straight chain starch content, thereby affecting the solubility and swelling.

[0165] The gelatinization characteristics data in Table 2 show that the gelatinization temperature of the starch after wet heat treatment increases compared with that of the original corn starch. With the increase of moisture content and time of wet heat treatment, the gelatinization temperature shows an increasing trend, but with the increase of wet heat treatment temperature, the gelatinization temperature gradually decreases; among them, C 30 T 100 H 16 The highest gelatinization temperature is 94.55℃, which corresponds to the highest content of amylose. In addition, the peak viscosity, trough viscosity and final viscosity of starch significantly decreased after wet heat treatment compared with the original starch, which indicates that wet heat treatment hydrolyzes part of the amylopectin, which is manifested as a decrease in the viscosity of starch. 30 T 120 H 16 The viscosity of the starch was the lowest because the treatment temperature was the highest, which greatly promoted the hydrolysis of starch, especially the cleavage of amylopectin, causing the cleavage and rearrangement of the starch crystal structure, thereby increasing the accessibility of amylase but inhibiting the excessive hydrolysis of the enzyme. Therefore, the surface starch prepared by enzymatic hydrolysis has good rheological properties, which is beneficial to the surface sizing process. In addition, C 30 T 100 H 16 The recovery value of 62 is also much lower than the 661 of original corn starch, which shows that it has better stability and is convenient for maintaining the stability of the product during storage and transportation.

[0166] Fig.10 The data show that the surface sizing starch prepared by wet heat treatment starch can give corrugated board higher mechanical properties compared with the original starch in the comparative example, among which the wet heat treatment starch C 25 T 100 H 16 The prepared surface sizing starch can make the corrugated board have higher folding endurance, bursting index, ring crush index and tensile strength. This may be because the starch treated under this condition has a higher gelatinization temperature (92.10°C), and the starch cooking process of the present invention (the final temperature is 85°C) cannot guarantee that the starch granules are fully swollen, and the interaction between α-amylase and starch is constrained to a certain extent, thereby alleviating the degradation of starch. Fig.11 The apparent morphology of starch shows that the surface of the original starch is very flat and dense, while under this condition, a peeling layer appears on the surface of the starch granules, and the surface becomes rough; combined with Figure 6 The data of amylose content in the starch granules fully demonstrate that amylose can be leached from the granules under this condition, but the amylose in the starch granules cannot be fully released into the solution due to the hindrance of the granule shell, so that the glucan with a larger molecular weight in the system can be retained. Fig. 9The viscosity change trend diagram also proves that the slurry viscosity under this condition is appropriate. Without affecting the viscosity demand in production, the larger the molecular weight of dextran, the better its reinforcing effect on the surface fiber of paper, thereby significantly improving the mechanical properties of corrugated board.

[0167] In summary, the present invention discloses a method for improving the sizing performance of surface starch prepared by bio-enzyme hydrolysis. Compared with the traditional method, the method does not add any chemical reagents, has a simple treatment process, strong operability, low cost, and can improve the sizing performance of surface starch prepared by bio-enzyme hydrolysis without consuming a lot of material resources. It is an environmentally friendly product and meets the current national call for low-carbon emission reduction and energy conservation. The experimental results show that it is feasible to apply wet heat treated starch to corrugated board to enhance its surface starch sizing performance.

[0168] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.

Claims

1. A method for improving the sizing performance of surface starch prepared by bio-enzyme hydrolysis, Features: The method comprises the following steps: Step 1: Wet heat treatment of corn starch: weigh 64.89 g of corn starch with a dryness of 92.47%, add distilled water to make a sample with a moisture content of 15%, and treat it in a 100°C forced air oven for 16 h. Take out the sample, cool it to room temperature, and dry it in a 30°C forced air oven for 12 h. Grind and sieve to obtain wet heat treated starch C. 15 T 100 H 16 , keep for future use; Step 2: Moist heat treatment of starch C 15 T 100 H 16 Determination of amylose content, solubility and swelling rate; Step 3: Preparation of surface sizing starch: weigh 15.24g of heat-treated starch, add distilled water to prepare a starch slurry with a solid content of 24%, stir in a constant temperature water bath at 38°C for 5 minutes to mix evenly, then add 6.8U / g of α-amylase to the starch slurry and stir continuously for 10 minutes at 38°C at a speed of 300rpm. Keep stirring and continue to heat to 85°C, keep warm for 30 minutes, place in a 120°C oil bath to inactivate the enzyme for 5 minutes, and obtain surface sizing starch. Determine the viscosity of the surface sizing starch slurry at this temperature and its viscosity when cooled to 25°C. Step 4: Glue the corrugated board surface. Take the surface glue starch in step 3 and add a certain amount of 85°C deionized water to dilute the surface glue starch solution to a solid content of 10%. Then use a semi-automatic coating machine to glue the corrugated board surface. The surface glue amount is 3g / m 2 After sizing, the paper was placed in a 105°C forced air oven for drying for 5 minutes, and then the paper was calendered; Moisture heat treated starch C 15 T 100 H 16 The straight chain starch content is 33.26%, the solubility is 9.8%, and the swelling ratio is 9.1; the starch C 15 T 100 H 16 The viscosity of the prepared surface sizing starch was 2628cp at 85℃, and the viscosity increased to 3175cp after cooling to room temperature, an increase of 20.8%. At the same time, the corrugated cardboard was sizing at 85℃, and the folding endurance of the cardboard after drying was 12.5±4.3 times, and the bursting index was 2.09±0.23 Kpa·m 2 / g, the ring compression index is 12.3±0.1 N·m / g, and the longitudinal tensile index is 46.1±2.0N·m / g.

2. Application of the method according to claim 1 in improving the sizing performance of surface starch prepared by bio-enzyme hydrolysis.

Citation Information

Patent Citations

  • Corn native starch surface sizing liquid and preparation method thereof, and paperboard

    CN111101399A

  • Modified sizing starch, surface sizing liquid and preparation method and application thereof

    CN111303307A

  • Use of cellulose derivatives and method for surface sizing

    CN115210426A

  • Method for preparing gelatinized starch

    CN101649576A

  • Method for producing starch glue by low-temperature fast enzymatic conversion

    CN101649582A