A precious metal doped cerium dioxide pseudo-homogeneous supported catalyst and its preparation method and application

By doping precious metals with ceria quasi-homogeneous supported catalysts, the problem of difficult separation of homogeneous catalysts and uneven surfaces of heterogeneous catalysts is solved, high activity and stability are achieved, and the mass transfer resistance of liquid-solid reaction is significantly reduced. , and suitable for liquid phase catalytic reactions.

CN116440897BActive Publication Date: 2024-11-12XIANGTAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310454561.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-12
Estimated Expiration
2043-04-25

AI Technical Summary

Technical Problem

The existing homogeneous catalysts are difficult to separate, the surface of the heterogeneous catalysts is uneven and there are internal diffusion restrictions, resulting in poor catalytic activity and selectivity, making it difficult to adapt to the demand for liquid phase reactions.

Method used

Using precious metal doped ceria quasi-homogeneous supported catalyst, the noble metal is anchored on the ceria support through spontaneous redox reaction, and ultrafine nanoparticles of 3-5nm can be prepared, which can be evenly dispersed in the reaction liquid. The gas-liquid-solid three-phase catalytic reactions such as hydrogenation, oxidation, and deoxygenation significantly reduces the mass transfer resistance.

Benefits of technology

The high activity and stability of the catalyst are achieved, and the conversion rate of liquid-solid reaction can be significantly improved under mild conditions and reduced mass transfer resistance. It is suitable for environments where stirring is not allowed, and the catalyst is easy to recover.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116440897B_ABST
    Figure CN116440897B_ABST
Patent Text Reader

Abstract

The present invention discloses a precious metal doped cerium dioxide pseudo-homogeneous supported catalyst and a preparation method and application thereof. The content of precious metal in the catalyst is 0.05-3wt%, and can be evenly dispersed in a reaction solution. The catalyst is prepared as follows: using a cerium dioxide dispersion as a carrier, during the impregnation loading process, utilizing the adsorption and reducibility of the carrier oxygen vacancies, anchoring the precious metal on the carrier through a spontaneous oxidation-reduction reaction, and then further liquid phase reduction. The preparation process of this method is simple to operate, and the obtained catalyst is evenly dispersed in the solution. In the gas-liquid-solid three-phase catalytic reaction, the catalytic effect of the active component is fully exerted, the mass transfer resistance is significantly reduced, and an excellent conversion rate can be exhibited even under non-stirring conditions, which is particularly suitable for catalytic processes in certain environments such as non-stirring and continuous liquid phase reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst research and development, and specifically relates to a precious metal-doped cerium dioxide pseudo-homogeneous supported catalyst and a preparation method and application thereof. Background Art

[0002] In a chemical reaction, some of the original chemical bonds of the reaction molecules must dissociate and form new chemical bonds, which requires a certain amount of activation energy. Adding a catalyst can reduce the activation energy of the reaction, change the reaction path, accelerate the chemical reaction and control the selectivity of the product, reduce energy consumption, improve operating conditions and reduce pollutant emissions, and simplify the production process route. In the modern petroleum and chemical industry, more than 90% of chemical processes and more than 60% of product production processes involve catalytic technology. The catalysts used exist in two forms, namely homogeneous and heterogeneous. Among them, homogeneous catalysts and reactants are in the same phase, the active center is relatively single, the selectivity is higher, and the side reactions are less, but it is difficult to separate from the system after use, and there are many restrictions when using it; however, heterogeneous catalysts use carriers with high specific surface area or a large number of pores to disperse and fix active substances. The catalyst can be easily separated and recycled, and is widely used in industrial processes. However, due to the uneven surface of the catalyst and only part of the active sites chemically adsorb the reactant molecules, and porous materials are often limited by internal diffusion, the activity and selectivity are generally poor. Therefore, how to develop highly active catalysts suitable for liquid phase reactions and their preparation technologies remains a huge challenge.

[0003] In recent years, the emergence of nanoparticles has provided people with a new research idea, especially transition noble metal nanoparticles have attracted the attention of researchers due to their high catalytic activity. Generally speaking, metal particles are loaded on a carrier, and the morphology of the carrier and the metal particle size have a great influence on the catalytic activity [Reference 1: Chem. Rev. 2020, 120, 11986]. When the active component is dispersed in a single atomic state, the catalytic effect of the active component can be fully exerted [Reference 2: Chem. Rev. 2018, 118, 4981]. If the loaded catalyst is further prepared into ultrafine nanoparticles, it can be evenly dispersed in the reaction solution. This system that is close to a homogeneous phase is called a pseudo-homogeneous phase, which enables it to have the characteristics of three-dimensional free rotation of homogeneous catalysis, so that the reactant molecules can fully contact with the catalyst surface, remove the internal diffusion restriction of multiphase catalysis, and have better heat and mass transfer performance, thereby improving the catalytic activity, such as Chinese invention CN 115007170 A discloses a palladium-copper alloy pseudo-homogeneous catalyst and a preparation method thereof. The prepared catalyst has excellent dispersibility in the liquid phase, and can catalyze the liquid-phase hydrogenation reaction of furfural for 2 hours under relatively mild reaction conditions to obtain a furfuryl alcohol yield of not less than 86%, significantly reducing the amount of active components used, saving costs and improving catalytic activity; Document 3 [Chem.Eng.J.2020,382,122883] uses a high-gravity rotating packed bed reactor to prepare palladium nanoparticles with controllable particle size and stable dispersion. Compared with other heterogeneous catalysts, the pseudo-homogeneous nanocatalyst exhibits higher catalytic activity in the reaction of catalyzing the reduction of nitrobenzene. Summary of the invention

[0004] In view of the technical problems in the prior art such as homogeneous catalysts being difficult to separate after use, heterogeneous catalysts having uneven surfaces, and only some active sites undergoing chemical adsorption, the present invention provides a quasi-homogeneous catalyst for reducing the mass transfer resistance of liquid-solid catalytic reactions, and a preparation method and application thereof. The catalyst has high activity and good stability, and the catalyst preparation method is simple to operate and is green and environmentally friendly.

[0005] The technical solution of the present invention is:

[0006] A precious metal doped cerium dioxide pseudo-homogeneous supported catalyst, the catalyst is 3-5nm ultrafine nanoparticles, can be evenly dispersed in a reaction solution, the precious metal active components in the catalyst are one or more of platinum, palladium, ruthenium, iridium and gold, the mass fraction of which is 0.05-3%, and the carrier is cerium dioxide.

[0007] Furthermore, the catalyst can be dispersed in C6-C 16 A solution composed of one or more of aromatic and alkane rings.

[0008] The above-mentioned catalyst is prepared by the following method: cerium dioxide is dispersed in a solvent, and then a metal salt solution is added to adsorb and anchor the precious metal ions on the cerium dioxide through a spontaneous oxidation-reduction reaction, and then the resulting solution is transferred into a high-pressure reactor and liquid-phase reduced under a hydrogen environment to obtain a precious metal-doped cerium dioxide pseudo-homogeneous supported catalyst.

[0009] Furthermore, the solvent is an aromatic hydrocarbon, an alkane or a cycloalkane.

[0010] Furthermore, the temperature of the spontaneous redox reaction is 0 to 80° C., preferably 20 to 60° C., and the time is 0.5 to 24 hours, preferably 6 to 12 hours.

[0011] Furthermore, the hydrogen pressure of the liquid phase reduction is 0.1-10 MPa, the temperature is 100-250° C., and the time is 0.1-24 hours.

[0012] The above catalyst is applied to gas-liquid-solid three-phase catalytic reactions such as hydrogenation, oxidation, and deoxygenation, and can demonstrate excellent activity. In intermittent reactions, it can significantly reduce mass transfer resistance and obtain a conversion rate of >99% without stirring.

[0013] Furthermore, the catalyst can be recovered by adding a polar solvent (such as ethanol) to the reaction solution.

[0014] The beneficial effects of the present invention are:

[0015] The present invention uses a cerium dioxide dispersion as a carrier. During the impregnation loading process, the adsorption and reducibility of oxygen vacancies in the carrier are utilized to anchor the noble metal on the carrier through a spontaneous redox reaction, and then further liquid-phase reduction is performed to prepare a noble metal pseudo-homogeneous catalyst. The obtained catalyst is ultrafine nanoparticles with a uniform size of 3 to 5 nm. The preparation operation is simple and the conditions are mild. Agglomeration of active components caused by high-temperature hydrogen reduction can be avoided. The obtained catalyst can be uniformly dispersed in a solution and exerts advantages similar to homogeneous catalysts. In liquid-phase reactions such as hydrogenation, deoxygenation, and oxidation, reactants and catalysts can be fully contacted, and the mass transfer resistance in liquid-solid reactions is significantly reduced. Even without stirring, a very high conversion rate is exhibited. The catalyst is particularly suitable for catalytic processes in certain environments such as non-stirring and continuous liquid-phase reactions, and provides an efficient and environmentally friendly preparation method for high-activity catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Figure 2 is a diagram showing the dispersion state of (a) the precious metal Pt doped ceria pseudo-homogeneous catalyst obtained in the present invention and (b) the commercial ceria-supported precious metal Pt catalyst in the liquid phase. Figure 1It can be seen that the precious metal Pt doped ceria pseudo-homogeneous catalyst obtained in the present invention can be uniformly dispersed in the reaction solution, while the commercial ceria-loaded precious metal Pt catalyst is in a precipitated state.

[0017] Figure 2 TEM images of (a) precious metal Pt doped ceria pseudo-homogeneous catalyst and (b) commercial ceria supported precious metal Pt catalyst, wherein: Figure 2 The black particles in a are Pt metal, with a size of about 10nm, and the particle size of the carrier cerium dioxide is 3-5nm. Figure 2 The particle size of the carrier cerium dioxide in b is 20 to 40 nm. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below with reference to specific embodiments, but the present invention is not limited thereto.

[0019] The reagents used in the examples were all analytically pure and the water was deionized water.

[0020] Example 1

[0021] Take 1g of CeO2 dispersion and add it to 3g of n-heptane, add chloroplatinic acid solution according to the Pt loading of 0.5wt%, stir and redox for 2h at 20℃, and evaporate to obtain solid. Take 0.2g of the above solid and add it to 15g of n-heptane, move it into the reactor for liquid phase reduction, remove the air in the reactor by displacement method, then heat it to 150℃, inject hydrogen to the pressure of 3MPa, the speed is 900r / min, and liquid phase reduction for 2h. After cooling, add 4g of nitrobenzene, remove the air in the reactor by displacement method, react for 4h at 50℃ and normal pressure hydrogen, the conversion rate of nitrobenzene is 100%, the selectivity of aniline is 99.9%, and after 5 cycles of reaction, the hydrodeoxygenation activity of the catalyst remains basically unchanged.

[0022] Example 2

[0023] Take 1g of CeO2 dispersion and add it to 3g of cyclohexane, add palladium ammonium nitrate solution according to the loading amount of Pd of 0.05wt%, stir and redox at 60℃ for 0.5h, evaporate to obtain solid. Take 1.0g of the above solid and add it to 15g of cyclohexane, move it into the reactor for liquid phase reduction, remove the air in the reactor by displacement method, then heat to 250℃, inject hydrogen to the pressure of 6MPa, the speed is 900r / min, and liquid phase reduction for 2h. After cooling, add 2g of nitrobenzene, remove the air in the reactor by displacement method, react for 4h at 50℃ and normal pressure hydrogen, the conversion rate of nitrobenzene is 100%, the selectivity of aniline is 99.9%, and after 5 cycles of reaction, the hydrodeoxygenation activity of the catalyst remains basically unchanged.

[0024] Example 3

[0025] Take 1g of CeO2 dispersion and add it to 3g of toluene, add ruthenium chloride solution according to the loading amount of Ru being 3wt%, stir and redox for 0.5h at 30℃, evaporate to dryness to obtain solid. Take 0.1g of the above solid and add it to 15g of toluene, move it into the reactor for liquid phase reduction, remove the air in the reactor by displacement method, then heat it to 250℃, inject hydrogen to the pressure of 10MPa, the speed is 900r / min, and liquid phase reduction is 0.1h. After cooling, add 4g of nitrobenzene, remove the air in the reactor by displacement method, react for 2h at 50℃ and normal pressure hydrogen, the conversion rate of nitrobenzene is 99%, the selectivity of aniline is 99.9%, and after 5 cycles of reaction, the hydrodeoxygenation activity of the catalyst remains basically unchanged.

[0026] Example 4

[0027] Take 1g of CeO2 dispersion and add it to 3g of cyclohexane, add chloroiridic acid solution according to the Ir loading of 1wt%, stir and redox at 0℃ for 24h, evaporate to obtain solid. Take 0.1g of the above solid and add it to 15g of cyclohexane, move it into a reactor for liquid phase reduction, remove the air in the reactor by displacement method, then heat it to 100℃, inject hydrogen to a pressure of 5MPa, the speed is 900r / min, and liquid phase reduction is carried out for 24h. After cooling, add 4g of nitrobenzene, remove the air in the reactor by displacement method, react for 4h at 50℃ and normal pressure hydrogen, the conversion rate of nitrobenzene is 99.9%, the selectivity of aniline is 99.9%, and after 5 cycles of reaction, the hydrodeoxygenation activity of the catalyst remains basically unchanged.

[0028] Example 5

[0029] Take 1g of CeO2 dispersion and add it to 3g of methylcyclohexane, add chloroauric acid solution according to the Au loading of 2wt%, stir and redox at 80℃ for 0.5h, evaporate to obtain solid. Take 0.5g of the above solid and add it to 15g of methylcyclohexane, move it into the reactor for liquid phase reduction, use displacement method to remove the air in the reactor, then heat to 150℃, inject hydrogen to the pressure of 0.1MPa, the speed is 900r / min, and liquid phase reduction is 12h. After cooling, add 4g of nitrobenzene, use displacement method to remove the air in the reactor, react at 50℃ and normal pressure hydrogen for 2h, the conversion rate of nitrobenzene is 100%, the selectivity of aniline is 99.9%, and after 5 cycles of reaction, the hydrodeoxygenation activity of the catalyst remains basically unchanged.

[0030] Example 6

[0031] Take 1g of CeO2 dispersion and add it to 3g of n-decane, add chloroplatinic acid acetone solution according to the Pt loading of 1wt%, stir and redox for 2h at 30℃, and evaporate to obtain solid. Take 0.2g of the above solid and add it to 15g of n-decane, move it into the reactor for liquid phase reduction, use displacement method to remove the air in the reactor, then heat it to 150℃, inject hydrogen to the pressure of 3MPa, and reduce it in liquid phase for 2h. After cooling, add 0.5g of guaiacol, use displacement method to remove the air in the reactor, react for 6h at 150℃ and 5.0MPa of hydrogen, the conversion rate of guaiacol is 99%, the selectivity of cyclohexane is 99%, and after 5 cycles of reaction, the hydrodeoxygenation activity of the catalyst remains basically unchanged.

[0032] Example 7

[0033] Take 1g of CeO2 dispersion and add it to 3g of n-decane, add chloropalladium acid solution according to the loading amount of Pd as 1wt%, stir and redox for 2h at 30℃, evaporate to obtain solid. Take 0.2g of the above solid and add it to 15g of n-decane, move it into a reactor for liquid phase reduction, remove the air in the reactor by displacement method, then heat it to 150℃, inject hydrogen to a pressure of 3MPa, and reduce it in liquid phase for 2h. After cooling, add 0.5g of benzyl alcohol, remove the air in the reactor by displacement method with oxygen, react for 6h at 100℃ and 1.0MPa oxygen conditions, the conversion rate of benzyl alcohol is 99%, the selectivity of benzaldehyde is 99%, and after 5 cycles of reaction, the hydrodeoxygenation activity of the catalyst remains basically unchanged.

[0034] Adding polar solvents such as ethanol to the reaction solutions obtained in the above examples can achieve catalyst recovery.

[0035] Comparative Example 1

[0036] In order to compare the difference between quasi-homogeneous catalysts and heterogeneous catalysts, commercial cerium dioxide was used as a carrier to prepare a Pt / CeO2 heterogeneous supported catalyst with a loading of 0.5 wt%. The catalyst (0.2 g), 15 g of n-heptane and 4 g of nitrobenzene were added to a high-pressure reactor. The device was installed and the air in the reactor was removed by displacement. The reaction was carried out at 50°C and normal pressure hydrogen for 4 hours. The conversion rate of nitrobenzene was only 24.8%, which was only 1 / 4 of the conversion rate in Example 1.

[0037] From the results of the examples, it can be seen that the quasi-homogeneous catalyst exhibits very high activity, significantly reduces mass transfer resistance, and the conversion rate of the raw material can be as high as 4 times that of the heterogeneous phase without stirring. At the same time, the catalyst obtained by the present invention can also show the characteristics of easy recovery of heterogeneous catalysts, and efficient recovery of the catalyst can be achieved by adding polar solvents such as ethanol.

Claims

1. A precious metal-doped cerium dioxide pseudo-homogeneous supported catalyst, characterized in that: The catalyst is 3-5 nm ultrafine nanoparticles, which can be evenly dispersed in the reaction solution. The noble metal active component in the catalyst is one or more of platinum, palladium, ruthenium, iridium and gold, with a mass fraction of 0.05-3%, and the carrier is cerium dioxide; The method for preparing the precious metal-doped cerium dioxide pseudo-homogeneous supported catalyst comprises the following steps: dispersing cerium dioxide in a solvent such as aromatic hydrocarbons, alkanes or cycloalkanes, adding a metal salt solution, adsorbing and anchoring precious metal ions on cerium dioxide through a spontaneous oxidation-reduction reaction, evaporating to obtain a solid, dissolving the solid in a solvent such as aromatic hydrocarbons, alkanes or cycloalkanes, and then transferring the obtained solution into a high-pressure reactor, performing liquid-phase reduction under a hydrogen environment, and obtaining a precious metal-doped cerium dioxide pseudo-homogeneous supported catalyst.

2. The method for preparing the precious metal-doped cerium dioxide pseudo-homogeneous supported catalyst according to claim 1 comprises the following steps: dispersing cerium dioxide in a solvent such as aromatic hydrocarbons, alkanes or cycloalkanes, adding a metal salt solution, adsorbing and anchoring the precious metal ions on the cerium dioxide through a spontaneous oxidation-reduction reaction, evaporating to obtain a solid, dissolving the solid in a solvent such as aromatic hydrocarbons, alkanes or cycloalkanes, and then transferring the obtained solution into a high-pressure reactor, and subjecting the solution to liquid-phase reduction in a hydrogen environment to obtain a precious metal-doped cerium dioxide pseudo-homogeneous supported catalyst.

3. The preparation method according to claim 2, characterized in that: The temperature of the spontaneous redox reaction is 20~60℃ and the time is 6~12 hours.

4. The preparation method according to claim 2, characterized in that: The hydrogen pressure of the liquid phase reduction is 0.1-10 MPa, the temperature is 100-250° C., and the time is 0.1-24 hours.

5. Use of the catalyst according to claim 1 or the catalyst obtained by the preparation method according to any one of claims 2 to 4 in a gas-liquid-solid three-phase catalytic reaction, characterized in that: The gas-liquid-solid three-phase catalytic reaction is a hydrogenation, oxidation or deoxygenation reaction.

6. The use according to claim 5, characterized in that: After the reaction, the catalyst can be recovered by adding a polar solvent to the reaction solution.

7. The use according to claim 6, characterized in that: The polar solvent is water or alcohol.