A method for preparing lithium carbonate using lithium-rich liquid obtained by lithium ion sieve adsorption method

Through the combined use of multi-layer adsorption towers and sodium-modified zeolite adsorbents, combined with sodium carbonate treatment, the problems of high energy consumption of lithium-rich liquid and low sodium ion removal efficiency after lithium ion sieve adsorption method is solved, and low-energy Preparation of lithium carbonate consumes less energy, thereby improving the yield of lithium ions and product quality.

CN116443901BActive Publication Date: 2024-10-25LIS (SHANGHAI) MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310287818.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-25
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

The energy consumption of the lithium-rich liquid extracted by the existing lithium ion sieve adsorption method is high and it is difficult to prepare marketable lithium carbonate products at low cost. In particular, the removal efficiency of sodium ions is low, resulting in the loss of lithium ions and increased energy consumption.

Method used

A multi-layer adsorption tower is used for lithium ion sieve adsorption treatment, sulfuric acid is used as the analytical solution, the lithium-rich liquid is adsorbed by sodium ions by adjusting the pH value and sodium modified zeolite adsorbent, combined with sodium carbonate treatment to prepare lithium carbonate, and further precipitated The mixed adsorption process of lithium mother liquor and lithium extraction solution improves the lithium recovery rate.

Benefits of technology

It achieves the preparation of lithium carbonate with low energy consumption and low cost, significantly improves the yield of lithium ions and product quality, reduces solid waste, and the process is environmentally friendly and has low energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116443901B_ABST
    Figure CN116443901B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium extraction from salt lakes, and specifically relates to a method for preparing lithium carbonate from a lithium-rich liquid obtained by a lithium ion sieve adsorption method, which has the advantage of low energy consumption. The method for preparing lithium carbonate from a lithium-rich liquid obtained by a lithium ion sieve adsorption method described in the present invention uses a multi-layer adsorption tower for efficient lithium extraction to perform lithium extraction by adsorption, and uses a sodium-modified zeolite adsorbent to perform sodium ion adsorption treatment on the lithium-rich liquid, and uses lithium precipitation mother liquor and lithium extraction analytical liquid to prepare lithium carbonate products. The lithium yield of the entire lithium extraction process is high, and almost no phase change occurs in the entire treatment process. Except for the final evaporation and crystallization process, other processes are carried out by low-energy filtration, water pumping and other methods, and the liquid can be recycled, which has the advantages of environmentally friendly process and low energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium extraction from salt lakes, and specifically relates to a method for preparing lithium carbonate using lithium-rich liquid obtained by a lithium ion sieve adsorption method, which has the advantage of low energy consumption. Background Art

[0002] Lithium is the lightest metal in the world, also known as "energy metal", and is an indispensable raw material to support the development of the new energy vehicle industry. With the increasing development of new energy technologies, the global demand for lithium continues to grow. Therefore, the development and utilization of lithium resources has become a hot spot in global research and development, and has received great attention. my country is rich in lithium resources, of which more than 70% are salt lake lithium resources. At present, the reported methods for extracting lithium from salt lake brine mainly include adsorption, precipitation, extraction, membrane separation, calcination, etc. Among them, lithium ion sieve adsorption method for lithium extraction from brine is one of the current research hotspots. This method uses lithium ion sieve adsorbents to adsorb Li in brine. + Adsorb and then use the desorption liquid to remove Li + Desorption is performed, and the obtained lithium-rich liquid is subjected to post-processing operations such as purification. As an emerging technology, the lithium-rich liquid produced by the lithium ion sieve adsorption method is different from the lithium-rich liquid obtained by the traditional ore method. At present, there is little research on how to prepare commercial lithium carbonate products from the lithium-rich liquid produced after lithium extraction by the lithium ion sieve adsorption method, especially how to prepare commercial lithium carbonate products from the lithium-rich liquid obtained by the lithium ion sieve adsorption method at low cost and low energy consumption.

[0003] In the process of lithium extraction by lithium ion sieve adsorption method, the existing adsorption tower is generally large in size, several meters high. When using manganese and titanium adsorbents with high adsorption speed and efficiency, no matter whether the brine enters from top to bottom or flows from top to bottom, during most of the adsorption process, the adsorbent in the adsorption tower is either in a state of being saturated and unable to adsorb any more, or in a state of not being saturated but the brine it contacts contains almost no lithium, resulting in low efficiency of the entire adsorption process.

[0004] In addition, after lithium ions are adsorbed from salt lake brine using a lithium ion screen, the adsorbed lithium ions need to be resolved into the analytical solution by an analytical process. After the analytical solution is concentrated, sodium hydroxide is added to adjust the pH to above 12, and calcium and magnesium ions can be filtered out. At this time, the lithium-rich solution mainly contains lithium ions, sodium ions (added in large quantities when adjusting the pH), and sulfate ions. The large presence of sodium ions makes it difficult to further concentrate the lithium-rich solution, and the energy consumption is high, and it also affects the effect of the final crystallization of lithium. In the prior art, the sodium ions of the lithium-rich solution of the sulfuric acid system can be removed by crystallization of mirabilite after freezing, but the energy consumption is high and some lithium ions will be lost during solid-liquid separation. The sodium ions of the lithium-rich solution of the chloride system cannot be removed, and only after the crystallization of lithium is precipitated, they are circulated or discharged with the mother liquor, resulting in a large amount of lithium ions being lost with the mother liquor. Therefore, how to remove the sodium ions in the lithium-rich solution with low energy consumption and without losing lithium ions is also a major problem faced in the field. Summary of the invention

[0005] To this end, the technical problem to be solved by the present invention is to provide a method for preparing lithium carbonate using a lithium-rich liquid obtained by a lithium ion sieve adsorption method, wherein the method has the advantages of low energy consumption, low cost and good economic benefits.

[0006] In order to solve the above technical problems, the present invention discloses a method for preparing lithium carbonate using a lithium-rich solution obtained by a lithium ion sieve adsorption method, characterized in that it comprises the following steps:

[0007] (1) transporting the salt lake brine to be treated to a multilayer adsorption tower provided with a lithium ion sieve adsorbent for lithium extraction, and performing decomposition using sulfuric acid as a decomposition liquid to obtain a sulfate solution, and performing concentration treatment to obtain an enriched sulfate solution;

[0008] (2) adjusting the pH value of the enriched sulfate solution to 11-12.5, collecting the liquid portion through solid-liquid separation to obtain a lithium-rich solution, and performing boron removal, calcium removal, magnesium removal, and manganese removal treatments on the lithium-rich solution;

[0009] (3) contacting the lithium-rich liquid with a sodium-modified zeolite adsorbent to perform sodium ion adsorption treatment to obtain a low-sodium lithium-rich liquid and performing a concentration treatment;

[0010] (4) adding excess sodium carbonate to the concentrated low-sodium lithium-rich solution and mixing, collecting the filter residue and the filtrate after solid-liquid separation to obtain a crude lithium carbonate product and a lithium precipitation mother liquor, respectively.

[0011] Specifically, in step (4), the sodium carbonate is controlled to be in excess of 10-30 wt %;

[0012] Preferably, in step (4), the mixing temperature of the low-sodium lithium-rich solution and the sodium carbonate is controlled to be 70-90°C.

[0013] Specifically, the step (4) further comprises the step of refining the crude lithium carbonate;

[0014] Preferably, the refining step includes the step of mixing the crude lithium carbonate with water, and the step of collecting the refined lithium carbonate and the refined filtrate respectively through solid-liquid separation;

[0015] Preferably, the step (4) further comprises the step of purifying the refined lithium carbonate through a hydrogenation reaction to prepare battery-grade lithium carbonate; and / or the step of combining the refined filtrate with the lithium precipitation mother liquor.

[0016] Specifically, in step (2), the pH value of the enriched sulfate solution is adjusted to 11-12.5, preferably 12.0, by adding sodium hydroxide.

[0017] In order to further prepare lithium carbonate products, the method for preparing lithium carbonate using the lithium-rich solution obtained by the lithium ion sieve adsorption method of the present invention also includes the step of preparing lithium carbonate using the lithium precipitation mother solution, including the following steps:

[0018] (a) mixing the lithium precipitation mother solution with the lithium extraction analysis solution to obtain a mixed solution;

[0019] (b) passing the mixed liquid through an adsorbent for adsorption treatment;

[0020] (c) After the adsorption is completed, the adsorbent is subjected to an analysis treatment, the obtained analysis solution is collected, and after lithium is precipitated by crystallization, a carbonation treatment is performed to obtain the desired lithium carbonate.

[0021] Specifically, in step (a), the lithium extraction analysis solution is a lithium-containing analysis solution obtained during the analysis process of lithium extraction from salt lake brine by adsorption method.

[0022] Specifically, in step (a), the mixing ratio of the lithium precipitation mother liquor and the lithium extraction analytical solution is such that the pH value of the obtained mixed liquid is regulated to be between 7.5 and 10.0.

[0023] Specifically, in step (a), the volume ratio of the lithium precipitation mother solution to the lithium extraction analysis solution is 1:1-1:20.

[0024] Specifically, the step (a) further includes filtering the precipitate generated in the mixed liquid. Since the analytical solution contains only a small amount of calcium and magnesium ions and the pH is weakly alkaline, a large amount of precipitate will not be generated. If a white precipitate appears during the mixing process, a simple filtration is sufficient, and this filtration process hardly generates lithium entrainment.

[0025] Specifically, in the step (b), the adsorbent includes manganese-based, titanium-based, and manganese-titanium-based lithium ion sieve adsorbents; preferably, the adsorbent is placed in an adsorption tower / column, and the amount of the adsorbent used can be based on the guided amount.

[0026] Preferably, the flow rate of the mixed liquid is controlled to be 2-20 times the volume of the adsorbent per hour.

[0027] Specifically, in the step (c), the eluent used in the analysis step includes acid solution;

[0028] Preferably, the eluent comprises an acid solution having a concentration of 0.01-1 mol / L;

[0029] Preferably, the eluent comprises at least one of sulfuric acid, hydrochloric acid, nitric acid or oxalic acid solution with a concentration of 0.01-1 mol / L.

[0030] Specifically, the step (c) further includes a step of washing the adsorbent before the analysis step;

[0031] Preferably, the rinsing step is rinsing with deionized water.

[0032] Specifically, the step (c) further includes the step of mixing the tail liquid of the mixed liquid after adsorption with the original brine of the salt lake and re-adsorbing it. Since the tail liquid after adsorption may still contain a small amount of lithium ions, and its pH is close to neutral, and the anions and cations it carries are all ions that must exist in the lithium-containing salt lake, it can be mixed into the original brine of the salt lake for another round of adsorption, thereby further improving the lithium yield of the entire system.

[0033] Specifically, in the step (c), the obtained analytical solution is the standard analytical solution in the adsorption method for lithium extraction from salt lakes production line, and the subsequent step also includes the step of recycling the obtained analytical solution to step (a) to mix with the lithium precipitation mother liquor for repeated adsorption.

[0034] Preferably, the analytical solution can be further concentrated and impurity-removed before crystallization and lithium precipitation, and after the lithium ion concentration reaches 20-30 g / L, it is heated to 60-80° C. and sodium carbonate is added or carbon dioxide is introduced to prepare a lithium carbonate product.

[0035] In order to achieve efficient lithium extraction from salt lake brine, the method of the present invention adopts an optimized multi-layer adsorption tower to carry out lithium ion adsorption and lithium extraction treatment.

[0036] Specifically, the multi-layer adsorption tower of the present invention at least comprises:

[0037] The main body has a hollow tower cavity, wherein the tower cavity has a water inlet and a water outlet;

[0038] Adsorption dishes are arranged in the tower cavity at intervals along the height direction of the main body, and each of the adsorption dishes is filled with an adsorbent;

[0039] The first water-permeable structure is arranged in the tower cavity and between two upper and lower adjacent layers of the adsorption dishes. The first water-permeable structure has a water-permeable state that allows water to pass through, and a water-isolating state that restricts water from passing through.

[0040] Furthermore, the first water-permeable structure includes a first partition and a second partition that are stacked, and a plurality of water-permeable holes are arranged on the plate surfaces of the first partition and the second partition; the first partition can rotate around its own axis so that the water-permeable holes on the first partition and the water-permeable holes on the second partition overlap with each other or are staggered with each other.

[0041] Furthermore, the first partition and the second partition are both inclined relative to the horizontal plane so that the lowest liquid level point and the highest liquid level point are formed between two adjacent first permeable structures; a liquid inlet and a liquid discharge port are provided at each of the lowest liquid level points, and a liquid discharge port is provided at each of the highest liquid level points.

[0042] Furthermore, the adsorption dish is of a columnar structure, a first filter screen is disposed on the top surface of the adsorption dish, and a second filter screen is disposed on the bottom surface of the adsorption dish; the first filter screen and the second filter screen are suitable for limiting leakage of the adsorbent in the adsorption dish.

[0043] Furthermore, the adsorption tower also includes a second water-permeable structure, which is arranged on the bottom surface of the adsorption dish and located on the side of the second filter screen facing away from the first filter screen. The second water-permeable structure has a water-permeable state that allows water to pass through, and a water-isolating state that restricts water from passing through.

[0044] Furthermore, a preset interval is left between the second water-permeable structure and the second filter screen, and the preset interval ranges from 1 mm to 2 mm.

[0045] Furthermore, a ring-shaped member is provided on the bottom surface of the adsorption dish, and a forklift moves the adsorption dish via the ring-shaped member.

[0046] Furthermore, the edges of the top and bottom surfaces of the adsorption dish are both provided with extensions, and the extensions extend in a direction away from the center of the adsorption dish, and are suitable for fixing the adsorption dish in the tower cavity through the extensions.

[0047] Furthermore, a door body is provided on the side wall of the tower cavity, which is suitable for taking out the adsorption dish in the tower cavity through the door body.

[0048] Furthermore, the bottom of the main body is a conical structure, and the water inlet and the water outlet are both located on the side wall of the conical structure.

[0049] Specifically, in the step (1), after the multi-layer adsorption tower is used to adsorb and extract lithium, sulfuric acid is used as the analytical solution to obtain a sulfate solution with a lithium ion concentration of 3-4 g / L, a sodium ion concentration of 3-4 g / L, a potassium ion concentration of 0.2-0.5 g / L, a magnesium ion concentration of 0.1-0.5 g / L, a calcium ion concentration of 0.05-0.2 g / L, and a boron concentration of 0.01-0.1 g / L.

[0050] Specifically, in step (1), the concentration step includes but is not limited to using reverse osmosis and the like, which can concentrate the sulfate solution after lithium extraction to a lithium ion concentration of about 10 g / L, and enrich the sulfate solution with other cations correspondingly enriched.

[0051] Specifically, in step (2), sodium hydroxide is added to adjust the solution to pH=12.0 and then filtered / centrifuged to obtain a lithium-rich solution with a lithium ion concentration of about 10 g / L. The lithium loss in this process is about 0.5%.

[0052] Specifically, in the step (2), according to the ion concentration of the lithium-rich solution, impurity removal treatment can be selectively performed by removing boron, calcium, magnesium, and manganese resins, and the lithium ion concentration of the obtained lithium-rich solution is about 10 g / L, the magnesium ion concentration is less than 1 ppm, the calcium ion concentration is less than 1 ppm, the boron concentration is less than 1 ppm, and the manganese ion concentration is less than 0.1 ppm.

[0053] Specifically, in order to further reduce the sodium ion concentration in the lithium-rich solution, the present invention selects to contact the lithium-rich solution with a sodium-modified zeolite adsorbent for sodium ion adsorption treatment to reduce the sodium ion concentration in the lithium-rich solution.

[0054] The invention provides a sodium modified zeolite adsorbent, which is modified by using analcime as raw material and subjected to saturated sodium sulfate treatment.

[0055] Optionally, the modification treatment is to boil the analcime in a saturated sodium sulfate solution for 2-4 hours.

[0056] Optionally, the modification process is repeated 3-6 times, and the turbid liquid is poured off after each modification process is completed.

[0057] Optionally, the usage ratio of the saturated sodium sulfate solution to analcime is 3-20 mL / g.

[0058] Optionally, the particle size of the analcime is 30-40 mesh.

[0059] Specifically, in the step (3), in the sodium ion adsorption step, the lithium-rich liquid is adsorbed using the sodium-modified zeolite adsorbent.

[0060] Optionally, the lithium-rich liquid is contacted with a sodium-modified zeolite adsorbent at a flow rate of 1-5 times the volume of the adsorbent per hour for a contact time of 2-5 hours to obtain a low-sodium lithium-rich liquid.

[0061] Optionally, the adsorption temperature is 10-60°C.

[0062] Optionally, the method further comprises performing analytical treatment on the adsorbed sodium-modified zeolite adsorbent;

[0063] Optionally, a solution with a pH of 1.5-2 and containing 0.05-0.3 mol / L lithium sulfate is used for analysis; optionally, a lithium ion sieve analysis solution is used for analysis.

[0064] Optionally, the lithium ion sieve analytical solution is brought into contact with the adsorbed sodium-modified zeolite adsorbent at a flow rate of 5-10 times the adsorbent volume / hour, and the contact time is 0.5-1 h.

[0065] Specifically, the preparation of the sodium modified zeolite is as follows: analcime is taken, ground into 30-40 meshes, placed in a saturated sodium sulfate solution and boiled for 2-4 hours, and the turbid liquid is poured off, and this process is repeated 3-6 times. After the zeolite modification is completed, it is dried and placed in an adsorption device.

[0066] Specifically, Figure 7 As shown, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution can be: the lithium-rich solution with a lithium ion concentration of about 10g / L, a sodium ion concentration of more than 10g / L, a pH of about 12.0, and anions mainly sulfate ions, is passed through an adsorption tower equipped with a sodium-modified zeolite adsorbent at a flow rate of 1-5 times the adsorbent volume / hour at room temperature or after heating, and the adsorption is completed after 2-5 hours. Since the adsorption selectivity of sodium-modified zeolite for hydrated sodium ions is much higher than that for hydrated lithium ions at 10-60°C and pH=11-12.5, the lithium ion concentration in the sodium-removed lithium-rich solution after adsorption is still about 10g / L, and the sodium ion concentration is not higher than 5g / L. The lithium-rich solution only needs to be simply concentrated to crystallize and precipitate lithium.

[0067] Since sulfate, sodium ions, and lithium ions are all valuable ions, there is no need to wash with water, and the sodium-type zeolite can be directly analyzed after adsorption. After using a lithium sulfate solution or lithium ion sieve analysis solution with a pH of about 1.5-2.0, 0.05-0.3 mol / L (i.e., the analysis solution obtained by using sulfuric acid analysis in the lithium ion sieve adsorption method for lithium extraction from salt lakes, hereinafter referred to as "lithium ion sieve analysis solution"), it is passed into the adsorption tower and circulated at a flow rate of 5-10 times the adsorbent volume / hour, and the analysis is completed in 0.5-1 hour. Since the lithium ion concentration in the lithium ion sieve analysis solution is higher than the sodium ion concentration, and the selectivity of the sodium-modified zeolite for hydrated sodium ions and hydrated lithium ions is not much different in an environment of pH = 1.5-2.0, a large amount of sodium ions are replaced by hydrogen ions and lithium ions from the zeolite. After the analysis of the zeolite is completed, the lithium ion sieve analysis solution becomes a zeolite analysis solution, in which the lithium ion concentration is reduced, the sodium ion concentration is greatly increased, and the pH is increased. The effective sites in the sodium-modified zeolite are occupied by hydrogen ions and lithium ions, which will be exchanged with sodium ions in the subsequent adsorption, and the lithium ions will enter the next round of lithium-rich solution for utilization.

[0068] After obtaining the zeolite analysis solution, the zeolite analysis solution is mixed with the lithium ion sieve analysis solution at a ratio of 1:1-1:5, and the sodium zeolite that has been adsorbed can be analyzed again. After the above analysis is completed, the sodium ion concentration in the zeolite analysis solution is much higher than the lithium ion concentration. When the sodium ion concentration in the zeolite analysis solution is ≥10g / L, it is simply concentrated to a sodium ion concentration of 30-40g / L and then frozen to below -10°C. A large amount of sodium sulfate decahydrate crystals precipitate. By centrifugation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained. Through this method, the sodium ions that are continuously enriched in the system can be stripped out of the system, thereby ensuring that the system itself can be recycled.

[0069] Typically, sodium sulfate decahydrate can be used to produce 0.5-2 mol / L sulfuric acid solution and 0.5-2 mol / L sodium hydroxide solution through bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration. At this point, all impurities have completed the cycle in the system without external discharge. The lithium-sodium ratio in the lithium-rich solution is increased to 2.5:1 or even 3:1, and the subsequent concentration and crystallization lithium precipitation process becomes very simple.

[0070] In the method of the present invention, after the sodium ion adsorption treatment in the lithium-rich liquid is carried out by the sodium-modified zeolite adsorbent, the obtained low-sodium lithium-rich liquid has a lithium ion concentration of about 10 g / L, a sodium ion concentration of about 5 g / L, a potassium ion concentration of about 0.1-0.3 g / L, a magnesium ion concentration of less than 1 ppm, a calcium ion concentration of less than 1 ppm, a boron concentration of less than 1 ppm, and a manganese ion concentration of less than 0.1 ppm.

[0071] Specifically, in step (4), the solution is concentrated to a concentration of about 30 g / L lithium ions, about 15 g / L sodium ions, and about 0.3-1 g / L potassium ions by high pressure reverse osmosis or the like; the solution is further evaporated and crystallized, and separated by centrifugation to obtain a solid, namely lithium hydroxide monohydrate crystals.

[0072] The method for preparing lithium carbonate by using lithium-rich liquid obtained by the lithium ion sieve adsorption method of the present invention uses a multi-layer adsorption tower for efficient lithium extraction to carry out lithium extraction by adsorption method, and the lithium yield is relatively high; and a sodium-modified zeolite adsorbent is used to carry out sodium ion adsorption treatment on the lithium-rich liquid, so that sodium ions can be continuously removed from a high-sodium and high-lithium solution in a low-energy consumption and recyclable process. Compared with the traditional method of removing sodium by freezing nitrate, energy consumption can be greatly saved. While removing sodium, part of potassium is also removed, so that the number of mother liquor cycles is greatly increased, thereby improving the lithium yield, reducing solid waste, and making the subsequent concentration, crystallization and lithium precipitation process very simple.

[0073] The method for preparing lithium carbonate by utilizing lithium-rich liquid obtained by the lithium ion sieve adsorption method of the present invention has a high lithium yield in the entire lithium extraction process. Considering the reuse of the mother liquor, the lithium yield in a single crystallization process is more than 97%. In addition, almost no phase change occurs in the entire treatment process. Except for the final evaporation and crystallization process, other processes are carried out in low-energy filtration, water pumping and other methods. The liquid can be recycled, and only a small amount of impurity ions leave the system in the form of solid waste. The method has the advantages of environmentally friendly process and low energy consumption.

[0074] The method for preparing lithium carbonate products from lithium precipitate mother liquor based on the adsorption method of the present invention, the lithium extraction method of mixing the lithium precipitate mother liquor after crystallization lithium precipitation with the lithium-containing analytical solution of the salt lake brine adsorption method lithium extraction process and then adsorbing, the introduction of the lithium extraction analytical solution significantly improves the lithium recovery rate of the adsorbent to the lithium precipitate mother liquor, and the sodium and potassium ions in the analytical solution obtained after adsorption have been significantly reduced, the quality of the analytical solution has been significantly improved, and there are no impurities in the lithium precipitate mother liquor that hinder the crystallization of lithium precipitation, and the crystallized lithium carbonate is of high quality. The method for preparing lithium products from lithium precipitate mother liquor based on the adsorption method of the present invention, the method of mixing and adsorbing the lithium extraction analytical solution with the lithium precipitate mother liquor, is mainly because the lithium precipitate mother liquor contains a large amount of carbonate ions, lithium ions, and a small amount of calcium and magnesium ions, which will form local precipitation during the adsorption process under a high pH environment, resulting in pore blockage in the adsorbent, thereby preventing the lithium precipitate mother liquor from further entering the internal structure of the adsorbent to complete the adsorption process. On the one hand, the introduction of the analytical solution greatly reduces the concentration of carbonate ions. At the same time, the introduced magnesium ions and calcium ions will also form a small amount of precipitates with excess carbonate. The concentration of carbonate ions in the mixed solution can be further reduced by simple filtration, reducing the clogging of the adsorbent. Moreover, the introduction of the analytical solution also reduces the pH value of the solution, further hindering the formation of local precipitation.

[0075] The method for preparing lithium carbonate products from lithium precipitate mother liquor based on adsorption method described in the present invention utilizes the method of mixing and adsorbing lithium extraction analysis solution with lithium precipitate mother liquor. The introduction of analysis solution greatly reduces the concentration of sodium ions and potassium ions in lithium precipitate mother liquor. Although the adsorbent itself has no selectivity for sodium and potassium ions, if the lithium precipitate mother liquor is directly adsorbed, high concentrations of sodium and potassium ions will always enter the new analysis solution through some holes, invalid points, etc., affecting the quality of the analysis solution. After the present invention introduces the analysis solution and mixes it with the lithium precipitate mother liquor, the sodium and potassium ions in the analysis solution obtained after adsorption have significantly decreased, so that the quality of the analysis solution has been significantly improved. The method for preparing lithium products from lithium precipitate mother liquor based on adsorption method described in the present invention can reuse the washing water after rinsing the adsorbent after adsorption is completed to further improve the total recovery efficiency of lithium ions.

[0076] The multi-layer adsorption tower described in the present invention has multiple adsorption dishes arranged at intervals in the tower cavity, and the first water-permeable structure can separate the various adsorption dishes, so that the adsorption tower has different combination modes of independent adsorption of a single dish and adsorption of multiple dishes in series, which ensures sufficient adsorption scale effect as a whole and ensures that the adsorbed brine can maintain as high an operating efficiency as possible under various conditions such as different lithium concentrations, different temperatures, and different flow rate conditions.

[0077] The multi-layer adsorption tower of the present invention, on the one hand, ensures sufficient scale effect in the overall adsorption scale, and on the other hand, fully considers the relative relationship between the diffusion velocity of brine inside the lithium ion sieve particles and the external flow velocity of the manganese / titanium adsorbent at conventional flow rates, thereby forming an adsorption dish that ensures the continuous and efficient operation of the lithium ion sieve. At the same time, through different combinations of independent adsorption of a single dish and adsorption of multiple dishes in series, it ensures that the adsorbed brine can maintain as high an operating efficiency as possible under various conditions such as different lithium concentrations, different temperatures, and different flow rate conditions.

[0078] The multi-layer adsorption tower of the present invention solves the problem of difficulty in loading and disassembling the adsorbent; improves the utilization efficiency of the adsorbent; reduces the dissolution loss of the adsorbent; solves the problem of standardization of the adsorption tower design, and the same adsorption tower design can be used for brines with different lithium concentrations; solves the problem of stability of lithium concentration in the desorption liquid of the adsorption tower, and the lithium concentration of the desorption liquid can be adjusted according to demand.

[0079] The sodium-modified zeolite adsorbent of the present invention, after the analcime is modified by saturated sodium sulfate, can show different adsorption selectivity for lithium ions and sodium ions in lithium-rich solution under different temperatures and different pH conditions, thereby realizing the continuous removal of sodium ions from high-sodium and high-lithium solutions in a low-energy consumption and recyclable process.

[0080] The sodium-modified zeolite adsorbent of the present invention utilizes the different adsorption selectivity of sodium-modified zeolite for lithium ions and sodium ions in lithium-rich solution under different temperatures and different pH conditions, and continuously removes sodium ions from high-sodium and high-lithium solutions in a low-energy, recyclable process. The lithium-sodium ratio in the lithium-rich solution can be increased to 2.5:1 or even 3:1, and the subsequent concentration, crystallization and lithium precipitation process becomes very simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0081] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0082] Figure 1 Schematic diagram of an adsorption tower in an embodiment of the present invention;

[0083] Figure 2 Schematic diagram of an adsorption dish in an adsorption tower in an embodiment of the present invention;

[0084] Figure 3 Schematic diagram of an insert ring in an adsorption tower in an embodiment of the present invention;

[0085] Figure 4 Schematic diagram of the first partition plate in the adsorption tower in an embodiment of the present invention;

[0086] Figure 5 It is a schematic diagram of the local structure at the lowest point of the liquid level formed by the first water permeable structure in the adsorption tower in the embodiment of the present invention;

[0087] Figure 6 It is a schematic diagram of the local structure at the highest point of the liquid level formed by the first water permeable structure in the adsorption tower in the embodiment of the present invention;

[0088] Figure 7 The specific operation process of reducing the sodium ion concentration in the lithium-rich solution of the present invention;

[0089] The reference numerals in the figure are as follows: 1-main body, 2-door body, 3-first water permeable structure, 4-adsorption dish, 5-extending edge, 6-first partition, 7-water permeable hole, 8-first filter screen, 9-second filter screen, 10-second water permeable structure, 11-insert ring, 12-liquid inlet, 13-liquid outlet, 14-liquid level meter, 15-thermometer, 16-pH meter. DETAILED DESCRIPTION

[0090] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0091] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0092] like Figure 1-6 The structure of the multi-layer adsorption tower used in the following embodiments of the present invention is shown. In the following embodiments of the present invention, the multi-layer adsorption tower with the above structure is used to perform lithium ion sieve adsorption and lithium extraction operations.

[0093] Figure 1 Schematic diagram of an adsorption tower in an embodiment of the present invention; Figure 2 Schematic diagram of an adsorption dish in an adsorption tower in an embodiment of the present invention; Figure 1 and Figure 2 As shown, this embodiment provides an adsorption tower, comprising at least: a main body 1, having a hollow tower cavity, the tower cavity having a water inlet and a water outlet; adsorption dishes 4, arranged in the tower cavity at intervals along the height direction of the main body 1, each adsorption dish 4 is filled with an adsorbent; a first water-permeable structure 3, arranged in the tower cavity and between two adjacent layers of adsorption dishes 4, the first water-permeable structure 3 having a water-permeable state allowing water to pass through, and a water-isolating state restricting the passage of water.

[0094] The adsorption tower provided in the present embodiment has a plurality of adsorption dishes 4 arranged at intervals in the tower cavity, and the first water-permeable structure 3 can separate the respective adsorption dishes 4, so that the adsorption tower has different combination modes of independent adsorption of a single dish and adsorption of multiple dishes in series, which ensures sufficient adsorption scale effect as a whole and ensures that the adsorbed brine can maintain as high an operating efficiency as possible under various conditions such as different lithium concentrations, different temperatures, and different flow rate conditions.

[0095] Figure 4 Schematic diagram of the first baffle in the adsorption tower in an embodiment of the present invention; Figure 4 As shown, the first water-permeable structure 3 includes a first partition plate 6 and a second partition plate which are stacked, and a plurality of water-permeable holes 7 are arranged on the plate surfaces of the first partition plate 6 and the second partition plate; the first partition plate 6 can rotate around its own axis so that the water-permeable holes 7 on the first partition plate 6 and the water-permeable holes 7 on the second partition plate overlap with each other or are staggered with each other.

[0096] Among them, the first partition 6 and the second partition are both inclined relative to the horizontal plane to form the lowest liquid level point and the highest liquid level point between the two adjacent first permeable structures 3; a liquid inlet 12 and a liquid discharge port 13 are provided at each lowest liquid level point, and a liquid discharge port 13 is provided at each highest liquid level point.

[0097] Figure 3 Schematic diagram of the insert ring in the adsorption tower in the embodiment of the present invention; Figure 3 As shown, the adsorption dish 4 is a columnar structure, a first filter screen 8 is arranged on the top surface of the adsorption dish 4, and a second filter screen 9 is arranged on the bottom surface of the adsorption dish 4; the first filter screen 8 and the second filter screen 9 are suitable for limiting the leakage of the adsorbent in the adsorption dish 4.

[0098] The adsorption tower further includes a second water-permeable structure 10, which is arranged on the bottom surface of the adsorption dish 4 and located on the side of the second filter screen 9 facing away from the first filter screen 8. The second water-permeable structure 10 has a water-permeable state that allows water to pass through, and a water-isolating state that restricts water from passing through.

[0099] There is a preset interval between the second water-permeable structure 10 and the second filter screen 9, and the preset interval ranges from 1 mm to 2 mm.

[0100] The bottom surface of the adsorption dish 4 is provided with an annular member, and the forklift moves the adsorption dish 4 via the annular member.

[0101] The edges of the top and bottom surfaces of the adsorption dish 4 are both provided with extensions 5 , which extend in a direction away from the center of the adsorption dish 4 , and are suitable for fixing the adsorption dish 4 in the tower cavity through the extensions 5 .

[0102] A door body 2 is provided on the side wall of the tower cavity, which is suitable for taking out the adsorption dish 4 in the tower cavity through the door body 2 .

[0103] The bottom of the main body 1 is a conical structure, and the water inlet and the water outlet are both located on the side wall of the conical structure.

[0104] Specifically, for example, the material of the main body 1 can be stainless steel or carbon steel, the inner lining can be made of acid and alkali resistant material, and the outer surface of the main body 1 can be sprayed with a coating resistant to high salt vapor corrosion.

[0105] For example, the adsorption column may be a cylindrical structure, the diameter of the main body 1 may range from 0.1 m to 10 m, and the height may range from 0.5 m to 20 m.

[0106] For example, the interior of the main body 1 can be divided into two to fifty layers, and each layer is provided with an adsorption dish 4 loaded with an adsorbent.

[0107] For example, a rectangular door 2 can be provided on each layer of the outer wall of one side of the main body 1, and when the door 2 is opened, it is used to load the adsorption dish 4. After the adsorption dish 4 is loaded, the door 2 is closed and the barrel wall of the adsorption tower is sealed.

[0108] For example, except for the bottom layer of the adsorption column, each layer has the same structure. The AB plane can be provided with a structural member for fixing the adsorption dish 4. For example, the structural member can be a rotating buckle provided on the inner wall of the tower cavity, or a ring-shaped protrusion can be provided on the inner wall of the tower cavity to fix the adsorption dish 4 in the tower cavity. After the adsorption dish 4 is installed, it cannot move in the vertical direction, and it cannot swing left and right in the tower cavity, which is conducive to improving the adsorption effect.

[0109] The first permeable structure 3 can be arranged at the CD plane in the tower cavity. The angle between the first partition plate 6 and the second partition plate and the horizontal plane can be 1°-45°. Preferably, the angle ranges from 1°-10°. Such an arrangement is beneficial to the liquid flow distribution and can facilitate the discharge and pumping of liquid.

[0110] For example, both the first partition 6 and the second partition can be composed of a thin circular plate with a plurality of circular water-permeable holes 7. When the first partition 6 and the second partition completely overlap, water can flow through quickly, and after rotating 1° to 30°, they can be completely water-proof. Both the first partition 6 and the second partition can be made of materials such as stainless steel or polytetrafluoroethylene, and can be fastened to each other by snaps at the black solid hole in the center of the circle. For example, the first partition 6 is on the upper layer, and the second partition is on the lower layer. Then, a magnet can be set every 60° on the rotatable circumference of the first partition 6, and an electromagnet is set every 60° at the corresponding position of the inner wall of the tower cavity. When the six electromagnets are energized at the same time, they can attract the magnets on the entire first partition 6, and the first partition 6 will rotate clockwise or counterclockwise by an angle with the center as the axis, so that the water-permeable holes 7 on the first partition 6 and the second partition overlap or stagger, and realize the switching of the water-permeable state or the water-proof state. For example, a spring connected between the first partition plate 6 and the second partition plate can be used to reset the first partition plate 6 and the second partition plate when the electromagnet is powered off.

[0111] Figure 5 Schematic diagram of the local structure at the lowest point of the liquid level formed by the first water permeable structure in the adsorption tower in the embodiment of the present invention; Figure 5 As shown, for example, position C is the lowest point of the liquid level in the upper layer after the first water-permeable structure 3 is water-proofed, and a liquid inlet 12 and a liquid outlet 13 are provided at this position, which can be connected to the corresponding pump body through pipelines. Position D is the highest point of the liquid level in the lower layer after the first water-permeable structure 3 is water-proofed, and a liquid outlet 13 is provided at this position, which can be connected to the corresponding pump body through pipelines.

[0112] Figure 6 FIG. 1 is a schematic diagram of a local structure at the highest point of the liquid level formed by the first water permeable structure in the adsorption tower in an embodiment of the present invention, as shown in FIG. Figure 6As shown, for example, a liquid level meter, a pH meter 16, a conductivity meter and a thermometer 14 and a liquid level meter 15 can be set on the inner wall of the tower cavity near the D position to collect corresponding data. The collected data can be directly read from the outside of the main body 1, and the collected corresponding data can also be sent to the central control system.

[0113] The bottom of the adsorption column is a conical structure, provided with a water inlet and a water outlet, which can be connected to the corresponding pump body through pipelines respectively.

[0114] For example, the adsorption dish 4 can be made of stainless steel or polytetrafluoroethylene and is acid and alkali resistant. The height of the adsorption dish 4 can be 0.05m-3m. The width of the edge 5 around the upper and lower circular surfaces of the adsorption dish 4 can be 0.5cm-5cm, and the thickness range can be 1mm-20mm. In this way, the edge 5 can not only facilitate the fixation of the adsorption dish 4 so that it remains horizontal after fixation, but also play a certain water-isolating role, ensuring that all water from the upper and lower sides passes through the middle of the adsorption dish 4, so that the water body can fully contact the adsorbent in the adsorption dish 4.

[0115] For example, the upper surface of the adsorption dish 4 is covered with a removable first filter screen 8. After the adsorption dish 4 is loaded with the adsorbent, the first filter screen 8 is fastened to prevent the adsorbent from overflowing upward from the adsorption dish 4. The lower surface of the adsorption dish 4 has three layers. From top to bottom, the first layer is a second filter screen 9 similar to the upper surface, which can be welded or bonded to the adsorption dish 4 to prevent the adsorbent from overflowing downward. Below the second filter screen 9 is the second layer, which is a second water-permeable structure 10. The second water-permeable structure 10 can be the same as the first water-permeable structure 3, and is also two thin plates. They are usually in a water-permeable state to facilitate the water permeation of the adsorbent. They are rotated to a water-proof state only when the adsorbent is taken out, so that the adsorbent can be sucked out / poured out together with the water. Below the second water-permeable structure 10 is the third layer, which is an insert ring 11. The insert ring 11 can be welded to the bottom of the adsorption dish 4 and is used for fixing and limiting when the forklift lifts the adsorption dish 4 and loads the adsorption dish 4 into the adsorption tower. For example, the insert rings 11 can also be two hollow rectangular tubes that match the outer shape of the adsorption dish 4, and do not move in the horizontal direction when the adsorption dish 4 is placed in the tower cavity.

[0116] For example, the spacing between the second filter screen 9 and the second water-permeable structure 10 is generally very small but must exist, for example, it can be 1mm-2mm. For the second water-permeable structure 10, the radius of the first baffle 6 of the upper layer can be slightly smaller than the inner diameter of the adsorption dish 4, so that it can rotate in the adsorption dish 4, and the second baffle of the lower layer can be firmly connected to the lower surface of the adsorption dish 4 by welding, snapping, etc. and flush with the lower surface of the adsorption dish 4, and the connection between the second baffle and the adsorption dish 4 can be sealed.

[0117] When in use, several pumps and acid tanks can be connected externally according to the design requirements of the adsorption tower to meet the needs of liquid inlet and outlet, liquid storage, etc. during the adsorption and desorption process.

[0118] The specific process is as follows:

[0119] Adsorbent unloading / loading:

[0120] When unloading the adsorbent, first adjust all the first permeable structures 3 to a permeable state, and drain the water in the adsorption tower through the drain port at F. Open the door 2 on the outer wall of the lowest or highest adsorption tower, and use a forklift to take out the adsorption dish 4 of that layer. Operate layer by layer until all the adsorption dishes 4 are taken out. Open the first filter screen 8 on the upper layer of all the adsorption dishes 4, and adjust the first permeable structure 3 on the lower layer of the adsorption dish 4 to a water-proof state. After filling each adsorption dish 4 with water, use the pump body to suck out / pour out all the adsorbent. Because there is a layer of water between the second filter screen 9 and the second permeable structure 10 on the lower layer of the adsorption dish 4, the adsorbent can be easily sucked out / poured out without sticking to the second filter screen 9. If you want to fill new adsorbent, adjust the second permeable structure 10 on the lower layer of the adsorption dish 4 to a permeable state, pump in the specified amount of new adsorbent, and then buckle the first filter screen 8 on the upper layer of the adsorption dish 4. After all the adsorption dishes 4 are loaded with new adsorbent, they are loaded into the adsorption tower one by one by a forklift, and then all the doors 2 on the outer wall of the main body 1 are closed, and the adsorbent loading is completed.

[0121] Adsorption and desorption:

[0122] Since the lithium ion sieve adsorbent has a strong adsorption capacity and a fast adsorption speed, according to different conditions such as the lithium concentration and pH value of the brine to be adsorbed, a single group of cycles can use one, two, three or even multiple layers of adsorption dishes 4 to adsorb the same part of brine at the same time. When only one layer of adsorption dishes 4 is used in a single group of cycles, the first permeable structure 3 below each layer of adsorption dishes 4 is adjusted to a water-proof state, the liquid inlet 12 above the C position is opened and connected to the brine tank, and the liquid discharge port 13 below the D position is opened and connected to the adsorption tail liquid tank, and each layer of adsorption dishes 4 is adsorbed separately. When two layers of adsorption dishes 4 are used in a single group of cycles, each two adjacent adsorption dishes 4 from the bottom of the adsorption tower are a unit, the first permeable structure 3 in the unit is adjusted to a permeable state, the first permeable structure 3 between the units is adjusted to a water-proof state, the liquid inlet 12 above the C position of the lower layer in the unit is opened and connected to the brine tank, and the liquid discharge port 13 below the D position of the upper layer in the unit is opened and connected to the adsorption tail liquid tank. The method of using three or more layers of adsorption dishes 4 in a single group of cycles is similar.

[0123] During water washing, all first permeable structures 3 are adjusted to a permeable state so that water can flow through as many adsorbents as possible, thereby achieving a water-saving effect. After water washing, the drain port at F can be opened to drain the washing water in the adsorption column, thereby increasing the lithium concentration of the desorption solution and reducing the impurity ion concentration.

[0124] During desorption, the first permeable structure 3 between each layer is adjusted to a water-proof state, the liquid inlet 12 at the C position is connected to the acid tank through the pump body, and the discharge port 13 at the D position is also connected back to the same acid tank to achieve cyclic desorption. After desorption is completed, the lithium concentration of the desorption liquid can be obtained in real time by a machine learning method for online monitoring of the lithium concentration of the desorption liquid. If the lithium concentration of the desorption liquid fails to meet the requirements of the subsequent process design, for example, the subsequent process design requires a lithium concentration greater than or equal to 2000ppm, and the lithium concentration of the desorption liquid is only 1500ppm in real time, the discharge port 13 at the C position can be opened and connected to another acid tank through the pump body, and after the desorption liquid is pumped to another acid tank, an appropriate amount of concentrated acid is added to the acid tank to mix thoroughly, and then the acid tank is connected to the 4 layers of the adsorption dish that have not yet been desorbed for desorption. After confirming that the lithium ion concentration of the desorption liquid meets the requirements, all of the desorption liquid is pumped into the desorption liquid tank. After all the adsorption dishes 4 are distributed according to the above process, as much desorption liquid as possible that meets the requirements can be obtained in the shortest time, and at the same time, the excess acid flowing through each part of the adsorbent is minimal, thereby greatly reducing the dissolution loss caused by acid leaching.

[0125] Example 1

[0126] The adsorption tower has a diameter of 1.6 meters, the adsorption dish is 30 cm high, there are 6 layers in total, the adsorption tower is 3 meters high, and the adsorbent is loaded in total of 3 cubic meters.

[0127] Unloading the old adsorbent and loading the new adsorbent requires 2 people, a forklift, and a pump body. It takes 0.8 hours to unload the old adsorbent and 1.5 hours to load the new adsorbent, for a total of 2.3 hours.

[0128] Single cycle adsorption of 60 cubic meters of brine from a salt lake. Each layer is selected as a unit during adsorption. The total adsorption and desorption time is 2 hours, the lithium ion recovery rate is 93%, the lithium ion concentration of the desorption solution is 2g / L, and the manganese dissolution loss is 0.012%.

[0129] Comparative Example 1

[0130] The adsorption tower has a diameter of 1.6 meters, a height of 3.5 meters, and is loaded with a total of 3 cubic meters of the same adsorbent.

[0131] Unloading the old adsorbent and loading the new adsorbent requires 3 people, a forklift, and a pump body. It takes 3.5 hours to unload the old adsorbent and 4 hours to load the new adsorbent, for a total of 7.5 hours.

[0132] A single cycle adsorption of 60 cubic meters of brine from the same salt lake took 4 hours, with a lithium ion recovery rate of 89%, a lithium ion concentration of 1.5 g / L in the desorption solution, and a manganese dissolution loss of 0.035%.

[0133] Example 2

[0134] The adsorption tower has a diameter of 1.6 meters, the adsorption dish is 30 cm high, with 6 layers in total, the adsorption tower is 3 meters high, and the adsorbent is loaded with 3 cubic meters. A single cycle adsorption of 240 cubic meters of brine from a salt lake was performed. During adsorption, 3 layers were selected as a unit. The total adsorption and desorption time was 4 hours, the lithium ion recovery rate was 95%, the lithium ion concentration of the desorption solution was 2g / L, and the manganese dissolution loss was 0.007%.

[0135] Comparative Example 2

[0136] The adsorption tower has a diameter of 1.6 meters and a height of 3.5 meters. It is loaded with 3 cubic meters of the same adsorbent. A single cycle adsorbs 240 cubic meters of brine from the same salt lake. The total adsorption and desorption time is 5 hours, the lithium ion recovery rate is 90%, the lithium ion concentration of the desorption solution is 1.4g / L, and the manganese dissolution loss is 0.03%.

[0137] Example 3

[0138] In this embodiment, the multilayer adsorption tower in the above embodiment 2 is used to extract lithium from the brine of JZCK Salt Lake in Tibet by adsorption method, and sulfuric acid is used as the analytical solution for analytical treatment to obtain a sulfate solution. The sulfate solution is subjected to reverse osmosis concentration treatment, and sodium hydroxide is added to adjust it to pH=12.0, and filtered or centrifuged to collect the liquid part, and the lithium-rich solution is treated by boron removal, calcium removal, magnesium removal, and manganese removal resin to obtain the desired lithium-rich solution.

[0139] After testing, the specific composition (g / L) of the lithium-rich solution in this embodiment includes: Li + 10.325g / L, Na + 12.672g / L, K + 0.986g / L, Ca 2+ <0.001g / L, Mg 2+ <0.001g / L, pH=12.

[0140] Example 4

[0141] In this example, the prepared sodium-modified zeolite adsorbent is used to perform sodium ion adsorption treatment on the lithium-rich solution in Example 3 to reduce the sodium ion concentration in the lithium-rich solution.

[0142] Preparation of sodium-modified zeolite: Take 40g of analcime (provided by Lingshou County Ningbo Mineral Products Co., Ltd., the same below), grind it to 30-40 mesh, place it in 120ml of saturated sodium sulfate solution and boil it for 4 hours, pour off the turbid liquid, repeat this process 3 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0143] The lithium-rich solution was passed through an adsorption tower filled with a sodium-modified zeolite adsorbent at a flow rate of 5 times the adsorbent volume / hour at room temperature of 15° C., and the adsorption was completed after 2 hours.

[0144] After testing, the lithium ion concentration in the low-sodium lithium-rich liquid after adsorption was 9.7g / L, and the sodium ion concentration was 4g / L.

[0145] Example 5

[0146] In this example, the prepared sodium-modified zeolite adsorbent is used to perform sodium ion adsorption treatment on the lithium-rich solution in Example 3 to reduce the sodium ion concentration in the lithium-rich solution.

[0147] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 800ml of saturated sodium sulfate solution and boil it for 2 hours, pour off the turbid liquid, repeat this process 6 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0148] After the lithium-rich solution was heated to 45° C., it was passed through an adsorption tower filled with a sodium-modified zeolite adsorbent at a flow rate of 1 times the adsorbent volume / hour. The adsorption was completed after 5 hours.

[0149] After testing, the lithium ion concentration in the low-sodium lithium-rich liquid after adsorption was 9.8g / L, and the sodium ion concentration was 3.3g / L.

[0150] Example 6

[0151] In this example, the prepared sodium-modified zeolite adsorbent is used to perform sodium ion adsorption treatment on the lithium-rich solution in Example 3 to reduce the sodium ion concentration in the lithium-rich solution.

[0152] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 400ml of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 4 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0153] After the lithium-rich solution was heated to 50°C, it was passed through an adsorption tower filled with sodium-modified zeolite adsorbent at a flow rate of 3 times the adsorbent volume / hour. The adsorption was completed after 4 hours.

[0154] After testing, the lithium ion concentration in the low-sodium lithium-rich solution after adsorption was 10.0 g / L, and the sodium ion concentration was 3.4 g / L.

[0155] Example 7

[0156] In this example, the prepared sodium-modified zeolite adsorbent is used to perform sodium ion adsorption treatment on the lithium-rich solution in Example 3 to reduce the sodium ion concentration in the lithium-rich solution.

[0157] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 200ml of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 5 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0158] like Figure 7 As shown in the figure, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution is: after the lithium-rich solution is heated to 50°C, it passes through an adsorption tower equipped with a sodium-modified zeolite adsorbent at a flow rate of 2 times the adsorbent volume / hour, and the adsorption is completed after 4 hours. The lithium ion concentration in the low-sodium lithium-rich solution after adsorption is 9.9g / L, and the sodium ion concentration is 3.5g / L. The lithium-rich solution only needs to be simply concentrated to crystallize and precipitate lithium.

[0159] After adsorption, sodium zeolite can be directly analyzed. + 2.032g / L, Na + 2.520g / L, K + 0.206g / L, Ca 2+ 0.020g / L, Mg 2+ 0.312g / L, pH=1.5) was passed into the adsorption tower, and then circulated and analyzed at a flow rate of 5 times the adsorbent volume / hour, and the analysis was completed in 1 hour. After the zeolite analysis was completed, the lithium ion sieve analysis liquid became the zeolite analysis liquid, in which the lithium ion concentration was 1.3g / L, the sodium ion concentration was 5.6g / L, and the pH was 2.0. The effective sites in the sodium-modified zeolite were occupied by hydrogen ions and lithium ions, which would be exchanged with sodium ions in the subsequent adsorption, and the lithium ions would enter the next round of lithium-rich solution for utilization.

[0160] After obtaining the zeolite analysis solution, the zeolite analysis solution is mixed with the lithium ion sieve analysis solution at a ratio of 1:1, and the adsorbed sodium zeolite can be analyzed again. After repeated use for 4 times, the sodium ion concentration in the zeolite analysis solution is 10.2g / L. After simply concentrating it to a sodium ion concentration of 30g / L and freezing it to -10°C, a large amount of sodium sulfate decahydrate crystals are precipitated. Through centrifugal separation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained.

[0161] The sodium sulfate decahydrate can be used to produce 1 mol / L sulfuric acid solution and 1 mol / L sodium hydroxide solution by bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration.

[0162] Example 8

[0163] In this example, the prepared sodium-modified zeolite adsorbent is used to perform sodium ion adsorption treatment on the lithium-rich solution in Example 3 to reduce the sodium ion concentration in the lithium-rich solution.

[0164] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 200ml of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 5 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0165] like Figure 7 As shown, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution is:

[0166] After the lithium-rich liquid is heated to 50°C, it is passed through an adsorption tower equipped with a sodium-modified zeolite adsorbent at a flow rate of 4 times the adsorbent volume / hour. The adsorption is completed after 4 hours. The lithium ion concentration in the low-sodium lithium-rich liquid after adsorption is 9.8g / L and the sodium ion concentration is 3.4g / L. The lithium-rich liquid only needs to be simply concentrated to crystallize lithium.

[0167] After the adsorption is completed, the sodium-type zeolite can be directly analyzed. After the lithium ion sieve analysis solution (same as Example 7) is passed into the adsorption tower, it is circulated and analyzed at a flow rate of 10 times the adsorbent volume / hour, and the analysis is completed in 0.5 hours. After the zeolite is analyzed, the lithium ion sieve analysis solution becomes a zeolite analysis solution, in which the lithium ion concentration is 1.5g / L, the sodium ion concentration is 5.1g / L, and the pH is 1.9. The effective sites in the sodium-modified zeolite are occupied by hydrogen ions and lithium ions, which will be exchanged with sodium ions in subsequent adsorption, and the lithium ions will enter the next round of lithium-rich solution for utilization.

[0168] After obtaining the zeolite analysis solution, the zeolite analysis solution was mixed with the lithium ion sieve analysis solution at a ratio of 1:5, and the adsorbed sodium zeolite was analyzed again. After repeated use 82 times, the sodium ion concentration in the zeolite analysis solution was 10.1 g / L. After simply concentrating it to a sodium ion concentration of 40 g / L and freezing it to -10°C, a large amount of sodium sulfate decahydrate crystals precipitated. Through centrifugal separation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained.

[0169] The sodium sulfate decahydrate can be used to produce 1 mol / L sulfuric acid solution and 1 mol / L sodium hydroxide solution by bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration.

[0170] Example 9

[0171] In this example, the prepared sodium-modified zeolite adsorbent is used to perform sodium ion adsorption treatment on the lithium-rich solution in Example 3 to reduce the sodium ion concentration in the lithium-rich solution.

[0172] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 200mL of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 4 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0173] like Figure 7 As shown, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution is:

[0174] After the lithium-rich liquid is heated to 50°C, it is passed through an adsorption tower equipped with a sodium-modified zeolite adsorbent at a flow rate of 3.5 times the adsorbent volume / hour. The adsorption is completed after 3.5 hours. The lithium ion concentration in the low-sodium lithium-rich liquid after adsorption is 9.5g / L and the sodium ion concentration is 3.7g / L. The lithium-rich liquid only needs to be simply concentrated to crystallize lithium.

[0175] After the adsorption is completed, the sodium-type zeolite can be directly analyzed. After the lithium ion sieve analysis solution (same as Example 7) is passed into the adsorption tower, it is circulated and analyzed at a flow rate of 8 times the adsorbent volume / hour, and the analysis is completed in 45 minutes. After the zeolite is analyzed, the lithium ion sieve analysis solution becomes a zeolite analysis solution, in which the lithium ion concentration is 1.4g / L, the sodium ion concentration is 5.4g / L, and the pH is 2.0. The effective sites in the sodium-modified zeolite are occupied by hydrogen ions and lithium ions, which will be exchanged with sodium ions in subsequent adsorption, and the lithium ions will enter the next round of lithium-rich solution for utilization.

[0176] After obtaining the zeolite analysis solution, the zeolite analysis solution was mixed with the lithium ion sieve analysis solution at a ratio of 1:3, and the adsorbed sodium zeolite was analyzed again. After repeated use 32 times, the sodium ion concentration in the zeolite analysis solution was 9.9 g / L. After simply concentrating it to a sodium ion concentration of 35 g / L and freezing it to -10°C, a large amount of sodium sulfate decahydrate crystals precipitated. Through centrifugal separation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained.

[0177] The sodium sulfate decahydrate can be used to produce 1 mol / L sulfuric acid solution and 1 mol / L sodium hydroxide solution by bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration.

[0178] Comparative Example 3

[0179] The only difference between this comparative example and Example 4 is that the natural analcime is not treated with sodium. The lithium ion concentration in the sodium-free lithium-rich solution after adsorption is about 9.2 g / L, and the sodium ion concentration is 10.4 g / L.

[0180] Comparative Example 4

[0181] Compared with Example 4, the only difference is that the adsorption temperature is a low temperature of 0°C (not frozen). After adsorption, the lithium ion concentration in the sodium-removed lithium-rich solution is about 10 g / L, and the sodium ion concentration is 11.3 g / L.

[0182] Comparative Example 5

[0183] Compared with Example 4, the only difference is that the adsorption temperature is room temperature 80° C. After adsorption, the lithium ion concentration in the sodium-removed lithium-rich solution is about 9.5 g / L, and the sodium ion concentration is 10.8 g / L.

[0184] Comparative Example 6

[0185] Compared with Example 4, the only difference is that saturated sodium carbonate is used instead of saturated sodium sulfate. After adsorption, the lithium ion concentration in the sodium-removed lithium-rich solution is about 8.2 g / L, and the sodium ion concentration is 8.9 g / L.

[0186] Example 10

[0187] In this embodiment, the multilayer adsorption tower in the above-mentioned embodiment 2 is used to extract lithium from brine taken from JZ Salt Lake in Tibet by adsorption method, and sulfuric acid is used as the analytical solution for analytical treatment to obtain a sulfate solution. The sulfate solution is subjected to reverse osmosis concentration treatment, and sodium hydroxide is added to adjust it to pH=12.0, and filtered or centrifuged to collect the liquid part, and the lithium-rich solution is treated by boron removal, calcium removal, magnesium removal, and manganese removal resin to obtain the desired lithium-rich solution.

[0188] The sodium-modified zeolite adsorbent prepared in Example 4 is further used to perform sodium ion adsorption treatment on the obtained lithium-rich solution to reduce the sodium ion concentration in the lithium-rich solution to obtain a low-sodium lithium-rich solution.

[0189] The obtained low-sodium lithium-rich liquid is concentrated to a lithium ion concentration of about 25g / L by reverse osmosis, and then an excess of 20wt% sodium carbonate at 80°C is added at 80°C, and the mixture is stirred at a constant temperature for 90 minutes and then centrifuged. The collected residue is the crude sodium carbonate, and the collected filtrate is the lithium precipitation mother liquor.

[0190] The crude sodium carbonate is stirred and washed with ultrapure water in a ratio of 1:1, and after 2 rounds of stirring and washing, the mixture is centrifuged to obtain a solid portion as refined lithium carbonate, which is dried to obtain an industrial grade or above lithium carbonate product. The obtained industrial grade lithium carbonate can be further purified by hydrogenation reaction to obtain battery grade lithium carbonate; and the liquid portion collected by centrifugation is the refined filtrate, which is combined with the lithium precipitation mother liquor to obtain the desired lithium precipitation mother liquor.

[0191] In the traditional lithium extraction process, the lithium precipitation mother liquor can only be discharged. In this embodiment, the analytical liquid after lithium extraction by the salt lake brine adsorption method is also selected for mixing treatment. The lithium precipitation mother liquor and the lithium extraction analytical liquid are mixed in a volume ratio of 1:10, and the precipitate produced in the mixed liquid is simply filtered to obtain a mixed liquid.

[0192] The mixed liquid was passed through an adsorption column filled with adsorbent LIS-S01 at a flow rate of 20 times the adsorbent volume / hour for adsorption treatment. After the adsorption was completed, the adsorbent was rinsed with deionized water, and then the adsorbent was analyzed using 0.05 mol / L sulfuric acid as the eluent, and the obtained analytical solution was collected.

[0193] In this embodiment, the obtained analytical solution is the standard analytical solution in the adsorption method for lithium extraction from salt lakes. It can be further concentrated and impurities removed before crystallization and lithium precipitation. After the lithium ion concentration reaches 20-30 g / L, it can be heated to 60-80°C and sodium carbonate can be added or carbon dioxide can be introduced to prepare a lithium carbonate product. The obtained analytical solution can also be circulated to mix with the lithium precipitation mother liquor for repeated adsorption steps.

[0194] In this embodiment, after the lithium precipitation mother liquor was adsorbed, 92% of the lithium in the lithium precipitation mother liquor was recovered and utilized, wherein the lithium recovery rate = (lithium concentration of brine - lithium concentration of adsorption tail liquid) / lithium concentration of brine * 100%.

[0195] However, when only the lithium precipitation mother liquor (without mixing with the lithium extraction analysis solution) is directly used for treatment based on the same adsorption method, only 42% of the lithium in the lithium precipitation mother liquor is recovered.

[0196] Embodiment 11

[0197] In this embodiment, the multilayer adsorption tower in the above-mentioned embodiment 2 is used to extract lithium from brine taken from the M salt lake in South America by adsorption method, and sulfuric acid is used as the analytical solution for analytical treatment to obtain a sulfate solution. The sulfate solution is subjected to reverse osmosis concentration treatment, and sodium hydroxide is added to adjust it to pH=12.0, and filtered or centrifuged to collect the liquid part, and the lithium-rich solution is treated by boron removal, calcium removal, magnesium removal, and manganese removal resin to obtain the desired lithium-rich solution.

[0198] The sodium-modified zeolite adsorbent prepared in Example 4 is further used to perform sodium ion adsorption treatment on the obtained lithium-rich solution to reduce the sodium ion concentration in the lithium-rich solution to obtain a low-sodium lithium-rich solution.

[0199] The obtained low-sodium lithium-rich liquid is concentrated to a lithium ion concentration of about 25g / L by reverse osmosis, and then an excess of 20wt% sodium carbonate at 80°C is added at 80°C, and the mixture is stirred at a constant temperature for 90 minutes and then centrifuged. The collected residue is the crude sodium carbonate, and the collected filtrate is the lithium precipitation mother liquor.

[0200] The crude sodium carbonate is stirred and washed with ultrapure water in a ratio of 1:1, and after 2 rounds of stirring and washing, the mixture is centrifuged to obtain a solid portion as refined lithium carbonate, which is dried to obtain an industrial grade or above lithium carbonate product. The obtained industrial grade lithium carbonate can be further purified by hydrogenation reaction to obtain battery grade lithium carbonate; and the liquid portion collected by centrifugation is the refined filtrate, which is combined with the lithium precipitation mother liquor to obtain the desired lithium precipitation mother liquor.

[0201] In the traditional lithium extraction process, the lithium precipitation mother liquor can only be discharged. In this embodiment, the analytical liquid after lithium extraction by the salt lake brine adsorption method is also selected for mixing and adsorption. The lithium precipitation mother liquor and the lithium extraction analytical liquid are mixed in a volume ratio of 1:20, and the precipitate produced in the mixed liquid is simply filtered to obtain a mixed liquid.

[0202] The mixed liquid was passed through an adsorption column filled with adsorbent LIS-S01 at a flow rate of 10 times the volume of the adsorbent per hour for adsorption treatment. After the adsorption was completed, the adsorbent was rinsed with deionized water, and then the adsorbent was analyzed using 1 mol / L hydrochloric acid as the eluent, and the obtained analytical solution was collected.

[0203] In this embodiment, the obtained analytical solution is the standard analytical solution in the adsorption method for lithium extraction from salt lakes. It can be further concentrated and impurities removed before crystallization and lithium precipitation. After the lithium ion concentration reaches 20-30 g / L, it can be heated to 60-80°C and sodium carbonate can be added or carbon dioxide can be introduced to prepare a lithium carbonate product. The obtained analytical solution can also be circulated to mix with the lithium precipitation mother liquor for repeated adsorption steps.

[0204] In this embodiment, after the lithium precipitation mother liquor is adsorbed, more than 90% of the lithium in the lithium precipitation mother liquor is recovered and utilized. However, when only the lithium precipitation mother liquor (without mixing with the lithium extraction analysis solution) is directly used for treatment based on the same adsorption method, only about 40% of the lithium in the lithium precipitation mother liquor is recovered and utilized.

[0205] It can be seen that the lithium content in the mixed solution obtained by the lithium extraction method of the present invention is greatly reduced, and the recovery rate of lithium obtained by adsorption is much higher than the recovery rate of lithium obtained by directly adsorbing the lithium precipitating mother liquor. The quality of the analysis solution obtained by adsorption by the method of the present invention (lithium-sodium ratio, lithium-potassium ratio, etc.) is also higher than the quality of the analysis solution obtained by directly adsorbing the lithium precipitating mother liquor, and the overall lithium extraction efficiency is greatly improved.

[0206] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing lithium carbonate using a lithium-rich solution obtained by a lithium ion sieve adsorption method, characterized in that: The steps include: (1) transporting the salt lake brine to be treated to a multilayer adsorption tower provided with a lithium ion sieve adsorbent for lithium extraction, and performing decomposition using sulfuric acid as a decomposition liquid to obtain a sulfate solution, and performing concentration treatment to obtain an enriched sulfate solution; The multi-layer adsorption tower at least comprises: The main body has a hollow tower cavity, wherein the tower cavity has a water inlet and a water outlet; Adsorption dishes are arranged in the tower cavity at intervals along the height direction of the main body, and each of the adsorption dishes is filled with an adsorbent; A first water-permeable structure is arranged in the tower cavity and between two upper and lower adjacent layers of the adsorption dishes, wherein the first water-permeable structure has a water-permeable state that allows water to pass through, and a water-isolating state that restricts water from passing through; The first water-permeable structure comprises a first baffle and a second baffle which are stacked, and a plurality of water-permeable holes are arranged on the plate surfaces of the first baffle and the second baffle; The first partition can rotate around its own axis so that the water holes on the first partition and the water holes on the second partition overlap or stagger with each other; The first partition plate and the second partition plate are both arranged to be inclined relative to the horizontal plane, so that the lowest point and the highest point of the liquid level are formed between two adjacent first permeable structures; A liquid inlet and a liquid discharge port are provided at each of the lowest points of the liquid level, and a liquid discharge port is provided at each of the highest points of the liquid level; The adsorption dish is in a columnar structure, a first filter screen is arranged on the top surface of the adsorption dish, and a second filter screen is arranged on the bottom surface of the adsorption dish; (2) adjusting the pH value of the enriched sulfate solution to 11-12.5, collecting the liquid portion through solid-liquid separation to obtain a lithium-rich solution, and performing boron removal, calcium removal, magnesium removal, and manganese removal treatments on the lithium-rich solution; (3) contacting the lithium-rich liquid with a sodium-modified zeolite adsorbent to perform sodium ion adsorption treatment to obtain a low-sodium lithium-rich liquid and performing a concentration treatment; (4) adding excess sodium carbonate to the concentrated low-sodium lithium-rich solution and mixing, collecting the filter residue and the filtrate after solid-liquid separation to obtain a crude lithium carbonate product and a lithium precipitation mother liquor, respectively.

2. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 1, characterized in that: In the step (4), the sodium carbonate is controlled to be in excess of 10-30 wt%.

3. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 2, characterized in that: In the step (4), the mixing temperature of the low-sodium lithium-rich solution and the sodium carbonate is controlled to be 70-90°C.

4. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 3, characterized in that: The step (4) also includes a step of refining the crude lithium carbonate.

5. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 4, characterized in that: The refining step includes the step of mixing the crude lithium carbonate with water, and the step of collecting the refined lithium carbonate and the refined filtrate respectively through solid-liquid separation.

6. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 5, characterized in that: The step (4) further includes the step of purifying the refined lithium carbonate through a hydrogenation reaction to prepare battery-grade lithium carbonate; and / or the step of combining the refined filtrate with the lithium precipitation mother liquor.

7. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to any one of claims 1 to 6, characterized in that: The method further comprises the step of preparing lithium carbonate using the lithium precipitation mother solution, comprising the following steps: (a) mixing the lithium precipitation mother solution with the lithium extraction analysis solution to obtain a mixed solution; (b) passing the mixed liquid through an adsorbent for adsorption treatment; (c) After the adsorption is completed, the adsorbent is subjected to an analysis treatment, the obtained analysis solution is collected, and after lithium is precipitated by crystallization, a carbonation treatment is performed to obtain the desired lithium carbonate.

8. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 7, characterized in that: In the step (a), the volume ratio of the lithium precipitation mother solution to the lithium extraction analytical solution is such that the pH value of the obtained mixed solution is regulated to be between 7.5 and 10.0; and / or, In the step (a), the volume ratio of the lithium precipitation mother solution to the lithium extraction analytical solution is 1:1-1:20; and / or, In the step (b), the adsorbent includes a manganese-based, titanium-based, or manganese-titanium-based lithium ion sieve adsorbent; and / or, In the step (b), the flow rate of the mixed liquid is controlled to be 2-20 times the volume of the adsorbent per hour; and / or, In the step (c), the eluent used in the analytical treatment includes acid solution.

9. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 8, characterized in that: In the step (c), the eluent comprises an acid solution with a concentration of 0.01-1 mol / L.

10. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 9, characterized in that: In the step (c), the eluent comprises at least one of sulfuric acid, hydrochloric acid, nitric acid or oxalic acid solution with a concentration of 0.01-1 mol / L.

11. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 7, characterized in that: The step (c) further comprises the step of washing the adsorbent before the analytical treatment; and / or, The step (c) further comprises the step of mixing the tail liquid of the mixed liquid after adsorption treatment with the original brine of the salt lake and re-adsorbing the mixture; and / or, The step (c) also includes the step of circulating the obtained analytical solution to the step (1) to mix with the lithium precipitation mother solution for repeated adsorption.

12. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to any one of claims 1 to 6, characterized in that: The multilayer adsorption tower also includes a second water-permeable structure, which is arranged on the bottom surface of the adsorption dish and located on the side of the second filter screen facing away from the first filter screen. The second water-permeable structure has a water-permeable state that allows water to pass through, and a water-isolating state that restricts water from passing through.

13. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to any one of claims 1 to 6, characterized in that: In the step (3), the sodium-modified zeolite adsorbent is prepared by using analcime as raw material and subjecting it to a modification treatment with saturated sodium sulfate.

14. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 13, characterized in that: The modification treatment of the sodium-modified zeolite adsorbent is to boil the analcime in a saturated sodium sulfate solution for 2-4 hours.

15. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 14, characterized in that: The modification process is repeated 3-6 times, and the turbid liquid is poured off after each modification process is completed.

16. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 15, characterized in that: The usage ratio of the saturated sodium sulfate solution to analcime is 3-20 mL / g.

17. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 16, characterized in that The particle size of the analcime is 30-40 meshes.

18. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 17, characterized in that: In the step (3), the sodium ion adsorption treatment step includes the step of contacting the lithium-rich solution with the sodium-modified zeolite adsorbent at a flow rate of 1 to 5 times the adsorbent volume per hour.

19. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 18, characterized in that: The temperature of the sodium ion adsorption treatment step is 10-60° C. and the time is 2-5 hours.

20. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 19, characterized in that: The step (3) also includes a step of performing analytical treatment on the sodium-modified zeolite adsorbent after adsorption.

21. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 20, characterized in that: In the step (3), a solution having a pH of 1.5-2 and containing 0.05-0.3 mol / L lithium sulfate is used for analysis.

22. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 20, characterized in that: In the step (3), a lithium ion sieve analytical solution is used for analytical treatment.

23. The method for preparing lithium carbonate using lithium-rich solution obtained by lithium ion sieve adsorption method according to claim 22, characterized in that: In the step (3), the analytical treatment step includes the step of contacting the lithium ion sieve analytical solution with the adsorbed sodium-modified zeolite adsorbent at a flow rate of 5-10 times the adsorbent volume / hour, and the contact time is 0.5-1h.