A method for preparing ternary positive electrode materials for lithium-ion batteries by mass transfer gradient driving
In the preparation of ternary positive electrode materials of lithium ion batteries, lithium ions are introduced in the co-precipitation stage of nickel-cobalt manganese/aluminum salts and lithiation reactions are carried out using high-concentration lithium ion mass transfer drive, which solves the complex process and energy in the existing technology. The problem of high consumption and mixed cation discharge achieves the effect of simplifying the process and improving the performance of the material.
Patent Information
- Application Number
- CN202310304848.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-27
AI Technical Summary
The existing preparation methods of lithium-ion battery ternary cathode materials have complex processes, high energy consumption, high cost, and mixed cations, and it is difficult to control the synthesis conditions.
By introducing lithium ions in the co-precipitation stage of nickel-cobalt manganese/aluminum salt, high-concentration lithium ion mass transfer drives the lithiation reaction with the ternary precursor in the liquid phase, forming a ternary positive electrode material with poor crystallinity, and passing through Subsequent heat treatment improves crystallinity, simplifies the process and reduces the heat treatment temperature and time.
One-step synthesis of ternary cathode materials is realized, the process flow is simplified, energy consumption and cost are reduced, cation mixed discharge problems are avoided, and material performance is improved.
Smart Images

Figure CN116443947B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery positive electrode materials, and in particular relates to a method for preparing a lithium ion battery ternary positive electrode material by mass transfer gradient driving. Background Art
[0002] With the development of the times and science and technology, traditional fossil energy technology is unable to meet the growing energy demand. New energy technology is booming and is gradually replacing the dominant position of fossil energy. Among new energy technologies, energy storage is a particularly critical link, among which lithium-ion batteries have become the most widely used technology representative. Among the main components of lithium-ion batteries, positive electrode materials play the most critical role. In the past decade, ternary positive electrode materials (NCM / NCA) have been constantly replacing the market of LMO / LFP and have become the mainstream choice of lithium-ion battery chemical systems for electric passenger vehicles.
[0003] The existing preparation method of ternary positive electrode materials is mainly to synthesize the hydroxide / carbonate precursor of NCM / NCA by co-precipitation method, and then physically mix the lithium source and the precursor and sinter them at high temperature. First of all, the preparation process of this method is complicated. The precursor synthesized by co-precipitation needs to be aged, washed, and dried. The lithium source needs to be ground before mixing. The mixing of the precursor and the lithium source also takes a long time. Secondly, this method requires a long time of high-temperature reaction, and the high-nickel precursor also requires a pure oxygen atmosphere, which has high energy consumption and cost. During the high-temperature process, Ni with close radii 2+ and Li + The above problems often lead to the long process of preparing ternary cathode materials by existing methods, the difficult control of synthesis conditions, and high requirements on equipment.
[0004] CN113772748B discloses a method for preparing a positive electrode material for a lithium-ion battery, which uses a precursor containing a small amount of water as a raw material, adjusts the pH and adds an oxidizing lithium salt to carry out a lithium insertion reaction, which not only efficiently converts Ni 2+ Converted to Ni 3+ , and complete lithium insertion is achieved, so the obtained positive electrode material has good electrochemical performance. However, this method has the problems of expensive oxidative lithium salts and the need for additional preparation of precursors.
[0005] CN113745514B discloses a fluorine-doped and lithium silicate-coated lithium-rich manganese-based material, in which a precursor with a micron rod-like morphology is grown by hydrothermal reaction, but the lithium salt does not react with the precursor to be embedded during the hydrothermal reaction, and still needs to be subsequently dried and ground for high-temperature solid-phase reaction. This results in high energy consumption during the material synthesis process, and there is still high-temperature volatilization loss of the lithium salt.
[0006] The existing patent CN110380040B discloses a wet method for synthesizing lithium-doped lithium-ion battery ternary precursors, which replaces dry mixing by mixing lithium with the precursor in a solution, does not cause lithiation reaction, and requires the addition of a precipitant to precipitate lithium to avoid washing away lithium during the washing process. This method has a narrow application range, high production costs, and a still complicated process. Summary of the invention
[0007] In order to solve the above problems, the present invention provides a method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving.
[0008] In view of the above technical problems, the following solutions are proposed:
[0009] The present invention introduces lithium ions during the nickel-cobalt-manganese / aluminum salt coprecipitation stage, so that lithium is evenly distributed inside the formed ternary precursor, and driven by high-concentration lithium ion mass transfer, under certain temperature and pressure conditions, lithium ions and ternary precursors undergo a lithiation reaction in the liquid phase to form a ternary positive electrode material with poor crystallinity, at which point the lithiation reaction has been completed; its reaction principle is an ion exchange mechanism, and no dissolution-recrystallization process occurs, and the morphology of the ternary precursor is retained; the purpose of subsequent heat treatment is to increase the crystallinity of the ternary positive electrode material, so that the grains formed by the liquid phase reaction continue to grow, and improve the lithium ion diffusion kinetics. Therefore, the preparation method of the present invention has a short flow and a simple process, and can synthesize the ternary positive electrode material in one step, which greatly reduces the heat treatment temperature and time compared to the prior art.
[0010] Specifically, the present invention provides a method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving, comprising:
[0011] S1, preparing a soluble lithium salt solution, preparing a mixed metal salt solution of nickel salt, cobalt salt, and manganese salt and / or aluminum salt, and preparing an ammonia solution;
[0012] S2, preparing a reaction kettle bottom liquid and adding it to a reaction kettle, then flowing a soluble lithium salt solution, a mixed metal salt solution, and an ammonia solution into the reaction kettle bottom liquid in parallel, adding an alkali as a precipitant to the reaction kettle bottom liquid, controlling the pH value to react under stirring conditions, and obtaining slurry 1;
[0013] S3, heating the reactor to a certain temperature, continuing to stir the reaction, and obtaining slurry 2;
[0014] S4, performing solid-liquid separation on slurry 2 to obtain a solid and a lithium-containing mother liquor;
[0015] S5. After drying the obtained solid, heat-treat it in air or oxygen atmosphere to obtain the product.
[0016] In the present technical solution, the stirring reaction in step S3 is a hydrothermal reaction.
[0017] Preferably, in step S2, the pH value is controlled at 9-13; the reaction temperature is 30-80°C; the stirring speed is 60-400 rpm; and the reaction time is 1-9 h.
[0018] Preferably, in step S3, the certain temperature is 120-374°C.
[0019] Preferably, in step S3, the stirring speed is 60-400 rpm; and the reaction time is 4-20 h.
[0020] Preferably, the molar ratio of lithium in the soluble lithium salt to the total amount of metal in the mixed metal salt is 5-20:1.
[0021] Preferably, in step S5, the heat treatment temperature is 500-900° C. and the heat treatment time is 3-10 hours.
[0022] Preferably, in step S4, the solid-liquid separation is carried out by filtering, washing or centrifugal drying.
[0023] Preferably, in step S1, the preparation of the soluble lithium salt solution comprises dissolving the soluble lithium salt in water; the soluble lithium salt is at least one of lithium hydroxide, lithium acetate, lithium chloride and lithium nitrate; the lithium ion concentration in the soluble lithium salt is 2.5~20.0 mol / L, and more preferably 5~20.0 mol / L.
[0024] Preferably, in step S1, the preparation of a mixed metal salt solution of nickel salt, cobalt salt, manganese salt and / or aluminum salt comprises dissolving soluble nickel salt, cobalt salt, manganese salt and / or aluminum salt in water; the nickel salt, cobalt salt, manganese salt and / or aluminum salt is at least one of sulfate, acetate, halide or nitrate; and the total concentration of metal ions in the mixed metal salt solution is 0.5~2.5 mol / L.
[0025] Preferably, in step S1, the ammonia solution is prepared by mixing ammonia solution with water and adjusting the pH value to 10-11.5 by using a base; the concentration of the ammonia solution is 0.1-10.0 mol / L; and the base is at least one of sodium hydroxide, lithium hydroxide and potassium hydroxide.
[0026] Preferably, in step S2, the alkali is added in the form of a solid alkali or an aqueous alkali solution, and the alkali is at least one of sodium hydroxide, lithium hydroxide and potassium hydroxide.
[0027] Preferably, the molecular formula of the ternary positive electrode material is LiNi x Co y Mn 1-x-y-z Al zO2, wherein 0<x<1, 0<y<1, 0≤z≤0.4; further preferably 0.4≤x≤0.9, 0<y≤0.3, 0≤z≤0.3.
[0028] Optionally, in step S5, the drying is performed at 60-200° C. for 1-12 hours, and the purpose of drying is to remove moisture from the solid.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention introduces lithium ions in the wet process stage without affecting the morphology and structure of the ternary precursor, thereby achieving uniform mixing at the molecular level; the lithiation reaction is driven by mass transfer of high-concentration lithium ions to complete the synthesis of the ternary cathode material, and only a short heat treatment process is required to improve the crystallinity, thereby solving the problems of long process, difficult preparation, high energy consumption and cost of solid-phase sintering, uneven lithium mixing, and high equipment requirements in the prior art. The ternary cathode material in the present invention has been synthesized in the wet process stage, which effectively solves the problem of cation mixing caused by high-temperature sintering in the prior art and improves material performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The lithium-nickel mixed arrangement refinement results of the ternary positive electrode materials prepared in Example 1(a) and Comparative Example 1(b);
[0032] Figure 2 XRD spectrum and lithium insertion amount of the ternary positive electrode material prepared in Comparative Example 2;
[0033] Figure 3 This is a charge and discharge performance diagram of the ternary positive electrode material prepared in Comparative Example 2;
[0034] Figure 4 XRD spectrum and lithium insertion amount of the ternary positive electrode material after hydrothermal ion exchange described in Example 1;
[0035] Figure 5 The XRD pattern of the ternary cathode material after heat treatment described in Example 1;
[0036] Figure 6 The SEM morphology of the ternary cathode material prepared in Example 1;
[0037] Figure 7 The first cycle charge and discharge curve of the ternary cathode material prepared in Example 1;
[0038] Figure 8 This is a rate performance diagram of the ternary positive electrode material prepared in Example 1. DETAILED DESCRIPTION
[0039] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings, but the present invention is not limited to the following embodiments. Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0040] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0041] Example 1
[0042] A method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving comprises the following steps:
[0043] (1) Add 8.392 kg of lithium hydroxide monohydrate to 10 L of deionized water and stir until the solution is supersaturated to obtain solution A; add 2.182 kg of nickel sulfate hexahydrate, 0.309 kg of cobalt sulfate heptahydrate and 0.101 kg of manganese sulfate monohydrate to 10 L of deionized water and stir until they are completely dissolved to obtain solution B; mix 0.3 kg of ammonia water with 25 L of deionized water and adjust the pH value to 11 with sodium hydroxide to obtain solution C;
[0044] (2) Add 5 L of deionized water to the reactor and start heating and stirring;
[0045] (3) Solutions A to C were introduced into the reactor in parallel, sodium hydroxide was added to control the pH to 10, and the mixture was stirred at 60 °C and 300 rpm for 3 h to obtain slurry D.
[0046] (4) The reactor was heated to 200 °C and stirred at 300 rpm for 9 h to obtain slurry E. This step was a hydrothermal reaction. In order to achieve a temperature of 200 °C for the liquid in the reactor, this step needed to be carried out under a certain pressure.
[0047] (5) The slurry E is washed and filtered to obtain a solid powder F, which is then dried at 60°C for 12 h. The dried solid powder F is then heat treated at 700°C for 5 h in an oxygen atmosphere to obtain LiNi 0.83 Co 0.11 Mn 0.06 O2.
[0048] The XRD pattern and lithium insertion amount of fixed powder F are as follows Figure 4 As shown, from Figure 4 It can be seen that after ion exchange through hydrothermal treatment, the ternary cathode material basically achieves full lithium insertion, and the ternary material is synthesized. The XRD pattern after heat treatment is as follows: Figure 5 As shown, the heat treatment improves the crystallization degree of the ternary cathode material, and the XRD pattern is refined. Figure 1 (a) is shown. The SEM image of the positive electrode material obtained after heat treatment is shown Figure 6 As shown, it can be seen that the obtained positive electrode material has a secondary spherical morphology obtained by agglomeration of primary particles.
[0049] The obtained positive electrode material was mixed with a conductive agent and PVDF, slurried and coated on aluminum foil. A lithium sheet was used as the negative electrode and EC-DMC-EMC (1:1:1, vol%) was used as the electrolyte to assemble a CR2032 button half-cell to test the electrochemical properties of the positive electrode material.
[0050] The first cycle charge and discharge curve of the assembled battery is as follows: Figure 7 As shown in the figure, the rate performance diagram is as follows Figure 8 shown.
[0051] Comparative Example 1
[0052] The method of preparing a ternary positive electrode material for a lithium-ion battery by a high-temperature solid phase method after mixing a precursor with lithium comprises the following steps:
[0053] (1) Put 0.925 kg Ni 0.83 Co 0.11 Mn 0.06 The (OH)2 precursor and 8.392 kg of lithium hydroxide monohydrate are uniformly mixed in a mixer to obtain a mixture A;
[0054] (2) Mixture A is placed in a pure oxygen atmosphere and sintered at 780°C for 15 hours to obtain LiNi 0.83 Co 0.11 Mn 0.06 O2. The lithium-nickel mixed arrangement refinement results of the XRD pattern of the prepared positive electrode material are as follows Figure 1 (b) Comparison Figure 1 As can be seen from (a) and 1 (b), the Li / Ni mixed arrangement of the ternary positive electrode material prepared in Example 1 is significantly improved compared with that in Comparative Example 1.
[0055] Comparative Example 2
[0056] The aged precursor is subjected to heat treatment with lithium salt water to prepare a ternary positive electrode material for a lithium ion battery, comprising the following steps:
[0057] (1) Add 2.182 kg of nickel sulfate hexahydrate, 0.309 kg of cobalt sulfate heptahydrate and 0.101 kg of manganese sulfate monohydrate into 10 L of deionized water and stir until completely dissolved to obtain solution A; mix 0.3 kg of ammonia water with 25 L of deionized water and adjust the pH value to 11 with sodium hydroxide to obtain solution B;
[0058] (2) Add 5 L of deionized water to the reactor and start heating and stirring;
[0059] (3) Solutions A and B were introduced into the reactor in parallel, sodium hydroxide was added to control the pH to 10, and the mixture was stirred at 60°C and 300 rpm for 3 h to obtain slurry C.
[0060] (4) The slurry C is maintained at the temperature in (3), aged for 24 h under stirring, washed, filtered, and dried with air to obtain Ni 0.83 Co 0.11 Mn 0.06 (OH)2 precursor;
[0061] (5) The obtained Ni 0.83 Co 0.11 Mn 0.06 The (OH)2 precursor and 8.392 kg of lithium hydroxide monohydrate were added to the hydrothermal reactor, and 50 L of deionized water was injected;
[0062] (6) The reactor was heated to 200 °C and stirred at 300 rpm for 9 h to obtain slurry D.
[0063] (7) Wash the slurry D, filter it, and dry it to obtain a solid powder E. Dry the solid powder E at 60°C for 12 h, and then heat treat the dried solid powder E at 700°C for 5 h in an oxygen atmosphere to obtain Li 0.22 H 0.78 Ni 0.83 Co 0.11 Mn 0.06 O2. The XRD pattern and lithium insertion amount of the prepared positive electrode material are shown in Figure 2 As shown, from Figure 2 It can be seen that this method only achieves a small amount of lithium insertion, and the electrochemical properties of the material are as follows Figure 3 As shown, due to the less lithium insertion, the charge and discharge capacity is also obviously low.
[0064] Example 2
[0065] A method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving comprises the following steps:
[0066] (1) Add 4.196 kg of lithium hydroxide monohydrate to 10 L of deionized water and stir until supersaturated to obtain solution A; add 1.742 kg of nickel acetate tetrahydrate, 0.124 kg of cobalt acetate tetrahydrate and 0.613 kg of manganese acetate tetrahydrate to 10 L of deionized water and stir until completely dissolved to obtain solution B; mix 0.5 kg of ammonia water with 20 L of deionized water and adjust the pH value to 11.5 with sodium hydroxide to obtain solution C;
[0067] (2) Add 10 L of deionized water to the reactor and start heating and stirring;
[0068] (3) Solutions A to C were introduced into the reactor in parallel, and sodium hydroxide was added to control the pH to 10.5. The mixture was stirred at 40 °C and 200 rpm for 5 h to obtain slurry D.
[0069] (4) The reactor was heated to 220°C and stirred at 300 rpm for 6 h to obtain slurry E.
[0070] (5) The slurry E is washed and filtered to obtain a solid powder F; the solid powder F is dried at 60 °C for 12 h, and then the dried solid powder F is heat treated at 720 °C for 3 h in an oxygen atmosphere to obtain LiNi 0.70 Co 0.05 Mn 0.25 O2.
[0071] Example 3
[0072] A method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving comprises the following steps:
[0073] (1) Add 4.196 kg of lithium hydroxide monohydrate to 5 L of deionized water and stir until supersaturated to obtain solution A; add 1.890 kg of nickel nitrate hexahydrate, 0.233 kg of cobalt nitrate hexahydrate and 0.775 kg of manganese nitrate hexahydrate to 10 L of deionized water and stir until completely dissolved to obtain solution B; mix 0.25 kg of ammonia water with 25 L of deionized water and adjust the pH value to 11.5 with sodium hydroxide to obtain solution C;
[0074] (2) Add 10 L of deionized water to the reactor and start heating and stirring;
[0075] (3) Solutions A to C were introduced into the reactor in parallel, sodium hydroxide was added to control the pH to 9, and the mixture was stirred at 70 °C and 400 rpm for 4 h to obtain slurry D.
[0076] (4) The reactor was heated to 190 °C and stirred at 400 rpm for 6 h to obtain slurry E.
[0077] (5) The slurry E is washed and filtered to obtain a solid powder F; the solid powder F is dried at 60°C for 12 h, and then the dried solid powder F is heat treated at 750°C for 6 h in an oxygen atmosphere to obtain LiNi 0.65 Co 0.08 Mn 0.27 O2.
[0078] Example 4
[0079] A method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving comprises the following steps:
[0080] (1) Add 2.098 kg of lithium hydroxide monohydrate to 5 L of deionized water and stir until supersaturated to obtain solution A; add 1.188 kg of nickel chloride hexahydrate, 0.476 kg of cobalt chloride hexahydrate and 0.594 kg of manganese chloride tetrahydrate to 15 L of deionized water and stir until completely dissolved to obtain solution B; mix 0.35 kg of ammonia water with 20 L of deionized water and adjust the pH value to 10.5 with sodium hydroxide to obtain solution C;
[0081] (2) Add 10 L of deionized water to the reactor and start heating and stirring;
[0082] (3) Solutions A to C were introduced into the reactor in parallel, sodium hydroxide was added to control the pH to 13, and the mixture was stirred at 50 °C and 300 rpm for 4 h to obtain slurry D.
[0083] (4) The reactor was heated to 240 °C and stirred at 300 rpm for 8 h to obtain slurry E.
[0084] (5) The slurry E is washed and filtered to obtain a solid powder F; the solid powder F is dried at 60°C for 12 h, and then the dried solid powder F is heat treated at 850°C for 3 h in an air atmosphere to obtain LiNi 0.5 Co 0.2 Mn 0.3 O2.
[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing ternary positive electrode materials for lithium-ion batteries driven by mass transfer gradient, It is characterized in that include: S1, preparing a soluble lithium salt solution, preparing a mixed metal salt solution of nickel salt, cobalt salt, and manganese salt and / or aluminum salt, and preparing an ammonia solution; S2, preparing a reaction kettle bottom liquid and adding it to a reaction kettle, then flowing a soluble lithium salt solution, a mixed metal salt solution, and an ammonia solution into the reaction kettle bottom liquid in parallel, adding a base as a precipitant to the reaction kettle bottom liquid, controlling the pH value to react under stirring conditions to obtain slurry 1; the reaction temperature is 30-80° C.; the molar ratio of lithium in the soluble lithium salt to the total amount of metal in the mixed metal salt is 5-20:1; S3, heating the reactor to a certain temperature, continuing the stirring reaction, and obtaining slurry 2; the certain temperature is 120-240° C.; the stirring reaction is a hydrothermal reaction; S4, performing solid-liquid separation on slurry 2 to obtain a solid and a lithium-containing mother liquor; S5. After drying the obtained solid, heat-treating it in air or oxygen atmosphere to obtain the ternary positive electrode material having the molecular formula of LiNi x Co y Mn 1-x-y-z Al z O 2 , where 0.65≤x≤0.9, 0<y≤0.3, 0≤z≤0.
3.
2. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to claim 1, It is characterized in that In step S2, the pH value is controlled at 9-13; the stirring speed is 60-400 rpm; and the reaction time is 1-9 h.
3. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to claim 1, It is characterized in that In step S3, the stirring speed is 60-400 rpm; and the reaction time is 4-20 h.
4. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to any one of claims 1 to 3, It is characterized in that In step S5, the heat treatment temperature is 500-900° C. and the heat treatment time is 3-10 hours.
5. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to any one of claims 1 to 3, It is characterized in that In step S4, the solid-liquid separation is carried out by filtering, washing or centrifugal drying.
6. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to any one of claims 1 to 3, It is characterized in that In step S1, the preparation of the soluble lithium salt solution includes dissolving the soluble lithium salt in water; the soluble lithium salt is at least one of lithium hydroxide, lithium acetate, lithium chloride and lithium nitrate; and the lithium ion concentration in the soluble lithium salt is 2.5-20.0 mol / L.
7. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to any one of claims 1 to 3, It is characterized in that In step S1, the preparation of a mixed metal salt solution of nickel salt, cobalt salt, manganese salt and / or aluminum salt comprises dissolving soluble nickel salt, cobalt salt, manganese salt and / or aluminum salt in water; the nickel salt, cobalt salt, manganese salt and / or aluminum salt is at least one of sulfate, acetate, halide or nitrate; and the total concentration of metal ions in the mixed metal salt solution is 0.5-2.5 mol / L.
8. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to any one of claims 1 to 3, It is characterized in that In step S1, the ammonia solution is prepared by mixing ammonia solution with water and adjusting the pH value to 10-11.5 by adding a base; the concentration of the ammonia solution is 0.1-10.0 mol / L; and the base is at least one of sodium hydroxide, lithium hydroxide and potassium hydroxide.
9. The method for preparing a ternary positive electrode material for a lithium-ion battery by mass transfer gradient driving according to any one of claims 1 to 3, It is characterized in that In step S2, the alkali is added in the form of a solid alkali or an aqueous solution of the alkali; the alkali is at least one of sodium hydroxide, lithium hydroxide and potassium hydroxide.