A hybrid coordination polymerization metal organic framework based anti-aging agent, modified asphalt and preparation method
By mixing metal organic frame materials with different pores, specific surface areas and metal points, adding nano powder to the asphalt to hinder the oxidative aging reaction, the problem of asphalt aging in the existing technology is solved, and the high-temperature performance improvement and road of asphalt is achieved Improve performance.
Patent Information
- Application Number
- CN202310528280.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-11
AI Technical Summary
The prior art is difficult to effectively inhibit the chemical oxidation reaction between asphalt and oxygen, resulting in asphalt aging, and the quality of existing anti-aging agents is uneven, making it difficult to achieve long-lived and high-durability road surface requirements.
Using a hybrid coordination polymeric metal organic frame anti-aging agent, by mixing metal organic frame materials with different pores, specific surface areas and metal points, synergistically, adding metal organic frame nanopowder to the matrix asphalt to hinder the oxidative aging reaction. .
It significantly delays the aging process of asphalt, improves the high-temperature performance of asphalt, reduces the volatility of light components and the formation of sulfoxide groups, and improves the construction ease and road performance of asphalt.
Smart Images

Figure CN116444815B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hybrid coordination polymerization type metal organic framework anti-aging agent, modified asphalt and a preparation method, belonging to the technical field of pavement asphalt materials. Background Art
[0002] Whether it is during the high-temperature paving and mixing in the construction stage or the long-term service stage in the later stage, asphalt will undergo chemical oxidation reaction with oxygen in the atmosphere, causing it to become hard and brittle. This is mainly because oxygen-containing polar groups are introduced into the surface of asphalt molecules, which enhances the interaction between molecules. At the same time, the oxidation reaction will also cause aromatization of asphalt molecules. These changes in chemical composition will increase the hardness of asphalt. With the increasing requirements for low carbon and environmental protection, the industry has an increasingly urgent demand for long-life and high-durability pavements. At present, it is common to add oily substances to aged asphalt to achieve asphalt regeneration, but aromatized substances still exist in asphalt, and there are still large differences in the properties of asphalt softened with light oil and new asphalt. In addition, the quality of existing anti-aging agents is uneven, and most of them are derived from a specific chemical substance that is also used in other fields. It is difficult to inhibit the occurrence of asphalt oxidation reactions from the source. Therefore, adding substances that can inhibit its reaction with oxygen to asphalt has become a new research direction.
[0003] Metal-organic frameworks (MOFs), also known as porous coordination polymers (PCPs), are a type of ordered porous crystalline nanomaterials formed by metal ions or metal cluster units and organic ligands through coordination bonds. As a new type of crystalline porous nanomaterial, MOFs have a periodic network structure and continuously adjustable pore size, which greatly fills the gap in pore size between micropores (zeolites) and mesopores (silica); at the same time, the ultra-high porosity and specific surface area (>6000m 2 / g), which makes it have good application prospects. MOFs are highly designable and tailorable, and their structure can be regulated at the molecular scale.
[0004] The use of a single MOFs material can only selectively adsorb specific gases and specific components in asphalt, and has limited anti-aging effects on asphalt. Currently, no research has been found to mix multiple MOFs materials to utilize the coupling effects of different porosities, specific surface areas, and metal sites to jointly delay asphalt aging. Summary of the invention
[0005] The purpose of the present invention is to provide an anti-aging agent based on a mixed coordination polymerization metal organic framework, a modified asphalt and a preparation method to achieve the effect of delaying the aging of base asphalt and solve the shortcomings of the prior art.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The invention provides a hybrid coordination polymerization type metal organic framework anti-aging agent, which comprises the following raw materials: 4 parts by weight of terephthalic acid, 10 parts by weight of dehydrated zinc acetate, 2000 parts by weight of N,N-dimethylformamide, 100 parts by weight of triethylamine, 2.5 parts by weight of cobalt nitrate hexahydrate, 10 parts by weight of 2-methylimidazole, 1250 parts by weight of anhydrous methanol, 1 part by weight of zirconium tetrachloride and 500 parts by weight of glacial acetic acid.
[0008] The present invention also provides a modified asphalt, comprising a mixed coordination polymerization type metal organic framework anti-aging agent and a base asphalt.
[0009] Preferably, the base asphalt is 70# road petroleum asphalt.
[0010] The present invention also provides a method for preparing a hybrid coordination polymerization type metal organic framework anti-aging agent, comprising the following steps:
[0011] Step 1, mixing 3 parts by weight of terephthalic acid, 10 parts by weight of dehydrated zinc acetate, 400 parts by weight of N,N-dimethylformamide and 100 parts by weight of triethylamine;
[0012] Step 2, centrifuging the mixture obtained in step 1 to separate solid crystals;
[0013] Step 3, drying and grinding the solid crystals obtained in step 2 into powder to obtain a white powder 1;
[0014] Step 4, mixing 2.5 parts by weight of cobalt nitrate hexahydrate with 625 parts by weight of anhydrous methanol;
[0015] Step 5, mixing 10 parts by weight of 2-methylimidazole with 625 parts by weight of anhydrous methanol;
[0016] Step 6, mixing the liquids obtained in step 4 and step 5, and subjecting the mixture to ultrasonic vibration;
[0017] Step 7, centrifuging the liquid obtained in step 6 to separate solid crystals;
[0018] Step 8, drying and grinding the solid crystals obtained in step 7 into powder to obtain purple powder 2;
[0019] Step 9, mixing 1 part by weight of zirconium tetrachloride with 800 parts by weight of N,N-dimethylformamide;
[0020] Step 10, mixing 1 part by weight of terephthalic acid with 800 parts by weight of N,N-dimethylformamide;
[0021] Step 11, mixing the liquids obtained in step 9 and step 10;
[0022] Step 12, adding 500 parts by weight of glacial acetic acid to the liquid obtained in step 11 and mixing;
[0023] Step 13, sealing and heating the solution obtained in step 12 for 48 hours;
[0024] Step 14, centrifuging the liquid obtained in step 13 to separate solid crystals;
[0025] Step 15, drying and grinding the solid crystals obtained in step 14 into powder to obtain white powder three;
[0026] Step 16, mixing and grinding the white powder 1, the purple powder 2 and the white powder 3 in a mass ratio of 2:1:1 to obtain a hybrid coordination polymerization-type metal-organic framework anti-aging agent.
[0027] Preferably, in step 1, the added substances are mixed and stirred at a speed of 300 rpm for 2.5 hours by a magnetic stirrer.
[0028] Preferably, in step 2, step 7 and step 14, a centrifuge is used to centrifuge at a rate of 6000 rpm for 20 min; in step 9 and step 10, stirring is performed at 800 rpm for 20 min; in step 11 and step 12, stirring is performed at 800 rpm for 10 min.
[0029] The present invention also provides a method for preparing modified asphalt, comprising the steps of:
[0030] Step 101, weighing a base asphalt, heating it to a molten state, stirring it for 10-20 minutes, and then keeping it warm to 120-150° C., adding a 1% amount of a hybrid coordination polymeric metal organic framework antioxidant prepared by the preparation method of a hybrid coordination polymeric metal organic framework antioxidant, stirring it for 5-15 minutes, and then shearing it, wherein the speed of the shearing machine during the shearing process is 3000 rpm, and the shearing time is 30 minutes;
[0031] Step 102, placing the asphalt in an oven at 160°C and leaving it to stand for 5 minutes to obtain a hybrid coordination polymerization metal organic framework modified asphalt.
[0032] Beneficial effects: The benefits and indicators achieved by the present invention. The present invention mixes three metal organic framework materials with different pores, specific surface areas and metal sites, and utilizes the synergistic effect and complementary advantages of multiple MOFs materials to achieve anti-aging effects, which are applied in the road field.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. Mix multiple metal organic framework materials to make up for the shortcomings of a single material due to differences in pores, specific surface areas, metal sites, etc. A single metal organic framework material can only directional adsorb specific material components, and its application and promotion are limited. The synergistic effect of different pore sizes, specific surface areas and different metal sites can effectively adsorb a variety of aging components in asphalt and prevent the oxidation and aging of asphalt.
[0035] 2. In the present invention, by adding mixed metal organic framework nano powder to the base asphalt, the high temperature performance of the asphalt is significantly improved. The prepared modified asphalt has a greater viscosity decay amplitude than the base asphalt as the temperature increases, has a higher viscosity at low temperatures, and is easy to flow at high temperatures, and has good construction and workability.
[0036] 3. In the present invention, under high temperature conditions, the mass loss of modified asphalt is slower than that of base asphalt, that is, under high temperature, the volatilization of light components is slower than that of base asphalt. The addition of hybrid metal organic framework material has a certain inhibitory effect on the volatilization of light components in asphalt.
[0037] 4. In the present invention, by adding a very small amount of hybrid metal organic framework powder to the base asphalt, the mass of the asphalt after aging is significantly reduced, the generation of sulfoxide groups (S=O) is significantly reduced, the oxidation reaction of the asphalt is weakened, and the anti-aging effect is obvious. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is the appearance of a mixed coordination polymer metal organic framework antioxidant
[0039] Figure 2 This is the transmission electron microscopy (TEM) test result of the mixed coordination polymeric metal organic framework anti-aging agent;
[0040] Figure 3 This is the scanning electron microscope (SEM) test result of the mixed coordination polymer metal organic framework anti-aging agent;
[0041] Figure 4 It is the thermogravimetric analysis (TGA) result of the mixed coordination polymeric metal organic framework antioxidant;
[0042] Figure 5 It is the viscosity-temperature variation curve of base asphalt and modified asphalt;
[0043] Figure 6 It is the thermogravimetric analysis (TGA) result of base asphalt and modified asphalt.
[0044] Figure 7 This is the surface morphology of base asphalt and modified asphalt after aging;
[0045] Figure 8 It is the infrared spectra (FTIR) of base asphalt and modified asphalt before and after aging; DETAILED DESCRIPTION
[0046] See also Figure 1-8 The embodiment of the present invention provides a hybrid coordination polymerization metal organic framework anti-aging agent, the raw materials of which include: terephthalic acid (4 parts by weight), dehydrated zinc acetate (10 parts by weight), N,N-dimethylformamide (2000 parts by weight), triethylamine (100 parts by weight), cobalt nitrate hexahydrate (2.5 parts by weight), 2-methylimidazole (10 parts by weight), anhydrous methanol (1250 parts by weight), zirconium tetrachloride (1 part by weight), and glacial acetic acid (500 parts by weight).
[0047] A modified asphalt comprises the above-mentioned hybrid coordination polymerized metal organic framework anti-aging agent and base asphalt. The amount of the hybrid coordination polymerized metal organic framework anti-aging agent is 1% of the base asphalt.
[0048] The preparation method of the hybrid coordination polymerization type metal organic framework modified asphalt comprises the following steps:
[0049] Step 1, 3 parts by weight of terephthalic acid and 10 parts by weight of dehydrated zinc acetate are charged into a reaction container;
[0050] Step 2, adding 400 parts by weight of N,N-dimethylformamide to the container of step 1;
[0051] Step 3, adding 100 parts by weight of triethylamine to the container of step 1;
[0052] Step 4, at room temperature, the substances added in steps 1-3 in the reaction container were mixed and stirred at 300 rpm for 2.5 hours using a magnetic stirrer, and the liquid was poured into a 50 ml centrifuge tube;
[0053] Step 5: Use a centrifuge to centrifuge at a rate of 6000 rpm for 20 minutes to separate the solid crystals to the bottom of the centrifuge tube in step 4, and filter to obtain the solid crystals.
[0054] Step 6, drying the solid crystals obtained in step 5 in an oven at 60° C. for 24 h, and grinding them into powder using a mortar to obtain white powder 1;
[0055] Step 7, adding 2.5 parts by weight of cobalt nitrate hexahydrate into a reaction container;
[0056] Step 8, adding 625 parts by weight of anhydrous methanol to the container of step 7;
[0057] Step 9, charging 10 parts by weight of 2-methylimidazole into a reaction container;
[0058] Step 10, adding 625 parts by weight of anhydrous methanol into the container of step 9.
[0059] Step 11, mixing the liquids obtained in step 8 and step 10, using an ultrasonic material disperser and an intelligent constant temperature bath,
[0060] The ultrasonic vibration was controlled at 10°C for 30 min, with a power of 30%, vibration for 2 s, and pause for 2 s.
[0061] Step 12, pour the liquid obtained in step 11 into a 50 ml centrifuge tube, use a centrifuge at 6000 rpm for 20 minutes to separate the solid crystals to the bottom of the centrifuge tube, and filter to obtain the solid crystals.
[0062] Step 13, drying the solid crystals obtained in step 12 in an oven at 60° C. for 24 h, and grinding them into powder using a mortar to obtain purple powder 2;
[0063] Step 14, placing 1 part by weight of zirconium tetrachloride into a reaction container;
[0064] Step 15, add 800 parts by weight of N,N-dimethylformamide to the container of step 14, and stir at 800 rpm for 20 min.
[0065] A clear solution was obtained.
[0066] Step 16, adding 1 part by weight of terephthalic acid into a reaction container;
[0067] Step 17, add 800 parts by weight of N,N-dimethylformamide to the container of step 16, and stir at 800 rpm for 20 min.
[0068] A clear solution was obtained.
[0069] Step 18, mixing the clear solutions obtained in step 15 and step 17, and stirring at 800 rpm for 10 min;
[0070] Step 19, adding 500 parts by weight of glacial acetic acid to the solution in step 18, stirring at 800 rpm for 10 min to obtain a clear solution.
[0071] Step 20, placing the clarified solution obtained in step 19 in a sealed oven at 60° C. and heating for 48 hours to obtain a white liquid;
[0072] Step 21, pour the liquid obtained in step 20 into a 50 ml centrifuge tube, use a centrifuge at a rate of 6000 rpm for 20 minutes to separate the solid crystals to the bottom of the centrifuge tube, and filter to obtain the solid crystals.
[0073] Step 22, drying the solid crystals obtained in step 21 in an oven at 60° C. for 24 h, and grinding them into powder using a mortar to obtain white powder 3;
[0074] Step 23, mixing and grinding the white powder 1 obtained in step 6, the purple powder 2 obtained in step 12, and the white powder 3 obtained in step 22 in a mass ratio of 2:1:1 to obtain a lavender mixed powder 4.
[0075] Step 24, weigh 500g of base asphalt, heat it to a molten state, stir it for 10-20min, and then keep it warm to 120-150°C, add 1% of the lavender powder obtained in step 23, stir it for 5-15min, and then shear it. During the shearing process, the speed of the shearing machine is 3000rpm and the shearing time is 30min.
[0076] Step 25, after the shearing is completed, the asphalt is placed in a 160° C. oven and allowed to stand for 5 minutes to obtain a hybrid coordination polymerization type metal organic framework modified asphalt.
[0077] The performance of hybrid coordination polymerization metal-organic framework modified asphalt binder was tested.
[0078]
Brown viscosity test
[0079] Test methods and contents:
[0080] The American Brookfield DV2 viscometer was used. Four test conditions were set at 100°C, 110°C, 120°C and 130°C, and the corresponding speeds were 10PPM, 50PPM, 100PPM and 200PPM, respectively. The test results are shown in Table 1:
[0081] Table 1 Test results
[0082]
[0083] From the results in Table 1, we can see that:
[0084] After adding 1% MOF-5 powder, the viscosity of the modified asphalt was significantly improved compared with the base asphalt, increasing by 20.45%, 19.35%, 19.34% and 16.61% at 100℃, 110℃, 120℃ and 130℃ respectively. The addition of MOF-5 powder can significantly improve the viscosity of asphalt.
[0085] By drawing the viscosity-temperature curve, it can be seen that as the temperature increases, the viscosity decay of MOF-5 modified asphalt is greater than that of the base asphalt, indicating that the viscosity of modified asphalt decreases faster with temperature, has a higher viscosity at low temperatures, and is easy to flow at high temperatures, making it suitable for construction. For modified asphalt, it is generally required that its viscosity value at 135°C is not greater than 3000mPa·s to ensure that the modified asphalt has good construction and workability. In this experiment, when the temperature reached 130°C, the viscosity of the modified asphalt was far less than 3000mPa·s, meeting the requirements.
[0086]
Thermogravimetric analysis
[0087] TGA was used to analyze the volatilization of light components in the base asphalt and MOF-5 modified asphalt under heating conditions. The two asphalts were heated from 30°C to 750°C in a N2 atmosphere at a heating rate of 10°C / min. They were kept at 750°C for 30 minutes, and then air was introduced and then kept for another 30 minutes. The test results are as follows:
[0088] The mass loss of modified asphalt with 1% MOF-5 powder after 300°C is slower than that of base asphalt, so MOF-5 powder has a certain inhibitory effect on the volatilization of light components of asphalt at high temperatures.
[0089]
Short-term aging and long-term aging tests
[0090] Test methods and contents:
[0091] According to the specification "Test Procedure for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011), two plates of base asphalt and one plate of 1% MOF-5 modified asphalt were subjected to short-term aging using the thin film oven test (TFOT), with the temperature set at 163°C and the time controlled at 5h. Subsequently, three plates of asphalt were subjected to a pressure aging test (PAV), with the temperature set at 100°C, the pressure at 2.1MPa, and the time at 24h.
[0092] Test results:
[0093] According to the specification, the mass of 2 plates of base asphalt and 1 plate of MOF-5 modified asphalt after short-term aging and long-term aging was weighed and calculated, and the results were as follows: Table 2
[0094] Table 2 Quality changes after aging
[0095] Material Base asphalt 1 Base Asphalt 2 1% MOF-5 modified asphalt <![CDATA[Empty plate mass m0 (g)]]> 136.6623 137.4986 136.6204 <![CDATA[Total mass m1 (g) after adding asphalt]]> 201.3974 198.8193 209.4667 <![CDATA[Total mass m2 (g) after short-term aging]]> 201.3551 198.7784 209.4454 <![CDATA[Total mass m3 (g) after long-term aging]]> 201.6620 199.0806 209.7289 Quality change after short-term aging (%) -0.065343222 -0.066698521 -0.029239646 Quality change after long-term aging (%) 0.474395914 0.493147824 0.389289392
[0096] The quality change after short-term aging is calculated according to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011):
[0097]
[0098] Where: L T —Change in heating mass of sample film (%)
[0099] m0—mass of sample dish (g)
[0100] m1—Total mass of sample dish and sample before heating in film oven (g)
[0101] m2—Total mass of sample dish and sample after heating in film oven (g)
[0102] Long-term aging quality change is calculated according to the following formula:
[0103]
[0104] Where: m3—total mass of sample dish and sample after pressure aging (g)
[0105] The calculation shows that the mass of the two base asphalts decreased by 0.0653% and 0.0667% respectively after short-term aging, with an average value of 0.0660% (the coefficient of variation was 1.45, which met the precision requirements), while the mass of 1% MOF-5 modified asphalt only decreased by 0.0292% after short-term aging, indicating that under the condition of 163℃ for 5h, the volatilization of light components in the modified asphalt was relatively small. The mass of the two base asphalts increased by 0.4744% and 0.4931% respectively after long-term aging (the coefficient of variation was 2.74, which met the precision requirements), while the mass of 1% MOF-5 modified asphalt only increased by 0.3893%. PAV simulates thermal oxidative aging, and the mass change comes from the volatilization of light components on the one hand, and the combination of oxygen atoms in the air with asphalt molecules on the other. The increase in mass indicates that the amount of oxygen atoms entering the asphalt system is greater than the volatilization of light components, while the increase in MOF-5 modified asphalt is smaller, indicating that oxygen reacts less with asphalt, that is, the addition of MOF-5 powder has a certain inhibitory effect on the oxidation of asphalt.
[0106]
FTIR (Fourier Transform Infrared Spectroscopy) Test
[0107] Fourier transform infrared spectroscopy (FTIR) was used to test the functional groups of base asphalt and modified asphalt before and after aging. The test results are as follows:
[0108] (1) 3650-3100cm -1At the position of the OH stretching vibration peak, the change patterns of the base asphalt and the modified asphalt are roughly the same, and both are reduced to a certain extent. Hydrogen bonding occurs between hydrogen connected to an electronegative atom (such as O or N) and another electronegative atom or electron-rich center. -OH is one of the main sources of hydrogen bonds in asphalt. Although the concentration of -OH is very low, its contribution to the properties of asphalt is very important. Phenols and alcohols in asphalt contain -OH. During the aging process, the weakening of the OH stretching vibration peak also means the loss of light components (saturated components and aromatic components) in the asphalt.
[0109] (2) at 1040 cm -1 At the left and right positions, the content of sulfoxide groups is: aged base asphalt > aged modified asphalt > unaged base asphalt > unaged modified asphalt. This shows that the addition of MOF-5 has a certain effect on the anti-oxidation of asphalt, whether before or after aging.
[0110] The hybrid polymeric metal-organic framework material used in the present invention has a wide source of raw materials, is simple to synthesize, and has a low cost; the present invention uses the hybrid polymeric metal-organic framework nanomaterial as a modifier to delay asphalt aging with very small dosage, and the modification effect is obvious; the modified asphalt based on the hybrid coordinated polymeric metal-organic framework anti-aging agent in the present invention has significantly improved high-temperature performance, good construction and workability, and excellent road performance.
Claims
1. A method for preparing a hybrid coordination polymerization metal organic framework anti-aging agent, It is characterized in that The hybrid coordination polymerization metal organic framework anti-aging agent comprises the following raw materials: 4 parts by weight of terephthalic acid, 10 parts by weight of dehydrated zinc acetate, 2000 parts by weight of N,N-dimethylformamide, 100 parts by weight of triethylamine, 2.5 parts by weight of cobalt nitrate hexahydrate, 10 parts by weight of 2-methylimidazole, 1250 parts by weight of anhydrous methanol, 1 part by weight of zirconium tetrachloride and 500 parts by weight of glacial acetic acid; The preparation method comprises the following steps: Step 1, mixing 3 parts by weight of terephthalic acid, 10 parts by weight of dehydrated zinc acetate, 400 parts by weight of N,N-dimethylformamide and 100 parts by weight of triethylamine; Step 2, centrifuging the mixture obtained in step 1 to separate solid crystals; Step 3, drying and grinding the solid crystals obtained in step 2 into powder to obtain a white powder 1; Step 4, mixing 2.5 parts by weight of cobalt nitrate hexahydrate with 625 parts by weight of anhydrous methanol; Step 5, mixing 10 parts by weight of 2-methylimidazole with 625 parts by weight of anhydrous methanol; Step 6, mixing the liquids obtained in step 4 and step 5, and subjecting the mixture to ultrasonic vibration; Step 7, centrifuging the liquid obtained in step 6 to separate solid crystals; Step 8, drying and grinding the solid crystals obtained in step 7 into powder to obtain purple powder 2; Step 9, mixing 1 part by weight of zirconium tetrachloride with 800 parts by weight of N,N-dimethylformamide; Step 10, mixing 1 part by weight of terephthalic acid with 800 parts by weight of N,N-dimethylformamide; Step 11, mixing the liquids obtained in step 9 and step 10; Step 12, adding 500 parts by weight of glacial acetic acid to the liquid obtained in step 11 and mixing; Step 13, heating the solution obtained in step 12 for 48 hours; Step 14, centrifuging the liquid obtained in step 13 to separate solid crystals; Step 15, drying and grinding the solid crystals obtained in step 14 into powder to obtain white powder three; Step 16, mixing and grinding the white powder 1, the purple powder 2 and the white powder 3 in a mass ratio of 2:1:1 to obtain a hybrid coordination polymerization-type metal-organic framework anti-aging agent.
2. The method for preparing the hybrid coordination polymerization metal organic framework anti-aging agent according to claim 1, It is characterized in that In step 1, the added materials were mixed and stirred at 300 rpm for 2.5 hours by a magnetic stirrer.
3. The method for preparing the hybrid coordination polymerization metal organic framework anti-aging agent according to claim 1, It is characterized in that In step 2, step 7 and step 14, centrifuge at 6000 rpm for 20 min; in step 9 and step 10, stir at 800 rpm for 20 min; in step 11 and step 12, stir at 800 rpm for 10 min.
4. A method for preparing modified asphalt, It is characterized in that Includes steps: Step 101, weighing the matrix asphalt, heating it to a molten state, stirring it for 10-20 minutes, and then keeping it warm to 120-150° C., adding 1% of the hybrid coordination polymeric metal organic framework antioxidant prepared by the preparation method of the hybrid coordination polymeric metal organic framework antioxidant according to claim 1, stirring it for 5-15 minutes, and then shearing it, wherein the speed of the shearing machine during the shearing process is 3000 rpm, and the shearing time is 30 minutes; Step 102, placing the asphalt in a 160°C oven and leaving it to stand for 5 minutes to obtain a hybrid coordination polymerization type metal organic framework modified asphalt.