A high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content and its application
The spray drying method is used to prepare ultra-fine natural rubber powder master glue and mix it with natural rubber block glue, which solves the problems of long production cycle and large energy consumption in the existing technology, and achieves low-cost and high-efficiency graphene modification Preparation of natural rubber nanocomposite materials, suitable for tire industry.
Patent Information
- Application Number
- CN202310300813.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-27
AI Technical Summary
The existing latex co-sinking method has a long production cycle and high energy consumption, resulting in high costs, which limits its application in the tire field.
Spray drying method is used to prepare ultrafine natural rubber powder masterbatch with a particle size of less than 5 μm, and mix it with natural rubber block glue and carbon black through mechanical blending process to prepare graphene modified natural rubber nanocomposite materials.
It significantly shortens the production cycle and energy consumption, reduces costs, improves the industrialization prospects of the process, and provides a green and environmentally friendly tire preparation method.
Smart Images

Figure CN116444870B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional rubber composite materials, and specifically relates to a high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content and application thereof. Background Art
[0002] Tires are an indispensable part of modern transportation and are mainly made of rubber. Natural rubber is easily available, inexpensive, and has excellent high elasticity and insulation. In particular, its typical self-reinforcement properties make natural rubber an indispensable matrix material. It is widely used in the field of engineering tire manufacturing and is the main material for preparing load-bearing tires and tank road wheel tires. However, natural rubber is a polymer material. Under the action of long-term dynamic stress, its unique viscoelasticity produces hysteresis, causing the material to convert the mechanical energy it receives into internal heat, resulting in reduced rubber performance and eventual failure. In order to improve the comprehensive performance of natural rubber composites so that they can better meet application requirements, the currently commonly used method is to add nanofillers such as nano carbon black, carbon nanotubes, nano montmorillonite, graphene, etc. to improve the performance of natural rubber composites.
[0003] Graphene is a sp 2 A new material in which hybrid connected carbon atoms are tightly stacked into a single-layer two-dimensional honeycomb lattice structure, it has excellent optical, electrical, and mechanical properties, and has important application prospects in the fields of materials, micro-nano processing, energy, biomedicine, and drug delivery, and is considered to be a revolutionary material in the future. Graphene oxide (GO) is a two-dimensional (2D) material with multiple oxygen-containing functional groups obtained by oxidizing graphite through physical and chemical means.
[0004] Graphene and its derivatives have excellent mechanical strength, electrical conductivity and thermal conductivity, making them widely used in rubber reinforcement modification, so that the prepared rubber composites have better mechanical strength, toughness and thermal conductivity. However, the existing graphene-modified natural rubber composites prepared by latex co-precipitation method have problems such as long production cycle and high energy consumption due to the dehydration and drying process, and also increase the cost, which has become a major obstacle to the application of graphene-modified natural rubber composites in the tire field.
[0005] According to the definition of British BS2955-1993, rubber with a particle size of less than 1mm is powdered rubber. Compared with block and sheet rubber, powdered rubber has many advantages in both processing and application. From the perspective of rubber processing technology, powdered rubber has the advantages of short mixing time, low power consumption, low discharge temperature and good dispersibility; in addition, powdered rubber can be transported by pipeline and automatically weighed like fillers such as carbon black, which helps to improve the degree of automation of factory mixing production. From the application point of view, powdered rubber has a wide range of uses. It can not only be used to prepare rubber products, but also as a modifier in the field of adhesives and polymers. Ultrafine powdered rubber with a particle size of less than 0.5mm has become a hot topic. Summary of the invention
[0006] In view of the above background and existing problems, the present invention provides an efficient and low-cost preparation method and application of ultrafine natural rubber powder masterbatch with high graphene content. First, a spray drying method that is easy to industrialize is used to obtain an ultrafine natural rubber powder masterbatch with a particle size of less than 5 μm, and then a mechanical blending process is used to mix the obtained ultrafine natural rubber powder masterbatch with high graphene content with natural rubber block rubber, carbon black, etc., and a graphene-modified natural rubber nanocomposite material that can be used in tire preparation is prepared.
[0007] The present invention is achieved through the following technical scheme: a high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content, comprising the following steps:
[0008] ① Adding an appropriate amount of deionized water to the graphene oxide dispersion, after ultrasonic dispersion at a certain power for a certain time, adding an anionic surfactant in a certain proportion to the ultrasonic graphene oxide dispersion, and mechanically stirring at a certain speed for a certain time to obtain a modified graphene oxide dispersion;
[0009] ② Add an appropriate amount of deionized water to the natural latex, mix well, and then slowly add the prepared latex suspension to the modified graphene oxide dispersion prepared in step ① under mechanical stirring, and stir and mix for a certain period of time to obtain a uniformly dispersed mixed emulsion;
[0010] ③ The uniformly dispersed mixed emulsion obtained in step ② is pumped into a spray drying device through a feed pump, and quickly dried into a powder at a set temperature to obtain an ultrafine natural rubber powder masterbatch with a high graphene content and a particle size of less than 5 μm.
[0011] As a further improvement of the technical solution of the preparation method of the present invention, in step ①, the anionic surfactant is a combination of one or more of anionic polyacrylamide, fatty acid salts, sulfonates, sulfate esters, and phosphate esters.
[0012] As a further improvement of the technical solution of the preparation method of the present invention, in step ①, the concentration of the graphene oxide dispersion after adding deionized water is 1 to 5 mg / ml, the ultrasonic power is 100 to 300 W, the ultrasonic time is 10 to 30 min, the mass ratio of graphene oxide to anionic surfactant in the graphene oxide dispersion is 7:1 to 3:1, the speed of mechanical stirring is 300 to 700 r / min, and the mechanical stirring time is 10 to 30 min.
[0013] As a further improvement of the technical solution of the preparation method of the present invention, in step ②, the latex concentration in the prepared latex suspension is 10% to 30%, the speed of mechanical stirring is 300 to 700 r / min, the mass ratio of the latex in the prepared latex suspension to the graphene oxide in the oxidized dispersion in step ① is 100:20 to 50, and the stirring and mixing time is 5 to 30 min.
[0014] As a further improvement of the technical solution of the preparation method of the present invention, in step ③, the feed speed of the feed pump is 10-50 ml / min, the inlet air temperature of the spray dryer is 80-120°C, and the outlet air temperature is 50-80°C.
[0015] The present invention further provides an efficient and low-cost preparation method for an ultrafine natural rubber powder masterbatch with a high graphene content, and application of the prepared ultrafine natural rubber powder masterbatch with a high graphene content in a graphene-modified natural rubber nanocomposite material.
[0016] As a further improvement of the application technical solution of the present invention, the application includes the following steps:
[0017] (1) adding ultrafine natural rubber powder masterbatch with high graphene oxide content and natural rubber raw rubber block into an internal mixer in a certain mass ratio, mixing at a certain temperature for a certain time, adding an antioxidant, an antioxidant, an activator and a reinforcing filler in sequence according to a certain proportion, and mixing evenly to obtain a mixed rubber;
[0018] (2) placing the rubber mixture obtained in step (1) in a double roll of an open mixing mill, mixing at a certain temperature, then adding an accelerator and a vulcanizing agent, mixing evenly, and thinning until there are no bubbles in the rubber material to obtain a rubber mixture;
[0019] (3) The mixed rubber obtained in step (2) is allowed to stand for a certain period of time, and vulcanized at a certain temperature and a certain pressure for a certain period of time to obtain a graphene-modified natural rubber nanocomposite material.
[0020] As a further improvement of the application technical solution of the present invention, the mass ratio of high graphene content natural rubber powder masterbatch: natural rubber raw rubber block: antioxidant: antioxidant: activator: accelerator: vulcanizer: reinforcing filler is 1.5-3:97.5-99:1:1:5:2:2:50-80; in step (1), the mixing temperature is 100-120°C, and the mixing time is 10-20min.
[0021] As a further improvement of the application technical solution of the present invention, in step (2), the refining temperature is 50-70°C.
[0022] As a further improvement of the application technical solution of the present invention, in step (3), the storage time of the mixed rubber is 18 to 36 hours, the vulcanization temperature is 140 to 160° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 10 to 30 minutes.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1) The present invention utilizes a spray drying process to prepare graphene-modified natural rubber masterbatch, which can greatly shorten the time and energy consumed by dehydration and drying, and greatly shorten the production cycle, thereby significantly reducing the cost of graphene-modified natural rubber masterbatch, providing a new idea for the application of graphene-modified natural rubber nanocomposites in the tire industry, and also laying a foundation for the green environmental protection of the tire industry.
[0025] 2) The process of preparing ultrafine powder masterbatch of graphene-modified natural rubber by spray drying of the present invention is conducive to reducing dust pollution and energy conservation and emission reduction, and is more in line with the preparation process requirements of green tires. In addition, the process can also be operated continuously, with low labor intensity, and the cost of the prepared masterbatch can be significantly reduced. Therefore, the process and the produced masterbatch have more industrial prospects.
[0026] 3) The high-graphene-content ultrafine natural rubber powder masterbatch provided by the present invention has a simple preparation process, does not require any stringent requirements, involves conventional equipment, is easy to implement, and is also easy to industrialize.
[0027] 4) The ultrafine natural rubber powder masterbatch with high graphene content prepared by the present invention can be directly added to the natural rubber raw rubber block by conventional processes, so as to conveniently obtain the graphene-modified natural rubber nanocomposite material used in the preparation of high-quality tires. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0030] Figure 1 This is a SEM photograph of the ultrafine natural rubber powder masterbatch with high graphene content prepared in Example 1 of the present invention.
[0031] Figure 2 This is a SEM photograph of the ultrafine natural rubber powder masterbatch with high graphene content prepared in Example 2 of the present invention.
[0032] Figure 3 This is a SEM photograph of the ultrafine natural rubber powder masterbatch with high graphene content prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0033] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0034] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0035] The present invention provides a specific embodiment of a method for preparing an ultrafine natural rubber powder masterbatch with a high graphene content at a high efficiency and low cost, comprising the following steps:
[0036] ① Adding an appropriate amount of deionized water to the graphene oxide dispersion, after ultrasonic dispersion at a certain power for a certain time, adding an anionic surfactant in a certain proportion to the ultrasonic graphene oxide dispersion, and mechanically stirring at a certain speed for a certain time to obtain a modified graphene oxide dispersion;
[0037] ② Add an appropriate amount of deionized water to the natural latex, mix well, and then slowly add the prepared latex suspension to the modified graphene oxide dispersion prepared in step ① under mechanical stirring, and stir and mix for a certain period of time to obtain a uniformly dispersed mixed emulsion;
[0038] ③ The uniformly dispersed mixed emulsion obtained in step ② is pumped into a spray drying device through a feed pump, and quickly dried into a powder at a set temperature to obtain an ultrafine natural rubber powder masterbatch with a high graphene content and a particle size of less than 5 μm.
[0039] In one embodiment provided by the present invention, in step ①, the anionic surfactant is a combination of one or more of anionic polyacrylamide, fatty acid salts, sulfonates, and sulfate esters. The fatty acid salts include potassium, sodium, ammonium salts, and triethanolammonium salts of higher fatty acids; the sulfonates include alkylbenzene sulfonates, α-olefin sulfonates, alkyl sulfonates, petroleum sulfonates, and alkyl glycerol ether sulfonates; the sulfate esters include fatty alcohol sulfate esters and secondary alkyl sulfate esters. .
[0040] In another embodiment provided by the present invention, in step ①, the concentration of the graphene oxide dispersion after adding deionized water is 1 to 5 mg / ml, the ultrasonic power is 100 to 300 W, the ultrasonic time is 10 to 30 min, the mass ratio of graphene oxide to anionic surfactant in the graphene oxide dispersion is 7:1 to 3:1, the speed of mechanical stirring is 300 to 700 r / min, and the mechanical stirring time is 10 to 30 min.
[0041] In one embodiment provided by the present invention, in step ②, the latex concentration in the prepared latex suspension is 10% to 30%, the speed of mechanical stirring is 300 to 700 r / min, the mass ratio of the latex in the prepared latex suspension to the graphene oxide in the oxidized dispersion in step ① is 100:20 to 50, and the stirring and mixing time is 5 to 30 min.
[0042] In another embodiment provided by the present invention, in step ③, the feed speed of the feed pump is 10-50 ml / min, the inlet air temperature of the spray dryer is 80-120°C, and the outlet air temperature is 50-80°C.
[0043] The present invention also provides an efficient and low-cost preparation method for an ultrafine natural rubber powder masterbatch with a high graphene content, and application of the prepared ultrafine natural rubber powder masterbatch with a high graphene content in a graphene-modified natural rubber nanocomposite material.
[0044] In one embodiment provided by the present invention, the application comprises the following steps:
[0045] (1) adding ultrafine natural rubber powder masterbatch with high graphene oxide content and natural rubber raw rubber block into an internal mixer in a certain mass ratio, mixing at a certain temperature for a certain time, adding an antioxidant, an antioxidant, an activator and a reinforcing filler in sequence according to a certain proportion, and mixing evenly to obtain a mixed rubber;
[0046] (2) placing the rubber mixture obtained in step (1) in a double roll of an open mixing mill, mixing at a certain temperature, then adding an accelerator and a vulcanizing agent, mixing evenly, and thinning until there are no bubbles in the rubber material to obtain a rubber mixture;
[0047] (3) The mixed rubber obtained in step (2) is allowed to stand for a certain period of time, and vulcanized at a certain temperature and a certain pressure for a certain period of time to obtain a graphene-modified natural rubber nanocomposite material.
[0048] In another embodiment provided by the present invention, the mass ratio of high graphene content natural rubber powder masterbatch: natural rubber raw rubber block: antioxidant: antioxidant: activator: accelerator: vulcanizer: reinforcing filler is 1.5-3: 97.5-99: 1: 1: 5: 2: 2: 50-80; in step (1), the mixing temperature is 100-120° C., and the mixing time is 10-20 min.
[0049] In one embodiment provided by the present invention, in step (2), the refining temperature is 50-70°C.
[0050] In another embodiment provided by the present invention, in step (3), the storage time of the rubber mix is 18 to 36 hours, the vulcanization temperature is 140 to 160° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 10 to 30 min.
[0051] The specific embodiments of the present invention are described in detail below.
[0052] Example 1
[0053] A high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content comprises the following steps:
[0054] ① Add a certain amount of deionized water to 2000g of graphene oxide (GO) dispersion with a concentration of 10mg / ml, ultrasonically disperse it at a power of 100W for 10min to obtain a GO aqueous dispersion with a concentration of 1mg / ml, add sodium dodecylbenzene sulfonate (SDBS) according to a mass ratio of GO to sodium dodecylbenzene sulfonate (SDBS) of 7:1, and continuously stir mechanically at a speed of 300r / min for 10min to obtain a modified GO dispersion.
[0055] ② Add an appropriate amount of deionized water to 166.7g of natural latex solution with a solid content of 60% to dilute it into a natural latex suspension with a solid content of 10%. Under mechanical stirring, add the natural latex suspension to the modified GO dispersion obtained in step ①. The concentration of GO in the entire dispersion is 1mg / ml. Continuous mechanical stirring for 10min at 25°C and 300r / min. After uniform mixing, a natural rubber and modified GO mixture with a GO content of 20phr is obtained.
[0056] ③ The natural rubber and modified GO mixture obtained in step ② was pumped into a spray drying device through a flow pump. The inlet air temperature of the spray drying device was 80°C, the outlet air temperature was 50°C, and the flow rate of the flow pump was 10 ml / min. An ultra-fine natural rubber powder masterbatch with a particle size of less than 5 μm and a GO content of 20 phr was obtained. The SEM photo of the masterbatch is shown in Figure 1 .
[0057] Example 2
[0058] A high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content comprises the following steps:
[0059] ① Add a certain amount of deionized water to 3000g of GO dispersion with a concentration of 10mg / ml, and ultrasonically disperse it at a power of 300W for 30min to obtain a GO aqueous dispersion with a concentration of 5mg / ml; add SDBS according to the mass ratio of GO to SDBS 5:1, and continuously stir mechanically at a speed of 300r / min for 10min to obtain a modified GO dispersion.
[0060] ② Add an appropriate amount of deionized water to 166.7g of natural latex solution with a solid content of 60%, and dilute it into a natural latex suspension with a solid content of 30%. Under mechanical stirring, add the natural latex suspension to the modified GO dispersion obtained in step ①. The concentration of GO in the entire dispersion is 5mg / ml. Continuous mechanical stirring is carried out for 30min at 25℃ and 700r / min. After uniform mixing, a natural rubber and modified GO mixture with a GO content of 30phr is obtained.
[0061] ③ The natural rubber and modified GO mixture obtained in step ② was pumped into a spray drying device through a flow pump. The inlet air temperature of the spray drying device was 110°C, the outlet air temperature was 70°C, and the flow rate of the flow pump was 30 ml / min. An ultra-fine natural rubber powder masterbatch with a particle size of less than 5 μm and a GO content of 30 phr was obtained. The SEM photo of the masterbatch is shown in Figure 2 .
[0062] Example 3
[0063] A high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content comprises the following steps:
[0064] ① Add a certain amount of deionized water to 5000g of GO dispersion with a concentration of 10mg / ml, and ultrasonically disperse it at a power of 300W for 30min to obtain a GO aqueous dispersion with a concentration of 5mg / ml; add SDBS according to the mass ratio of GO to SDBS 3:1, and continuously stir mechanically at a speed of 700r / min for 30min to obtain a modified GO dispersion.
[0065] ② Add an appropriate amount of deionized water to 166.7g of natural latex solution with a solid content of 60% to dilute it into a natural latex suspension with a solid content of 30%. Under mechanical stirring, add the natural latex suspension to the modified GO dispersion obtained in step ①. The concentration of GO in the entire dispersion is 5mg / ml. Continuous mechanical stirring is carried out for 30min at 25°C and 700r / min. After uniform mixing, a natural rubber and modified GO mixture with a GO content of 50phr is obtained.
[0066] ③ The natural rubber and modified GO mixture obtained in step ② was pumped into the spray drying equipment through a flow pump. The inlet air temperature of the spray drying equipment was 120°C, the outlet air temperature was 80°C, and the flow rate of the flow pump was 50 ml / min. An ultra-fine natural rubber powder masterbatch with a particle size of less than 5 μm and a GO content of 50 phr was obtained. The SEM photo of the masterbatch is shown in Figure 3 .
[0067] Example 4
[0068] A process for preparing a graphene-modified natural rubber nanocomposite material using ultrafine natural rubber powder masterbatch with a high graphene content, comprising the following steps:
[0069] (1) 3 g of the ultrafine natural rubber masterbatch with high graphene oxide content prepared in Example 1 and 97.5 g of natural rubber raw rubber block were added to an internal mixer and kneaded at 100° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and kneaded for 5 min. Then, 5 g of ZnO, 2 g of stearic acid and 25 g of carbon black were added in sequence and kneaded for 2.5 min. Then, 25 g of carbon black was added and kneaded for another 2.5 min to obtain a kneaded rubber.
[0070] (2) The rubber mixture obtained in step (1) is placed in a double roll of an open mixing mill and mixed at 50° C., and then 2 g of accelerator 2-(4-morpholinethio)benzothiazole and 2 g of sulfur are added. After mixing evenly, the mixture is passed through a thin tube until there are no bubbles in the rubber to obtain a rubber mixture.
[0071] (3) The rubber mixture obtained in step (2) was allowed to stand for 18 hours, and vulcanized on a flat plate vulcanizer at 140° C. and 10 MPa for 30 minutes to obtain a graphene-modified natural rubber nanocomposite material.
[0072] Example 5
[0073] A process for preparing a graphene-modified natural rubber nanocomposite material using ultrafine natural rubber powder masterbatch with a high graphene content, comprising the following steps:
[0074] (1) 2.17 g of the ultrafine natural rubber masterbatch with high graphene oxide content prepared in Example 2 and 98.33 g of natural rubber raw rubber block were added to an internal mixer and kneaded at 110° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and kneaded for 5 min. Then, 5 g of ZnO, 2 g of stearic acid and 25 g of carbon black were added in sequence and kneaded for 5 min. Then, 25 g of carbon black was added and kneaded for 5 min to obtain a kneaded rubber.
[0075] (2) The rubber mixture obtained in step (1) is placed in a double roll of an open mixing mill and mixed at 70° C., and then 2 g of accelerator 2-(4-morpholinethio)benzothiazole and 2 g of sulfur are added. After mixing evenly, the mixture is passed through a thin tube until there are no bubbles in the rubber to obtain a rubber mixture.
[0076] (3) The rubber mixture obtained in step (2) was allowed to stand for 36 hours, and vulcanized on a flat plate vulcanizer at 160° C. and 30 MPa for 10 minutes to obtain a graphene-modified natural rubber nanocomposite material.
[0077] Example 6
[0078] A process for preparing a graphene-modified natural rubber nanocomposite material using ultrafine natural rubber powder masterbatch with a high graphene content, comprising the following steps:
[0079] (1) 1.5 g of the ultrafine natural rubber masterbatch with high graphene oxide content prepared in Example 3 and 99 g of natural rubber raw rubber block were added to an internal mixer and kneaded at 120° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and kneaded for 5 min. Then, 5 g of ZnO, 2 g of stearic acid and 25 g of carbon black were added in sequence and kneaded for 5 min. Then, 25 g of carbon black was added and kneaded for 5 min to obtain a mixed rubber.
[0080] (2) The rubber mixture obtained in step (1) is placed in a double roll of an open mixing mill and mixed at 70° C., and then 2 g of accelerator 2-(4-morpholinethio)benzothiazole and 2 g of sulfur are added. After mixing evenly, the mixture is passed through a thin tube until there are no bubbles in the rubber to obtain a rubber mixture.
[0081] (3) The rubber mixture obtained in step (2) was allowed to stand for 36 hours, and vulcanized on a flat plate vulcanizer at 160° C. and 30 MPa for 20 minutes to obtain a graphene-modified natural rubber nanocomposite material.
[0082] Comparative Example 1:
[0083] A method for preparing a natural rubber powder masterbatch with a high graphene content without modification of graphene oxide comprises the following steps:
[0084] ① Add a certain amount of deionized water to 2000g of GO dispersion with a concentration of 10mg / ml, ultrasonically disperse it at a power of 100W for 10min to obtain a GO aqueous dispersion with a concentration of 1mg / ml, and continuously mechanically stir it at a speed of 300r / min for 10min to obtain a GO dispersion.
[0085] ② Add an appropriate amount of deionized water to 166.7g of natural latex solution with a solid content of 60% to dilute it into a natural latex suspension with a solid content of 10%. Under mechanical stirring, add the natural latex suspension to the GO dispersion obtained in step ①. The concentration of GO in the entire dispersion is 1mg / ml. Continuously stir mechanically for 10min at 25℃ and 300r / min. After mixing evenly, a mixture of natural rubber and GO with a GO content of 20phr is obtained.
[0086] ③ The mixed solution of natural rubber and GO obtained in step ② is pumped into a spray drying device through a flow pump. The inlet air temperature of the spray drying device is 80°C, the outlet air temperature is 50°C, and the flow rate of the flow pump is 10ml / min to obtain a natural rubber powder masterbatch with a GO content of 20phr.
[0087] Comparative Example 2
[0088] A process for preparing a graphene-modified natural rubber composite material by using natural rubber powder masterbatch with a high graphene content without modification of graphene oxide, comprising the following steps:
[0089] (1) 3 g of the natural rubber masterbatch with high graphene oxide content prepared in Comparative Example 1 and 97.5 g of natural rubber raw rubber block were added to an internal mixer and kneaded at 100° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and kneaded for 5 min. Then, 5 g of ZnO, 2 g of stearic acid and 25 g of carbon black were added in sequence and kneaded for 5 min. Then, 25 g of carbon black was added and kneaded for 5 min to obtain a kneaded rubber.
[0090] (2) The internal rubber obtained in step (1) is placed in a double roll of an open mixing mill and mixed at 50° C., and then 2 g of accelerator 2-(4-morpholinethio)benzothiazole and 2 g of sulfur are added. After mixing evenly, the mixture is thinly passed until there are no bubbles in the rubber to obtain a mixed rubber.
[0091] (3) The rubber mixture obtained in step (2) was allowed to stand for 18 hours, and vulcanized on a flat plate vulcanizer at 140° C. and 10 MPa for 30 minutes to obtain a graphene-modified natural rubber nanocomposite material.
[0092] The formulas of Examples 1 to 3 and Comparative Example 1 are shown in Table 1, the formulas of Examples 4 to 6 and Comparative Example 2 are shown in Table 2, and the performance test results of Examples 4 to 6 and Comparative Example 2 are shown in Table 3.
[0093] Table 1 Formula table of Examples 1 to 3 of the present invention and Comparative Example 1
[0094] sample Comparative Example 1 Example 1 Example 2 Example 3 Graphene oxide / g 20 20 30 40 Natural rubber / g 100 100 100 100
[0095] Table 2 Formula table of Examples 4 to 6 of the present invention and Comparative Example 2
[0096]
[0097] The mechanical, thermal conductivity, heat generation, abrasion and compression permanent deformation properties of Examples 4 to 6 and Comparative Example 2 were tested. The test standard for mechanical properties was ISO37-2005, with a tensile rate of 500 mm / min and a tearing speed of 500 mm / min; the test standard for thermal conductivity was GB / T3399; the test standard for heat generation and compression permanent deformation was ISO 4666; and the test standard for abrasion properties was GB / T9867-2008.
[0098] Table 3 Properties of graphene-modified natural rubber nanocomposites prepared by the present invention
[0099]
[0100]
[0101] It can be seen from Table 3 that the mechanical, thermal conductivity, heat generation, wear resistance and permanent deformation properties of the graphene-modified natural rubber nanocomposite prepared by using the ultrafine natural rubber powder masterbatch with high graphene content of the present invention are all very excellent. Compared with the comparative example 2 in which the graphene oxide is not modified but the other processes are exactly the same, the mechanical, thermal conductivity, heat generation, wear resistance and permanent deformation properties of the graphene-modified natural rubber nanocomposite prepared by using the ultrafine natural rubber powder masterbatch with high graphene content of the present invention in Example 4 are all more excellent. Figure 1-3 It can be seen that the particle size of the high graphene content natural rubber powder masterbatch prepared by the present invention is less than 5 μm, which is an ultrafine powder masterbatch.
[0102] The above is only a specific implementation of the present invention, which enables those skilled in the art to understand or implement the present invention. Although detailed descriptions are given with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments, and they should all be covered by the protection scope of the claims.
Claims
1. A method for preparing a graphene-modified natural rubber nanocomposite material, characterized in that: The steps include: (1) adding high-graphene-content ultrafine natural rubber powder masterbatch and natural rubber raw rubber block in a certain mass ratio into an internal mixer, and mixing them at a certain temperature for a certain time, during which antioxidant, antioxidant, activator and reinforcing filler are added in proportion, and mixed evenly to obtain a mixed rubber; the mass ratio of high-graphene-content ultrafine natural rubber powder masterbatch: natural rubber raw rubber block: antioxidant: antioxidant: activator: accelerator: vulcanizer: reinforcing filler is 1.5-3: 97.5-99: 1: 1: 5: 2: 2: 50-80; (2) placing the rubber mixture obtained in step (1) in a double roll of an open mixing mill, mixing at a certain temperature, then adding an accelerator and a vulcanizing agent, mixing evenly, and thinning until there are no bubbles in the rubber material to obtain a rubber mixture; (3) allowing the rubber mixture obtained in step (2) to stand for a certain period of time, and vulcanizing it at a certain temperature and a certain pressure for a certain period of time to obtain a graphene-modified natural rubber nanocomposite material; The method for preparing the ultrafine natural rubber powder masterbatch with high graphene content in step (1) comprises the following steps: ① Adding an appropriate amount of deionized water to the graphene oxide dispersion, after ultrasonic dispersion at a certain power for a certain time, adding an anionic surfactant in a certain proportion to the ultrasonic graphene oxide dispersion, and mechanically stirring at a certain speed for a certain time to obtain a modified graphene oxide dispersion; ② Add an appropriate amount of deionized water to the natural latex, mix well, and then slowly add the prepared latex suspension to the modified graphene oxide dispersion prepared in step ① under mechanical stirring. The mass ratio of the latex in the prepared latex suspension to the graphene oxide in the oxidized dispersion in step ① is 100:20-50. After stirring and mixing for a certain period of time, a uniformly dispersed mixed emulsion is obtained; ③ The uniformly dispersed mixed emulsion obtained in step ② is pumped into a spray drying device through a feed pump, and the feed speed of the feed pump is 10-50 ml / min; it is quickly dried into a powder at a set temperature, and the inlet air temperature of the spray dryer is 80-120° C., and the outlet air temperature is 50-80° C.; thus, a high graphene content ultrafine natural rubber powder masterbatch with a particle size of less than 5 μm is obtained.
2. The method for preparing the graphene-modified natural rubber nanocomposite material according to claim 1, characterized in that: In step ①, the anionic surfactant is a combination of one or more of anionic polyacrylamide, fatty acid salts, sulfonates, sulfate esters, and phosphate esters.
3. The method for preparing the graphene-modified natural rubber nanocomposite material according to claim 1, characterized in that: In step ①, the concentration of the graphene oxide dispersion after adding deionized water is 1 to 5 mg / ml, the ultrasonic power is 100 to 300 W, the ultrasonic time is 10 to 30 min, the mass ratio of graphene oxide to anionic surfactant in the graphene oxide dispersion is 7:1 to 3:1, the speed of mechanical stirring is 300 to 700 r / min, and the mechanical stirring time is 10 to 30 min.
4. The method for preparing the graphene-modified natural rubber nanocomposite material according to claim 1, characterized in that: In step ②, the latex concentration in the prepared latex suspension is 10% to 30%, the speed of the mechanical stirring is 300 to 700 r / min, and the stirring and mixing time is 5 to 30 min.
5. The method for preparing the graphene-modified natural rubber nanocomposite material according to claim 1, characterized in that: In step (1), the banburying temperature is 100-120°C, and the banburying time is 10-20 min.
6. The method for preparing the graphene-modified natural rubber nanocomposite material according to claim 1, characterized in that: In step (2), the refining temperature is 50-70°C.
7. The method for preparing the graphene-modified natural rubber nanocomposite material according to claim 1, characterized in that: In step (3), the storage time of the rubber mix is 18 to 36 hours, the vulcanization temperature is 140 to 160° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 10 to 30 minutes.