A method for preparing a cerium-based monolithic catalyst by electrodeposition and its application in the field of catalytic oxidation of OVOCs
By adjusting the deposition voltage and time in the electrodeposition method, different amounts and density of CeO2 are loaded on the foam nickel support, the problems of uneven loading and high temperature and high pressure in the prior art are solved, and the activity and stability of the catalyst are improved. It is suitable for Industrial application.
Patent Information
- Application Number
- CN202310435539.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-21
AI Technical Summary
In the prior art, when the electrodeposition method loads the Al2O3 coating, the coating is uneven due to the small deposition voltage, which affects the catalyst activity. In situ hydrothermal method requires high temperature and high pressure conditions and is difficult to control the load amount and load of the active components. Density limits the industrial application of catalysts.
By adjusting the deposition voltage and deposition time, the electrodeposition method is used to load different amounts and density of CeO2 on the foam nickel support, and a high activity and convenience cerium-based integral catalyst is prepared, solving the problem of difficult loading and density control. .
It has achieved significant improvement in catalyst activity and stability, the process is simple and convenient to operate, it is suitable for industrial mass production, the active components of the catalyst are evenly dispersed, with moderate quantity and density, and is suitable for the catalytic oxidation of oxygen-containing volatile organic compounds.
Smart Images

Figure CN116459841B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of low-temperature thermal catalytic treatment of waste gas, and specifically relates to an electrodeposition preparation method of a cerium-based monolithic catalyst and its application in the field of OVOCs catalytic oxidation. Background Art
[0002] With the promotion of the use of water-based raw materials, more and more industries that need to use coatings and inks (represented by the coating, packaging and printing industries) have changed solvents from oily substances such as toluene to water-based raw materials such as butyl acetate. Under the background of water-based, the emission of oxygen-containing volatile organic compounds such as butyl acetate has further intensified. Catalytic oxidation is a method of efficiently removing organic waste gas, and its core lies in the low-temperature efficiency of the catalyst. At present, monolithic catalysts are receiving widespread attention because of their porous structure and large specific surface area, small bed pressure drop, and better ability to avoid the problem of catalyst pore clogging.
[0003] In order to avoid problems such as catalyst deactivation caused by coating shedding, non-coating loading methods of catalysts are widely used, including in-situ hydrothermal method and electrodeposition method. For example, studies have used in-situ hydrothermal method to load rare earth element cerium onto Co-Ni carrier and Co carrier, so that the catalyst presents a polygonal morphology with holes and has good activity (patent number: 202211282301.9). However, since the in-situ hydrothermal method requires high temperature and high pressure conditions, and it is difficult to control the loading amount and loading density of active components, the progress of industrial application is slow. The electrodeposition method can directly deposit the active components on the required integral catalyst through electrochemical action. It has a simple process and convenient operation, and has great practical application significance.
[0004] At present, the latest research (patent number: 202110793982.4) uses the electrodeposition method to load Al2O3 coating to increase the specific surface area of the catalyst and increase the loading amount of the active component. However, due to the low deposition voltage, the coating will be unevenly distributed, affecting the activity of the catalyst. Since the monolithic catalyst itself has a large specific surface area, the metal component can be directly deposited on the carrier, and the loading amount of the active component can be controlled by adjusting the deposition voltage and deposition time. Existing studies (patent number: 201711099461.9) also deposited the Co element on the surface of nickel foam by electrodeposition. The active component has a flaky morphology and can completely catalyze the oxidation of propane at 290°C. However, its deposition time is long and the catalytic effect needs to be improved. Therefore, the metal element can be replaced on this basis, and a single-component electrodeposition catalyst with better performance can be prepared by adjusting the deposition voltage, stirring speed and deposition time. Summary of the invention
[0005] In order to enrich the examples of electrodeposition methods for rare earth elements, explore the optimal electrodeposition time to further change the loading amount and loading density of active components, thereby improving the activity of the catalyst, the present invention aims to provide a method for preparing a cerium-based monolithic catalyst by electrodeposition, and demonstrate its application in the field of OVOCs catalytic oxidation. In order to solve the problem of difficult control of loading amount and loading density in the in-situ hydrothermal method, the present invention adopts the electrodeposition method, adjusts the deposition voltage and deposition time, and successfully loads CeO2 of different quantities and densities on the surface of the nickel foam carrier, so that the catalytic activity and stability of the monolithic catalyst are significantly improved. This method has the advantages of simple process, short operation time, high safety, etc., and is suitable for industrial mass production.
[0006] The present invention is achieved through the following technical solutions:
[0007] The invention provides an integral catalyst with CeO2 as an active component and nickel foam as a carrier, which has high activity and high convenience.
[0008] The invention provides a method for preparing a cerium-based monolithic catalyst by electrodeposition. Oxygen-containing volatile organic matter is used as the catalytic object, a constant deposition voltage, a stirring speed and a specific deposition time are determined, and an active component CeO2 is in-situ grown on a foam nickel carrier in different quantities and densities.
[0009] The electrodeposition preparation method of the cerium-based monolithic catalyst comprises the following steps:
[0010] (1) cutting a high-purity nickel foam carrier into a working nickel foam sheet with a length of 1-5 cm, a width of 1-5 cm, and a thickness of 1-2 mm;
[0011] (2) immersing the entire nickel foam carrier in a hydrochloric acid solution and performing ultrasonic acid washing; after the ultrasonic washing is completed, the acid solution is discarded, the surface of the nickel foam carrier is washed with deionized water, and ethanol is added and ultrasonic washing is performed again; after the ultrasonic washing is completed, the surface of the nickel foam carrier is washed again with ethanol; the washed nickel foam carrier is placed in a tube furnace, vacuum dried, and a pure nickel foam carrier is obtained after the drying is completed;
[0012] (3) Weighing Ce(NO3)3·6H2O and dissolving it in deionized water, stirring, to obtain Ce(NO3)3 electrolyte;
[0013] (4) Put the prepared Ce(NO3)3 electrolyte into the electrolytic cell, clamp a cleaned nickel foam carrier with an electrode clamp, and connect the electrode clamp to the working electrode, then connect the calomel electrode and the platinum electrode to the reference electrode and the counter electrode respectively, fix the position of each electrode with a rubber ring, make the working part of the electrode completely immersed in the electrolyte, adjust the electrochemical workstation to the constant voltage deposition mode, set a specific deposition voltage and deposition time, turn on the stirring device, adjust the rotor speed, and start deposition;
[0014] (5) taking off the deposited nickel foam, placing it in a culture dish and sending it into an oven for drying;
[0015] (6) The dried nickel foam is loaded into a porcelain boat, sent into a tubular furnace, and calcined at a certain temperature for a period of time to obtain a cerium-based monolithic catalyst, which is recorded as Ce / Ni-foam.
[0016] In the above method, in step (2), the concentration of the hydrochloric acid solution is 1-3 mol / L.
[0017] In the above method, in step (2), the hydrochloric acid pickling is performed for 5-10 minutes, and the ethanol pickling is performed twice, each for 5-10 minutes.
[0018] In the above method, in step (2), the vacuum drying temperature is 60-80° C. and the drying time is 6-12 h.
[0019] In the above method, in step (3), the concentration of the prepared Ce(NO3)3 electrolyte is 0.1-0.15 mol / L.
[0020] In the above method, in step (4), the deposition voltage is (-1.7)-(-1.8) V, the deposition time is 30s-1800s, and the stirring speed and rotor speed are 300-400r / min.
[0021] In the above method, in step (5), the drying temperature is 60-80° C. and the drying time is 6-12 h.
[0022] In the above method, in step (6), the calcination temperature is 400-600°C, the calcination time is 1-3h, and the calcination heating and cooling rates are both 1-5°C / min.
[0023] A cerium-based monolithic catalyst is used in the field of catalytic oxidation of oxygen-containing volatile organic compounds, specifically in the auto repair and furniture painting industries.
[0024] Compared with the prior art, the advantages of the present invention are:
[0025] 1. The present invention successfully grows the active component CeO2 in situ on the surface of nickel foam through an electrodeposition method with specific parameters, and prepares a cerium-based monolithic catalyst with high activity and high convenience, in which the active components are evenly dispersed, the number of active components is moderate, and the density of active components is moderate.
[0026] 2. The electrodeposition preparation method adopted by the present invention has a simple process, convenient operation, short preparation time and controllable process, and is very suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1The XRD pattern of the cerium-based monolithic catalyst prepared by electrodeposition for 30 seconds in Example 1;
[0028] Figure 2 The XRD pattern of the cerium-based monolithic catalyst prepared by electrodeposition for 60 seconds in Example 2;
[0029] Figure 3 The XRD pattern of the cerium-based monolithic catalyst prepared by electrodeposition for 300 s in Example 3;
[0030] Figure 4 The XRD pattern of the cerium-based monolithic catalyst prepared by electrodeposition for 900 s in Example 4;
[0031] Figure 5 XRD pattern of the cerium-based monolithic catalyst prepared by electrodeposition for 1800 s in Example 5;
[0032] Figure 6 The SEM comparison pictures of the cerium-based monolithic catalysts prepared by electrodeposition in Example 1, Example 3 and Example 5;
[0033] Figure 7 The activity diagrams of the cerium-based monolithic catalysts prepared by electrodeposition at different times in Examples 1-5. DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with examples and drawings: The following examples are implemented on the premise of the technical solution of the present invention, and the active component elements, preparation methods, and specific parameters of the operation process of the examples are given, but the protection scope of the present invention is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the invention shall be included in the protection scope of the present invention.
[0035] Example 1
[0036] This example provides a method for preparing a cerium-based monolithic catalyst for electrodeposition for 30 seconds, and the specific steps are as follows:
[0037] (1) A nickel foam carrier with a length of 1 cm, a width of 5 cm, and a thickness of 1.6 mm was completely immersed in 3 mol / L hydrochloric acid, and the acid solution was poured out after ultrasonic treatment for 10 minutes. The surface of the nickel foam was cleaned with an ethanol solution. After cleaning, an ethanol solution was added to completely cover the nickel foam, and ultrasonic treatment was performed for 5 minutes. After the end, the ethanol solution was poured out, and the operation steps were repeated once. The cleaned nickel foam was placed in a clean porcelain boat, sent to a tube furnace for evacuation, and dried at 80°C for 12 hours under vacuum conditions.
[0038] (2) Weigh 5.2106 g of Ce(NO3)3·6H2O on a balance and add it to 80 ml of deionized water. Stir with a magnetic stirrer until Ce(NO3)3·6H2O is completely dissolved. Pour all of the above solution into the electrolytic cell and wait for use.
[0039] (3) Take a piece of pure nickel foam carrier, clamp it with an electrode clamp and connect the electrode clamp to the working electrode, then connect the calomel electrode and the platinum electrode to the reference electrode and the counter electrode respectively. Fix the position of each electrode with a rubber ring so that the working part of the electrode is completely immersed in the electrolyte. Adjust the electrochemical workstation to the constant voltage deposition mode, set the deposition voltage to -1.78V and the deposition time to 30s. Turn on the stirring device, adjust the rotor speed to 400r / min, and start deposition.
[0040] (4) Place the deposited nickel foam sample in a glass dish, place it in an oven, and dry it at 80°C for 12 hours.
[0041] (5) The dried nickel foam is loaded into a porcelain boat, sent into a tube furnace, provided with air atmosphere, and calcined at 500° C. for 2 h, with a heating / cooling rate of 3° C. / min. After calcination, a cerium-based monolithic catalyst with a deposition time of 30 s is obtained, which is recorded as 30-Ce / Ni-foam, and has a loading of 13.58%.
[0042] Example 2
[0043] This example provides a method for preparing a cerium-based monolithic catalyst for electrodeposition for 60 seconds, and the specific steps are as follows:
[0044] (1) A nickel foam carrier with a length of 1 cm, a width of 5 cm, and a thickness of 1.6 mm was completely immersed in 3 mol / L hydrochloric acid, and the acid solution was poured out after ultrasonic treatment for 10 minutes. The surface of the nickel foam was cleaned with an ethanol solution. After cleaning, an ethanol solution was added to completely cover the nickel foam, and ultrasonic treatment was performed for 5 minutes. After the end, the ethanol solution was poured out, and the operation steps were repeated once. The cleaned nickel foam was placed in a clean porcelain boat, sent to a tube furnace for evacuation, and dried at 80°C for 12 hours under vacuum conditions.
[0045] (2) Weigh 5.2106 g of Ce(NO3)3·6H2O on a balance and add it to 80 ml of deionized water. Stir with a magnetic stirrer until Ce(NO3)3·6H2O is completely dissolved. Pour all of the above solution into the electrolytic cell and wait for use.
[0046] (3) Take a piece of pure nickel foam carrier, clamp it with an electrode clamp and connect the electrode clamp to the working electrode, then connect the calomel electrode and the platinum electrode to the reference electrode and the counter electrode respectively. Fix the position of each electrode with a rubber ring so that the working part of the electrode is completely immersed in the electrolyte. Adjust the electrochemical workstation to the constant voltage deposition mode, set the deposition voltage to -1.78V and the deposition time to 60s. Turn on the stirring device, adjust the rotor speed to 400r / min, and start deposition.
[0047] (4) Place the deposited nickel foam sample in a glass dish, place it in an oven, and dry it at 80°C for 12 hours.
[0048] (5) The dried nickel foam is loaded into a porcelain boat, sent into a tube furnace, provided with air atmosphere, and calcined at 500° C. for 2 h, with a heating / cooling rate of 3° C. / min. After calcination, a cerium-based monolithic catalyst with a deposition time of 60 s is obtained, which is recorded as 60-Ce / Ni-foam, and has a loading of 12.45%.
[0049] Example 3
[0050] This example provides a method for preparing a cerium-based monolithic catalyst by electroplating for 300s, and the specific steps are as follows:
[0051] (1) A nickel foam carrier with a length of 1 cm, a width of 5 cm, and a thickness of 1.6 mm was completely immersed in 3 mol / L hydrochloric acid, and the acid solution was poured out after ultrasonic treatment for 10 minutes. The surface of the nickel foam was cleaned with an ethanol solution. After cleaning, an ethanol solution was added to completely cover the nickel foam, and ultrasonic treatment was performed for 5 minutes. After the end, the ethanol solution was poured out, and the operation steps were repeated once. The cleaned nickel foam was placed in a clean porcelain boat, sent to a tube furnace for evacuation, and dried at 80°C for 12 hours under vacuum conditions.
[0052] (2) Weigh 5.2106 g of Ce(NO3)3·6H2O on a balance and add it to 80 ml of deionized water. Stir with a magnetic stirrer until Ce(NO3)3·6H2O is completely dissolved. Pour all of the above solution into the electrolytic cell and wait for use.
[0053] (3) Take a piece of pure nickel foam carrier, clamp it with an electrode clamp and connect the electrode clamp to the working electrode, then connect the calomel electrode and the platinum electrode to the reference electrode and the counter electrode respectively. Fix the position of each electrode with a rubber ring so that the working part of the electrode is completely immersed in the electrolyte. Adjust the electrochemical workstation to the constant voltage deposition mode, set the deposition voltage to -1.78V and the deposition time to 300s. Turn on the stirring device, adjust the rotor speed to 400r / min, and start deposition.
[0054] (4) Place the deposited nickel foam sample in a glass dish, place it in an oven, and dry it at 80°C for 12 hours.
[0055] (5) The dried nickel foam is loaded into a porcelain boat, sent into a tube furnace, provided with air atmosphere, and calcined at 500° C. for 2 h, with a heating / cooling rate of 3° C. / min. After calcination, a cerium-based monolithic catalyst with a deposition time of 300 s is obtained, which is recorded as 300-Ce / Ni-foam, and has a loading of 18.93%.
[0056] Example 4
[0057] This example provides a method for preparing a cerium-based monolithic catalyst for electrodeposition for 900 s, and the specific steps are as follows:
[0058] (1) A nickel foam carrier with a length of 1 cm, a width of 5 cm, and a thickness of 1.6 mm was completely immersed in 3 mol / L hydrochloric acid, and the acid solution was poured out after ultrasonic treatment for 10 minutes. The surface of the nickel foam was cleaned with an ethanol solution. After cleaning, an ethanol solution was added to completely cover the nickel foam, and ultrasonic treatment was performed for 5 minutes. After the end, the ethanol solution was poured out, and the operation steps were repeated once. The cleaned nickel foam was placed in a clean porcelain boat, sent to a tube furnace for evacuation, and dried at 80°C for 12 hours under vacuum conditions.
[0059] (2) Weigh 5.2106 g of Ce(NO3)3·6H2O on a balance and add it to 80 ml of deionized water. Stir with a magnetic stirrer until Ce(NO3)3·6H2O is completely dissolved. Pour all of the above solution into the electrolytic cell and wait for use.
[0060] (3) Take a piece of pure nickel foam carrier, clamp it with an electrode clamp and connect the electrode clamp to the working electrode, then connect the calomel electrode and the platinum electrode to the reference electrode and the counter electrode respectively. Fix the position of each electrode with a rubber ring so that the working part of the electrode is completely immersed in the electrolyte. Adjust the electrochemical workstation to the constant voltage deposition mode, set the deposition voltage to -1.78V and the deposition time to 900s. Turn on the stirring device, adjust the rotor speed to 400r / min, and start deposition.
[0061] (4) Place the deposited nickel foam sample in a glass dish, place it in an oven, and dry it at 80°C for 12 hours.
[0062] (5) The dried nickel foam is loaded into a porcelain boat, sent into a tube furnace, provided with air atmosphere, and calcined at 500° C. for 2 h, with a heating / cooling rate of 3° C. / min. After calcination, a cerium-based monolithic catalyst with a deposition time of 900 s is obtained, which is recorded as 900-Ce / Ni-foam and has a loading of 26.70%.
[0063] Example 5
[0064] This example provides a method for preparing a cerium-based monolithic catalyst for electrodeposition for 1800s, and the specific steps are as follows:
[0065] (1) A nickel foam carrier with a length of 1 cm, a width of 5 cm, and a thickness of 1.6 mm was completely immersed in 3 mol / L hydrochloric acid, and the acid solution was poured out after ultrasonic treatment for 10 minutes. The surface of the nickel foam was cleaned with an ethanol solution. After cleaning, an ethanol solution was added to completely cover the nickel foam, and ultrasonic treatment was performed for 5 minutes. After the end, the ethanol solution was poured out, and the operation steps were repeated once. The cleaned nickel foam was placed in a clean porcelain boat, sent to a tube furnace for evacuation, and dried at 80°C for 12 hours under vacuum conditions.
[0066] (2) Weigh 5.2106 g of Ce(NO3)3·6H2O on a balance and add it to 80 ml of deionized water. Stir with a magnetic stirrer until Ce(NO3)3·6H2O is completely dissolved. Pour all of the above solution into the electrolytic cell and wait for use.
[0067] (3) Take a piece of pure nickel foam carrier, clamp it with an electrode clamp and connect the electrode clamp to the working electrode, then connect the calomel electrode and the platinum electrode to the reference electrode and the counter electrode respectively. Fix the position of each electrode with a rubber ring so that the working part of the electrode is completely immersed in the electrolyte. Adjust the electrochemical workstation to the constant voltage deposition mode, set the deposition voltage to -1.78V and the deposition time to 1800s. Turn on the stirring device, adjust the rotor speed to 400r / min, and start deposition.
[0068] (4) Place the deposited nickel foam sample in a glass dish, place it in an oven, and dry it at 80°C for 12 hours.
[0069] (5) The dried nickel foam is loaded into a porcelain boat, sent into a tube furnace, provided with air atmosphere, and calcined at 500° C. for 2 h, with a heating / cooling rate of 3° C. / min. After calcination, a cerium-based monolithic catalyst with a deposition time of 1800 s is obtained, which is recorded as 1800-Ce / Ni-foam, and has a loading of 25.61%.
[0070] The activity of the monolithic catalysts 30-Ce / Ni-foam, 60-Ce / Ni-foam, 300-Ce / Ni-foam, 900-Ce / Ni-foam and 1800-Ce / Ni-foam prepared above was tested. The test conditions were as follows: the catalyst was cut to about 0.3 g, the air velocity was 60000 h -1 , the exhaust gas inlet concentration is 1000-2000ppm.
[0071] Characterization results
[0072] 1. X-ray diffraction (XRD) characterization
[0073] Figure 1 , 2 , 3, 4, 5 are the XRD spectra of the monolithic catalysts 30-Ce / Ni-foam, 60-Ce / Ni-foam, 300-Ce / Ni-foam, 900-Ce / Ni-foam and 1800-Ce / Ni-foam of Examples 1-5, respectively. Comparing the spectra with the standard PDF card, it can be seen that CeO2 is successfully loaded on the catalysts prepared by the five deposition times, and NiO exists in some catalysts. From the XRD graphs of the monolithic catalysts of Examples 1, 2, and 3 alone, it can be seen that with the increase of deposition time, the peak intensity of CeO2 and NiO both decreases. This may be related to the smaller particle size on the load and the better overall dispersion of the particles. From the XRD of the monolithic catalysts of Examples 3, 4, and 5 alone, it can be seen that with the increase of time, the peak intensity of NiO increases again.
[0074] According to the half-peak width of the diffraction peak of cerium dioxide in the XRD graph, the average particle size of CeO2 grains can be calculated using the Scherrer formula. After calculation, the average particle size of CeO2 grains in the five examples is between 0.1nm and 0.2nm, and within the time range of 30s-1800s, the particle size first decreases with the increase of deposition time, and after more than 900s, the particle size increases with the increase of time.
[0075] 2. Scanning electron microscopy (SEM) characterization
[0076] Figure 6 The scanning electron microscope characterization images of the integral catalysts 30-Ce / Ni-foam, 300-Ce / Ni-foam, and 1800-Ce / Ni-foam of Examples 1, 3, and 5. From the comparison images of Examples 1, 3, and 5 with sizes of 1 mm and 50 μm, it can be seen that the surface of the active components loaded by the electrodeposition method is relatively rough and has uneven cracks. The catalyst 30-Ce / Ni-foam prepared in Example 1 deposited a layer of cerium dioxide on the surface of the carrier, and a small part of the area was not completely covered; the catalyst 300-Ce / Ni-foam prepared in Example 3 deposited more than one layer of cerium dioxide on the surface of the carrier; the catalyst 1800-Ce / Ni-foam prepared in Example 5 deposited multiple layers of cerium dioxide on the surface of the carrier.
[0077] From the comparison diagram of Examples 1, 3, and 5 with a size of 1 μm, it can be seen that the catalyst 30-Ce / Ni-foam prepared in Example 1 has a smaller number of cerium dioxide particles on its surface, and a smaller density of active components on the load; the catalyst 300-Ce / Ni-foam prepared in Example 3 has a larger number of cerium dioxide particles on its surface, and the particle density is moderate; the catalyst 1800-Ce / Ni-foam prepared in Example 5 has the largest number of cerium dioxide particles on its surface, a large density of active components on the load, and little difference in particle size and uniform distribution.
[0078] 3. Activity test
[0079] Figure 7 The activity diagram of the integral catalysts 30-Ce / Ni-foam, 60-Ce / Ni-foam, 300-Ce / Ni-foam, 900-Ce / Ni-foam and 1800-Ce / Ni-foam of Examples 1-5 shows that among the five catalysts deposited for 30-1800s, the catalyst activity first increases and then decreases, and the catalyst 300-Ce / Ni-foam with a deposition time of 300s has the best activity. The temperature required for 300-Ce / Ni-foam to convert 90% of butyl acetate is between 210°C and 220°C, and the temperature required to completely convert butyl acetate is around 230°C.
Claims
1. Application of a cerium-based monolithic catalyst in catalytic oxidation of oxygen-containing volatile organic compound butyl acetate, characterized in that: The cerium-based monolithic catalyst is prepared by electrodeposition, with butyl acetate, an oxygen-containing volatile organic compound, as the catalytic object. The constant deposition voltage, stirring speed and specific deposition time are determined to make the active component CeO2 adhere to the nickel foam carrier in different quantities and densities. The catalyst preparation method comprises the following steps: (1) Cutting the nickel foam carrier into working nickel foam sheets with a length of 1-5 cm, a width of 1-5 cm, and a thickness of 1-2 mm; (2) immersing the entire nickel foam carrier in a hydrochloric acid solution and performing ultrasonic acid washing; after the ultrasonic washing is completed, the acid solution is discarded, the surface of the nickel foam carrier is washed with deionized water, and ethanol is added and ultrasonic washing is performed again; after the ultrasonic washing is completed, the surface is washed again with ethanol; the washed nickel foam is placed in a tubular furnace and vacuum dried to obtain a pure nickel foam carrier; (3) Weigh Ce(NO3)3·6H2O and dissolve it in deionized water, stirring to obtain Ce(NO3)3 electrolyte; (4) Place the prepared Ce(NO3)3 electrolyte in the electrolytic cell, clamp a cleaned nickel foam carrier with an electrode clamp, and connect the electrode clamp to the working electrode. Then connect the calomel electrode and the platinum electrode to the reference electrode and the counter electrode respectively. Fix the position of each electrode with a rubber ring so that the working part of the electrode is completely immersed in the electrolyte. Adjust the electrochemical workstation to the constant voltage deposition mode, set a specific deposition voltage and deposition time, turn on the stirring device, adjust the rotor speed, and start deposition; (5) The deposited nickel foam is removed, placed in a culture dish and sent to an oven for drying; (6) The dried nickel foam is loaded into a porcelain boat, sent into a tubular furnace, and calcined at a certain temperature for a period of time to obtain a cerium-based monolithic catalyst, which is recorded as Ce / Ni-foam; In step (3), the concentration of the prepared Ce(NO3)3 electrolyte is 0.1-0.15 mol / L; In step (4), the deposition voltage is (-1.7)-(-1.8) V, the deposition time is 30s-1800s, and the stirring rotor speed is 300-400r / min; In step (6), the calcination temperature is 400-600°C, the calcination time is 1-3h, and the calcination heating and cooling rates are both 1-5°C / min.
2. The application according to claim 1, characterized in that: In step (2), the concentration of the hydrochloric acid solution is 1-3 mol / L.
3. The application according to claim 1, characterized in that: In step (2), the surface is washed with hydrochloric acid for 5-10 minutes and then washed twice with ethanol, each time for 5-10 minutes.
4. The use according to claim 1, characterized in that: In step (2), the vacuum drying temperature is 60-80°C and the drying time is 6-12h.
5. The use according to claim 1, characterized in that: In step (5), the drying temperature is 60-80°C and the drying time is 6-12h.