A kind of silicate cement clinker and preparation method thereof

By mixing and firing the mine tailings, sludge gasified dry distillation slag, clay and modified red sludge-based catalytic components in a specific proportion, efficient silicate cement clinker is prepared, which solves the problem of mine tailings and sludge Low utilization and environmental pollution problems have achieved economic production and efficient reuse of cement clinker.

CN116462427BActive Publication Date: 2024-11-19DALIAN CEMENT GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310393159.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-11-19
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

The comprehensive utilization rate of mine tailings and sludge gasification dry distillation slag is low, resulting in solid waste storage and environmental pollution problems. The existing pyrolysis dry distillation gasification disposal methods have caused solid waste treatment problems.

Method used

Mining tailings, sludge gasified dry distillation slag, clay and modified red mud-based catalytic components are mixed in a specific proportion, and then grinded and fired to prepare silicate cement clinker, using red mud, desulfurization gypsum and The combined action of fluorite promotes firing and mineral formation.

Benefits of technology

It reduces the production cost of cement clinker, effectively reduces calcination energy consumption, and improves the mechanical properties of cement clinker, realizes efficient reuse of mine tailings and sludge, and solves the problems of solid waste storage and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004176567710000081
    Figure BDA0004176567710000081
  • Figure HDA0004176567720000011
    Figure HDA0004176567720000011
  • Figure HDA0004176567720000012
    Figure HDA0004176567720000012
Patent Text Reader

Abstract

This invention relates to the field of waste recycling technology, specifically to a method for preparing silicate cement clinker using mine tailings and sludge gasification pyrolysis residue. The raw materials used in this method include mine tailings, sludge gasification pyrolysis residue, clay, and modified red mud-based catalyst components. This method can reduce the production cost of cement clinker and has significant economic and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste recycling, and in particular to a method for preparing silicate cement clinker by utilizing mine tailings and sludge gasification dry distillation slag. Background Art

[0002] With the increase of urban population and the development of industrial production, the discharge of mine tailings, urban wastewater and sewage is increasing day by day, which also leads to the increasing risk factor of potential solid waste storage. The sludge in sewage contains some heavy metals, pathogens and toxic organic matter, which will cause land pollution, decay, odor, groundwater pollution and other environmental hazards. In order to deal with the sludge in the city, the pyrolysis and dry distillation gasification treatment method of urban sludge is proposed, but this method will produce a large amount of solid waste such as sludge gasification and dry distillation residue.

[0003] The amount of mine tailings in my country is also very large, but the comprehensive utilization rate of mine tailings is still relatively low, and the disposal of mine tailings is still a problem to be solved. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a method for preparing silicate cement clinker by utilizing mine tailings and sludge gasification dry distillation slag.

[0005] The technical solution adopted by the present invention is:

[0006] A silicate cement clinker is prepared from the following raw materials: 65-80 parts of mine tailings, 10-25 parts of sludge gasification dry distillation residue, 1-5 parts of clay, and 1-5 parts of modified red mud-based catalytic components.

[0007] The modified red mud-based catalytic component comprises the following components in parts by weight: 80-90 parts of red mud, 5-10 parts of desulfurized gypsum and 1-5 parts of fluorite.

[0008] The CaO content in the mine tailings is greater than 45%, and the water content is less than 3%.

[0009] The SiO 2 The content is greater than 45% and the moisture content is less than 3%.

[0010] The SiO in the clay 2 The content is greater than 55% and the moisture content is less than 3%.

[0011] The method for preparing silicate cement clinker comprises the following steps:

[0012] 1) Take 80-90 parts of red mud, 5-10 parts of desulfurized gypsum and 1-5 parts of fluorite, and mix them to obtain a modified red mud-based catalytic component;

[0013] 2) taking mine tailings, sludge gasification dry distillation residue, clay and modified red mud-based catalytic components in proportion and mixing them to obtain a mixture;

[0014] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0015] 4) The raw material is burned to obtain Portland cement clinker.

[0016] The firing temperature in step 4) is 1300-1400° C., and the holding time is 30-60 minutes.

[0017] The modified red mud-based catalyst group added in the present invention contains red mud, desulfurized gypsum and fluorite. Specifically, the iron component in the red mud can undergo sintering reaction with the calcium and aluminum components in mine tailings, sludge gasification dry distillation slag and clay, contributing to the formation of the iron phase in the silicate cement clinker, and its alkaline components such as Na and K can play a fluxing role and promote the burning of clinker. Desulfurized gypsum undergoes a melting and decomposition reaction in the calcination temperature range of 1300-1400°C. On the one hand, the liquid phase produced by melting promotes the burning of clinker, and on the other hand, the CaO produced by decomposition can supplement the calcium source required for the burning of clinker. At the same time, the SO 2 Gas can control the O 2 The addition of fluorite can reduce the melting point of red mud and desulfurized gypsum, and easily form a low eutectic product, which is beneficial to the low-temperature sintering of clinker. The low-temperature melting brought by fluorite can promote the dissociation and clinkerization reaction of silicon, aluminum and calcium components in mine tailings, sludge gasification and dry distillation slag and clay. The iron and aluminum components in red mud can undergo a solid solution reaction with the CaO produced by the decomposition of desulfurized gypsum to form an iron phase solid solution, thereby eliminating the side effects of free calcium oxide.

[0018] In addition to iron components, red mud also contains alkali metal oxides and rare earth oxides. Alkali metal oxides can promote the decomposition of carbonates. Although rare earth oxides have little effect on the decomposition of carbonates, they can significantly improve the burnability of raw materials and promote the formation and development of minerals in clinker, which is beneficial to increase the size of mineral crystals in clinker and promote their uniform distribution. Although the iron components, alkali metal oxides and rare earth elements in red mud are beneficial to the formation of cement clinker, the amount of red mud added needs to be strictly controlled and cannot be excessive. This is because when the rare earth oxide content in red mud is too high, it is easy to cause mineral melting.

[0019] Compared with the prior art, the beneficial technical effects of the present invention are:

[0020] 1. The present invention reuses mine tailings, sludge gasification dry distillation slag and red mud to make silicate cement clinker, which reduces the production cost of cement clinker and has important economic and social benefits.

[0021] 2. The mine tailings in the present invention mainly provide a calcium source, the sludge gasification dry distillation slag mainly provides a silicon source and an effective combustion mass, which can effectively reduce the calcination energy consumption, and the clay mainly provides a silicon source. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1-Figure 11 The following are typical petrographic photographs of the Portland cement clinker obtained in Examples 1-11 respectively. DETAILED DESCRIPTION

[0023] The specific implementation modes of the present invention are described below in conjunction with examples. However, the following examples are only used to illustrate the present invention in detail and are not intended to limit the scope of the present invention in any way.

[0024] Example 1: A method for preparing silicate cement clinker using mine tailings and sludge gasification dry distillation slag, comprising the following steps:

[0025] 1) Take 2.65 kg of red mud, 0.25 kg of desulfurized gypsum and 0.1 kg of fluorite, and mix them to obtain 3 kg of modified red mud-based catalytic component;

[0026] 2) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 3 kg of modified red mud-based catalytic component were taken in proportion and mixed to obtain a mixture;

[0027] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0028] 4) The raw material is fired at 1400°C for 50 minutes to obtain Portland cement clinker.

[0029] Embodiment 2:

[0030] A method for preparing silicate cement clinker by using mine tailings and sludge gasification dry distillation slag, comprising the following steps:

[0031] 1) Take 0.9 kg of red mud, 0.05 kg of desulfurized gypsum and 0.05 kg of fluorite, and mix them to obtain 1 kg of modified red mud-based catalytic component;

[0032] 2) 75 kg of mine tailings, 21 kg of sludge gasification dry distillation residue, 3 kg of clay and 1 kg of modified red mud-based catalytic component were taken in proportion and mixed to obtain a mixture;

[0033] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0034] 4) The raw material is fired at 1350°C for 60 minutes to obtain Portland cement clinker.

[0035] Embodiment 3:

[0036] A method for preparing silicate cement clinker by using mine tailings and sludge gasification dry distillation slag, comprising the following steps:

[0037] 1) Take 1.78 kg of red mud, 0.2 kg of desulfurized gypsum and 0.02 kg of fluorite, and mix them to obtain 2 kg of modified red mud-based catalytic component;

[0038] 2) 80 kg of mine tailings, 13 kg of sludge gasification dry distillation residue, 5 kg of clay and 2 kg of modified red mud-based catalytic component were taken in proportion and mixed to obtain a mixture;

[0039] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0040] 4) The raw material is fired at 1400°C for 30 minutes to obtain Portland cement clinker.

[0041] Embodiment 4:

[0042] A method for preparing silicate cement clinker by using mine tailings and sludge gasification dry distillation slag, comprising the following steps:

[0043] 1) Take 0.9 kg of red mud, 0.08 kg of desulfurized gypsum and 0.02 kg of fluorite, and mix them to obtain 1 kg of modified red mud-based catalytic component;

[0044] 2) 80 kg of mine tailings, 18 kg of sludge gasification dry distillation residue, 1 kg of clay and 1 kg of modified red mud-based catalytic component are taken in proportion and mixed to obtain a mixture;

[0045] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0046] 4) The raw material is fired at 1400°C for 30 minutes to obtain Portland cement clinker.

[0047] Embodiment 5:

[0048] A method for preparing Portland cement clinker comprises the following steps:

[0049] 1) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 3 kg of red mud were mixed to obtain a mixture;

[0050] 2) Grinding the mixed material to a fineness of less than 16% on an 80 μm sieve to obtain a raw material;

[0051] 3) The raw material is fired at 1400°C for 50 minutes to obtain Portland cement clinker.

[0052] Embodiment 6:

[0053] A method for preparing Portland cement clinker comprises the following steps:

[0054] 1) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 3 kg of desulfurized gypsum were mixed to obtain a mixture;

[0055] 2) Grinding the mixed material to a fineness of less than 16% on an 80 μm sieve to obtain a raw material;

[0056] 3) The raw material is fired at 1400°C for 50 minutes to obtain Portland cement clinker.

[0057] Embodiment 7:

[0058] A method for preparing Portland cement clinker comprises the following steps:

[0059] 1) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 3 kg of fluorite are mixed to obtain a mixed material;

[0060] 2) Grinding the mixed material to a fineness of less than 16% on an 80 μm sieve to obtain a raw material;

[0061] 3) The raw material is fired at 1400°C for 50 minutes to obtain Portland cement clinker.

[0062] Embodiment 8:

[0063] A method for preparing Portland cement clinker comprises the following steps:

[0064] 1) Take 2.74 kg of red mud and 0.26 kg of desulfurized gypsum, mix them and obtain 3 kg of catalytic component;

[0065] 2) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 3 kg of catalytic component are taken in proportion and mixed to obtain a mixture;

[0066] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0067] 4) The raw material is fired at 1400°C for 50 minutes to obtain Portland cement clinker.

[0068] Embodiment 9:

[0069] A method for preparing Portland cement clinker comprises the following steps:

[0070] 1) Take 2.9 kg of red mud and 0.1 kg of fluorite and mix them to obtain 3 kg of catalytic component;

[0071] 2) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 3 kg of catalytic component are taken in proportion and mixed to obtain a mixture;

[0072] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0073] 4) The raw material is fired at 1400°C for 50 min to obtain Portland cement clinker.

[0074] Embodiment 10:

[0075] A method for preparing Portland cement clinker comprises the following steps:

[0076] 1) Take 2.2 kg of desulfurized gypsum and 0.8 kg of fluorite, mix them and obtain 3 kg of catalytic component;

[0077] 2) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 3 kg of catalytic component are taken in proportion and mixed to obtain a mixture;

[0078] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0079] 4) The raw material is fired at 1400°C for 50 minutes to obtain Portland cement clinker.

[0080] Embodiment 11:

[0081] A method for preparing Portland cement clinker comprises the following steps:

[0082] 1) Take 17.7 kg of red mud, 1.67 kg of desulfurized gypsum and 0.63 kg of fluorite, and mix them to obtain 20 kg of catalytic components;

[0083] 2) 70 kg of mine tailings, 22 kg of sludge gasification dry distillation residue, 5 kg of clay and 20 kg of catalytic components are taken in proportion and mixed to obtain a mixture;

[0084] 3) Grinding the mixture until the fineness is less than 16% on a 80 μm sieve to obtain a raw material;

[0085] 4) The raw material is fired at 1400°C for 50 minutes to obtain Portland cement clinker.

[0086] The cement clinker of Example 1-11 was sulfur-embedded and solidified, and its surface was polished, and then the petrographic observation was carried out using an optical microscope (the surface of the clinker block was treated with 1% HNO 3 Solution for corrosion and coloring), see Figure 1-Figure 11 .

[0087] Depend on Figures 1 to 11It can be seen that in the clinker petrographic structure obtained in Examples 1-4, alite minerals are well developed, evenly distributed, with complete edges and corners, no rosette or ring-band structure, few inclusions, and no pile aggregation phenomenon; belite minerals are evenly distributed between alite minerals, mostly in the form of well-developed round particles; there is little free calcium oxide in the clinker. The overall petrographic structure shows the characteristics of a good first-class clinker.

[0088] In the clinker petrographic structure obtained in Example 5, alite and belite mineral crystals both showed large aggregation, and the edges of the mineral crystals were missing, and the morphology was not complete. The petrographic structure as a whole showed the characteristics of under-burned clinker, which was the main reason for the decline in the mechanical properties of cement.

[0089] In the clinker petrographic structure obtained in Example 6, a large amount of free calcium oxide appeared, and the alite and belite minerals were irregular in shape. The petrographic structure as a whole showed the characteristics of low-quality clinker, which was also the main reason for the decline in the mechanical properties of cement.

[0090] In the clinker petrographic structure obtained in Example 7, alite and belite minerals are incomplete, most of the surfaces are rough, and no iron phase minerals are observed. The petrographic structure as a whole shows the characteristics of low-quality clinker, which is the main reason for the decline in cement mechanical properties.

[0091] In the clinker petrographic structure obtained in Example 8, the crystal size of alite and belite minerals grew too large, and excessively large crystal size would inhibit their dissolution and hydration, thereby causing a decrease in the mechanical properties of cement.

[0092] In the clinker petrographic structure obtained in Example 9, alite minerals are aggregated, and their grains are missing corners, with rough edges, showing dissociation; and belite minerals are irregular in shape. The overall petrographic structure shows the characteristics of low-quality clinker, which is the main reason for the decline in cement mechanical properties.

[0093] In the clinker petrographic structure obtained in Example 10, alite and belite mineral particles are aggregated, there are many pores, and the presence of iron phase is not observed. The petrographic structure as a whole shows the characteristics of low-quality clinker, which is the main reason for the decline in cement mechanical properties.

[0094] In the clinker petrographic structure obtained in Example 11, the alite and belite mineral particles are incomplete in shape, with missing corners and melting. The petrographic structure as a whole shows the characteristics of low-quality clinker, which is the main reason for the decline in cement mechanical properties.

[0095] The ordinary Portland cement obtained by grinding the Portland cement clinker obtained in Examples 1 to 11 according to the ratio of 95% Portland cement clinker + 5% desulfurized gypsum meets the requirements of "Portland Cement Clinker" GB / T21372-2008. The specific basic properties are shown in Table 1.

[0096] Table 1 Basic properties of ordinary Portland cement made from 95% cement clinker + 5% desulfurized gypsum

[0097]

[0098] The inventors have verified through a large number of experiments that:

[0099] When the catalytic component contains only red mud, due to the lack of liquid phase produced by the melting of desulfurized gypsum and the lack of fluorite to reduce the melting point of red mud, the raw materials cannot reach a completely molten state when fired at 1400°C, affecting the clinker reaction and the formation of clinker. The setting time of the obtained silicate cement is long, and the flexural strength and compressive strength are reduced. When the catalytic component contains only desulfurized gypsum, the desulfurized gypsum melts and decomposes to produce a large amount of CaO, resulting in a large amount of f-CaO in the fired silicate cement clinker, causing the silicate cement to flash, affecting the stability of the cement, and reducing the flexural strength and compressive strength. When the catalytic component contains only fluorite, due to the lack of iron components contained in red mud, the content of iron phase in the fired silicate cement clinker is greatly reduced, and the early flexural strength and compressive strength of the obtained silicate cement are reduced. When the catalytic component lacks fluorite, due to the lack of fluxing effect of low eutectic compounds, the time required for clinker burning is prolonged, and the hydration activity of the clinker minerals formed is reduced, resulting in prolonged cement setting time and reduced flexural strength and compressive strength of cement. When the catalytic component lacks desulfurized gypsum, the high-temperature thermal stability of the clinker minerals formed is reduced, and the clinker minerals are prone to high-temperature dissociation, forming minerals with reduced activity, resulting in prolonged cement setting time and reduced flexural strength and compressive strength of cement. When the catalytic component lacks red mud, it leads to uneven distribution of minerals during clinker burning and reduced iron phase content, which is not conducive to the development of early mechanical properties of cement, resulting in prolonged cement setting time and reduced flexural strength and compressive strength of cement. When the amount of catalytic component added is too large, the rare earth oxide components contained therein will cause mineral melting, affect the hydration activity of minerals such as alite, hinder the development of cement mechanical properties, resulting in prolonged cement setting time and reduced flexural strength and compressive strength of cement.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A Portland cement clinker, characterized in that: The raw materials used in the preparation are: 65-80 parts of mine tailings, 10-25 parts of sludge gasification dry distillation residue, 1-5 parts of clay and 1-5 parts of modified red mud-based catalytic components; The modified red mud-based catalytic component is composed of the following raw materials: 80-90 parts of red mud, 5-10 parts of desulfurized gypsum and 1-5 parts of fluorite.

2. The Portland cement clinker according to claim 1, characterized in that: The CaO content in the mine tailings is greater than 45% and the water content is less than 3%.

3. The Portland cement clinker according to claim 1, characterized in that: The SiO2 content in the sludge gasification dry distillation residue is greater than 45%, and the moisture content is less than 3%.

4. The Portland cement clinker according to claim 1, characterized in that: The SiO2 content in the clay is greater than 55% and the water content is less than 3%.

5. The method for preparing the Portland cement clinker according to claim 1, characterized in that: The following steps are included: 1) Take 80-90 parts of red mud, 5-10 parts of desulfurized gypsum and 1-5 parts of fluorite, and mix them to obtain a modified red mud-based catalytic component; 2) taking mine tailings, sludge gasification dry distillation residue, clay and modified red mud-based catalytic components in proportion and mixing them to obtain a mixed material; 3) Grinding the mixture to obtain raw material; 4) Burning the raw material to obtain Portland cement clinker.

6. The preparation method according to claim 5, characterized in that: The firing temperature in step 4) is 1300-1400° C. and the firing time is 30-60 minutes.

Citation Information

Patent Citations

  • Silicate cement clinker prepared by using marble powder and preparation method thereof

    CN103803819A

  • High-iron belite cement and preparation method thereof

    CN111393047A

  • Preparation method for firing Portland cement clinker by using sludge incineration ash

    CN114057416A

  • Portland cement clinker taking tungsten tailings as raw material and preparation method of Portland cement clinker

    CN114163149A

  • Portland slag cement clinker prepared from stone coal vanadium extraction tailings and preparation method