A composite accelerating anti-corrosion material and preparation method thereof
Through the synergistic effect of mineral blends and anticorrosion components in composite pro-coagulant anticorrosion materials, the problem of sprayed concrete being susceptible to erosion in tunnel engineering is solved, the resistance to sulfate and chloride ion corrosion is improved, and the tunnel structure is extended Service life and reduce production costs.
Patent Information
- Application Number
- CN202310323342.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-03-30
AI Technical Summary
In tunnel engineering, sprayed concrete is susceptible to external environment erosion, resulting in a decrease in mechanical properties and durability. The existing preservatives are high and the production costs are high, which affects construction efficiency and engineering applications.
Using composite pro-coagulant anticorrosion materials, including mineral blends, anticorrosion components, reinforcers, pro-coagulant components and expansion agents, through modification of red mud, calcium carbide slag fine powder, ultrafine mica powder, basalt fiber powder and EVA Components such as glue powder form synergistic effects, shorten the cement hydration time, and improve sulfate corrosion resistance and chloride ion permeability.
Significantly improve the sulfate corrosion resistance and chloride ion permeability of sprayed concrete, extend the service cycle of tunnel structure, reduce the amount of liquid alkali-free quick-coagulant, improve construction effect, and realize the resource utilization of industrial waste, reduce production costs .
Smart Images

Figure CN116462442B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a composite accelerating coagulation type anticorrosive material and a preparation method thereof. Background Art
[0002] Shotcrete is a type of concrete that is formed by sending a concrete mixture of cementitious materials, aggregates, etc. mixed in a certain proportion into a spraying device, and spraying it at high speed onto the sprayed surface with the help of compressed air or other power. Compared with cast concrete, in terms of molding technology, the spray molding process integrates the three processes of transportation, pouring, and tamping, which is easy to operate and greatly improves the construction efficiency of the staff; in terms of physical properties, shotcrete has many characteristics such as short setting time, fast strength growth, and strong bonding force. Therefore, it has gradually become a key structural support material and is widely used in a series of major underground construction projects such as tunnel lining, mine anchor support, and foundation pit support.
[0003] The geological environment in tunnel engineering is complex. Shotcrete, as a protective layer of the tunnel structure, is extremely susceptible to external environmental erosion. For example, sulfate ions and chloride ions in groundwater can cause cracks in the internal structure of shotcrete, while chloride ions can cause corrosion on the surface of the steel bars in the concrete. Under the influence of both, the mechanical properties and durability of shotcrete will be significantly reduced, thus greatly shortening the service life of the tunnel structure. In addition, liquid alkali-free accelerators are essential admixtures in shotcrete, but the mainstream liquid alkali-free accelerators in the market at this stage are all developed with high content of sulfate. Therefore, a large amount of liquid alkali-free accelerators will cause the sulfate ion concentration in the shotcrete to be high, further exacerbating the erosion and degradation of the shotcrete by sulfate.
[0004] Concrete preservatives are important admixtures that can adjust the chemical composition of the cementitious system and enhance the resistance of concrete structures to salt corrosive media. Within a reasonable dosage range, they can significantly improve the concrete's resistance to salt ion corrosion, freeze-thaw resistance, and impermeability. In terms of application areas, concrete preservatives are mainly used in reinforced concrete structures in coastal ports, coastal salt pans, and seawater infiltration areas. Therefore, the academic community is more inclined to study special preservatives for marine engineering concrete, while there is relatively little research on special preservatives for shotcrete. In the prior art, the patent with the publication number CN111333362A on August 25, 2020 discloses a multi-component composite synergist for shotcrete and its preparation method. The composite synergist is prepared from the following raw materials: 20-40% nano-scale silica fume, 30-50% modified mineral powder, 10-20% expansion agent, 0-5% crystal nucleus early strength agent, 1-5% fluidizer, 1-5% sodium tripolyphosphate, 0.5-2% sodium carboxymethyl cellulose, 0.5-2% sodium gluconate, 5-10% sodium thiocyanate, 0-0.5% polypropylene fiber, and 0.05-0.2% silicone defoamer. Among them, the dosage of the composite synergist is 5%-15% of the mass of cement. Obviously, the amount of nano-scale materials in the composite synergist is too large, resulting in high production costs; at the same time, the nano-scale materials themselves have high water requirements, and excessive use will cause the working performance of shotcrete to decline, which is not conducive to its application in actual engineering. The patent with publication number CN113735489A on December 3, 2021 discloses an anti-sulfate corrosion preservative, shotcrete and its preparation method. The anti-sulfate corrosion preservative is prepared from the following raw materials: 30-50 parts of mineral admixture, 10-25 parts of silica fume, 5-15 parts of calcium powder, 5-10 parts of expansion agent, 5-10 parts of silicon dioxide, 0-5 parts of graphene oxide, 0-5 parts of gypsum, 1-2.5 parts of dispersant, 0-0.2 parts of defoamer, and 0-1 parts of surfactant. Among them, the dosage of anti-sulfate corrosion preservative is 8% to 12% of the mass of cement. In this concrete preservative, the amount of mineral admixture is relatively high, resulting in a relative reduction in the amount of alkaline substances in cement, and no early strength component is introduced into the above raw materials. Therefore, the early process of cement hydration and the early strength development of concrete are both delayed to a certain extent, thereby affecting the construction effect of shotcrete. Summary of the invention
[0005] One of the purposes of the present invention is to provide a composite accelerating coagulation anti-corrosion material, which can improve the sulfate corrosion resistance of shotcrete, inhibit the corrosion behavior of chloride ions on the steel bars of the shotcrete layer, enhance the durability of shotcrete, and extend the service life of the tunnel structure; at the same time, accelerate the early process of cement hydration, stimulate the synergistic and complementary effects of anti-corrosion materials and accelerators in shotcrete, reduce the actual dosage of liquid alkali-free accelerators, and improve the construction effect of shotcrete.
[0006] The second object of the present invention is to provide a method for preparing a composite accelerating anti-corrosion material, which can realize the resource utilization of various industrial wastes, reduce the use cost of shotcrete, and simplify the production process of anti-corrosion materials.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] A composite accelerating coagulant anti-corrosion material comprises the following raw materials in parts by mass: 45-55 parts of mineral admixture, 16-25 parts of anti-corrosion components, 8-12 parts of reinforcing agent, 10-15 parts of accelerating coagulant components and 4-8 parts of expansion agent.
[0009] The mineral admixture is composed of carbide slag powder and modified red mud in a weight ratio of 1:2.5-4, and is obtained by mixing the carbide slag powder and modified red mud in a mixer at a speed of 80-120 r / min for 4-6 hours. Carbide slag powder as a mineral admixture can increase the Ca content in the cement liquid phase. 2+ concentration, which accelerates the hydration reaction process of C3A and forms an irregular network structure in the cement liquid phase, effectively shortening the setting time of the cement paste; the content of mineral components such as C3A and β-C2S in the modified red mud is relatively high, which helps to increase the early hydration rate of cement and accelerate the setting and hardening of the cement paste.
[0010] The particle size of the carbide slag fine powder is less than 75 μm;
[0011] The modified red mud is obtained by drying, ball milling, screening and roasting red mud, and the roasting condition is 500-600° C. for 1-2 hours.
[0012] The preparation method of the modified red mud specifically comprises the following steps:
[0013] 1) The weighed red mud is dried in a drying oven. The specific drying conditions are: the drying temperature is in the range of 100 to 105° C., the drying time is in the range of 1 to 3 hours, and the red mud is dried until a constant weight is obtained;
[0014] 2) ball milling the dried red mud, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is in the range of 300 to 350 r / min, and the ball milling time is in the range of 2 to 4 hours;
[0015] 3) Screening the red mud after ball milling, the specific screening conditions are: the test sieve number is 200 meshes, and the particle size of the red mud powder after screening is less than 75 μm;
[0016] 4) The screened red mud is subjected to roasting and activation treatment. The specific roasting conditions are: the roasting temperature is in the range of 500 to 600° C. and the roasting time is in the range of 1 to 2 hours to stimulate the intrinsic activity of the red mud.
[0017] The preparation method of the carbide slag fine powder is as follows: the carbide slag is dried, ball-milled and sieved to obtain the powder.
[0018] The preparation method of the carbide slag fine powder specifically comprises the following steps:
[0019] a) The weighed carbide slag is dried in a drying oven. The specific drying conditions are: the drying temperature is in the range of 120 to 140°C, the drying time is in the range of 2.5 to 3.5 hours, and the carbide slag is dried until constant weight is obtained;
[0020] b) ball milling the dried carbide slag, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is in the range of 200 to 250 r / min, and the ball milling time is in the range of 4 to 5 hours;
[0021] c) Screening the carbide slag after ball milling. The specific screening conditions are: the test mesh number is 200 meshes, the particle size of the carbide slag powder after screening is less than 75 μm, and it has good dispersibility and surface activity.
[0022] The anti-corrosion component is composed of ultrafine mica powder, basalt fiber powder, and EVA glue powder in a weight ratio of 1:1.5 to 2:0.8 to 1.2. The ultrafine mica powder has good electrical insulation, which can significantly improve the resistivity of shotcrete, and can fill the pore structure in the concrete, which increases the density of the concrete on the one hand, and blocks the propagation path of chloride ions in the concrete on the other hand, thereby enhancing the anti-chloride ion permeability of the shotcrete; the basalt fiber powder can prevent the extension of cracks in the concrete in the late corrosion period, and the fiber powder can improve the density of the concrete, delay the chemical reaction in the matrix, reduce the expansion stress in the concrete, and enhance the sulfate corrosion resistance of the shotcrete; the EVA glue powder can promote the formation of calcium aluminate crystals in the cement hydration process, which helps to improve the mechanical strength of the shotcrete at various hydration ages, and the EVA glue powder has good stress cracking resistance and bonding properties, which can effectively improve the durability of the shotcrete.
[0023] The ultrafine mica powder is any one of muscovite powder or sericite powder, and the particle size distribution is in the range of 1500-2000 mesh; the fiber diameter of the basalt fiber powder is in the range of 9-18 μm, and the fiber length is in the range of 30-60 μm; the particle size of the EVA rubber powder is in the range of 30-60 μm. Such ultrafine mica powder, basalt fiber powder, and EVA rubber powder can meet the particle grading of cement. The composite accelerating coagulation anti-corrosion material provided in the present invention is used to replace cement or mineral admixtures when preparing shotcrete, and the cement particle size in the range of 3-32 μm and 32-65 μm contributes more to the later strength of concrete. Therefore, the present invention limits the ultrafine mica powder to the above-mentioned particle size, basalt fiber powder, and EVA rubber powder to the above-mentioned size range.
[0024] The reinforcing agent is silica fume; silica fume can provide a "nucleation" effect for cement hydration products, allowing the hydration products to deposit on the surface of silica fume particles, accelerating the hydration rate of cement minerals, shortening the setting time of cement paste, and improving the compressive strength of concrete at various hydration ages. At the same time, silica fume also has a filling effect, which can reduce the pore structure of concrete and enhance the sulfate erosion resistance and chloride ion penetration resistance of shotcrete.
[0025] The accelerating component is composed of aluminate, carbonate and limestone powder in a weight ratio of 1:1.5 to 2:1.5 to 2.5. Aluminate can accelerate the hydration process of C3A, form a large number of calcium sulfonate crystals in the cement liquid phase, overlap with other hydration products to form an irregular network structure, accelerate the speed of cement coagulation and hardening, and at the same time, the hydrolyzed OH- will promote the dissolution of C3S and the formation of CSH gel in the early stage of hydration, shortening the setting time of cement paste; carbonate can also promote the rapid hydration of C3A, and achieve the accelerating effect by forming a hydration product similar to calcium sulfonate crystals (C3A·3CaCO3·30H2O) in the cement liquid phase; limestone powder can provide a crystallization point position for CSH growth, play a role in microstructure refinement, improve the mechanical properties of the hardened paste, and at the same time, limestone powder can promote the formation of carbon aluminate hydration products, further shortening the setting time of cement paste.
[0026] The aluminate is any one or both of sodium aluminate and potassium aluminate;
[0027] The carbonate is any one or more of sodium carbonate, potassium carbonate or lithium carbonate;
[0028] The particle size of the limestone powder is distributed in the range of 10 to 30 μm.
[0029] The expansion agent is any one or both of magnesium oxide and calcium oxide. The magnesium oxide or calcium oxide crystals will cause volume expansion in the process of forming magnesium hydroxide or calcium hydroxide, which can improve the pore structure inside the concrete, reduce the intrusion of sulfate, and inhibit the further extension of microcracks by filling effect.
[0030] The composite accelerating coagulation anticorrosive material partially replaces cement or mineral admixtures when used, and the admixture amount is 6-10% of the mass of the cementitious material, and is mainly used in the field of construction materials such as shotcrete.
[0031] The preparation method of the composite accelerating coagulant anti-corrosion material provided by the present invention comprises the following steps: uniformly mixing the raw materials in the formula amount, specifically: putting the raw materials in the formula amount into a mixer and mixing them at a speed of 80 to 120 r / min for 4 to 6 hours.
[0032] Compared with the prior art, the present invention has the following advantages:
[0033] 1. It stimulates the synergistic effect of modified red mud, carbide slag powder and EVA powder in cement paste. Modified red mud and carbide slag powder can provide sufficient aluminum and calcium sources. Both can form a large number of fibrous calcium sulfonate crystals in the cement liquid phase under alkaline conditions, effectively promoting the coagulation and hardening of the cement paste; while EVA powder will generate hydroxyl-bearing polymer chains under alkaline conditions. On the one hand, it will be adsorbed on the cement surface and form hydrogen bonds with the surface of CAH gel, further promoting the formation of calcium sulfonate crystals, shortening the cement setting time and improving the mechanical strength of the shotcrete; on the other hand, the hydroxyl-bearing polymer chains can complex the Al in the cement liquid phase. 3+ , Ca 2+ , overlapping with the fibrous structure of calcium aluminate to form an organic-inorganic irregular network interpenetrating structure, which significantly enhances the compactness of the shotcrete.
[0034] 2. The composite accelerating coagulant anti-corrosion material of the present invention is used to optimize the pore structure of shotcrete, avoid volume expansion inside the concrete, improve the sulfate corrosion resistance of shotcrete, and block the migration path of chloride ions inside the concrete, effectively inhibiting the corrosion behavior of chloride ions on the steel bars of the shotcrete layer. Under the combined action of the two, the durability of shotcrete is enhanced, the cost of shotcrete reinforcement and maintenance is reduced, and the service life of the tunnel structure is effectively extended.
[0035] 3. On the premise of using a large amount of mineral admixtures to replace cementitious materials, the introduction of accelerating components accelerates the early process of cement hydration, while stimulating the synergistic and complementary effects of anti-corrosion materials and accelerators in shotcrete, reducing the dosage of liquid alkali-free accelerators, avoiding excessive erosion of shotcrete by sulfates, and effectively improving the construction effect of shotcrete.
[0036] 4. It realizes the resource utilization of various industrial wastes, reduces the use cost of shotcrete, and helps the cement industry to save energy and reduce consumption, and promotes the sustainable development of the circular economy. In addition, no toxic or polluting raw materials are introduced in the process of preparing anti-corrosion materials, which is green, safe and environmentally friendly, and the production process tends to be simplified. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The invention discloses a synergistic mechanism of EVA rubber powder, modified red mud and carbide slag fine powder in cement paste in the composite accelerating coagulant anti-corrosion material provided by the invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Unless otherwise specified, the test materials and reagents used in the examples can be obtained from commercial sources.
[0040] The particle size of the ultrafine mica powder used in each embodiment and comparative example is distributed in the range of 1500-2000 mesh; the fiber diameter of the basalt fiber powder is in the range of 9-18 μm, and the fiber length is in the range of 30-60 μm; the particle size of the EVA rubber powder is in the range of 30-60 μm; and the particle size of the limestone powder is distributed in the range of 10-30 μm.
[0041] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0042] Example 1
[0043] The present embodiment provides a composite accelerating coagulant anti-corrosion material, which is made of the following raw materials in parts by weight: 45 parts of mineral admixture, 25 parts of anti-corrosion component, 12 parts of silica fume, 10 parts of accelerating coagulant component, and 8 parts of magnesium oxide.
[0044] The mineral admixture is prepared by mixing carbide slag fine powder and modified red mud in a weight ratio of 1:2.5.
[0045] The preparation method of the carbide slag fine powder is:
[0046] 1) The weighed carbide slag is dried in a drying oven. The specific drying conditions are: drying temperature is 120°C, drying time is 3.5h, and drying the carbide slag until constant weight is achieved;
[0047] 2) ball milling the dried carbide slag, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is 250r / min, and the ball milling time is 4h;
[0048] 3) The carbide slag after ball milling is screened. The specific screening conditions are: the test mesh number is 200 meshes, the particle size of the carbide slag powder after screening is less than 75 μm, and it has good dispersibility and surface activity.
[0049] The preparation method of the modified red mud is:
[0050] 1) The weighed red mud is dried in a drying oven. The specific drying conditions are: drying temperature is 105° C., drying time is 3 h, and the red mud is dried until constant weight is reached;
[0051] 2) ball milling the dried red mud, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is 350r / min, and the ball milling time is 2h;
[0052] 3) Screening the red mud after ball milling, the specific screening conditions are: the test sieve number is 200 meshes, and the particle size of the red mud powder after screening is less than 75 μm;
[0053] 4) The screened red mud is subjected to a roasting activation treatment, and the specific roasting conditions are: a roasting temperature of 600° C. and a roasting time of 1 h to stimulate the intrinsic activity of the red mud.
[0054] The preparation method of the mineral admixture is:
[0055] 1) Carbide slag fine powder and modified red mud are weighed according to the set weight ratio, and mixed in a mixer. The specific mixing conditions are: the mixer speed is 120r / min, the mixing time is 4h, and after the mixing is uniform, a modified mineral admixture is obtained.
[0056] The anti-corrosion component is prepared by mixing ultrafine mica powder, basalt fiber powder and EVA rubber powder in a weight ratio of 1:1.5:0.8;
[0057] The accelerating coagulant component is prepared by mixing sodium aluminate, sodium carbonate and limestone powder in a weight ratio of 1:2:2.5;
[0058] The preparation method of the above-mentioned composite accelerating coagulant anti-corrosion material is specifically as follows: modified mineral admixtures, anti-corrosion components, reinforcing agents, expansion agents and accelerating coagulant components are weighed in sequence according to the set ratio, and mixing is carried out in a mixer. The specific mixing conditions are: the mixer speed is 120r / min, the mixing time is 8h, and after the mixing is uniform, a composite accelerating coagulant anti-corrosion material is obtained.
[0059] Example 2
[0060] The present embodiment provides a composite accelerating coagulant anti-corrosion material, which is made of the following raw materials in parts by weight: 50 parts of mineral admixture, 20 parts of anti-corrosion component, 10 parts of silica fume, 12 parts of accelerating coagulant component, and 8 parts of calcium oxide.
[0061] The mineral admixture is prepared by mixing carbide slag fine powder and modified red mud in a weight ratio of 1:4.
[0062] The preparation method of the carbide slag fine powder is:
[0063] 1) The weighed carbide slag is dried in a drying oven. The specific drying conditions are: drying temperature is 120°C, drying time is 3.5h, and drying the carbide slag until constant weight is achieved;
[0064] 2) ball milling the dried carbide slag, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is 200r / min, and the ball milling time is 5h;
[0065] 3) The carbide slag after ball milling is screened. The specific screening conditions are: the test mesh number is 200 meshes, the particle size of the carbide slag powder after screening is less than 75 μm, and it has good dispersibility and surface activity.
[0066] The preparation method of the modified red mud is:
[0067] 1) The weighed red mud is dried in a drying oven. The specific drying conditions are: drying temperature is 100° C., drying time is 3 h, and the red mud is dried until constant weight is reached;
[0068] 2) ball milling the dried red mud, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is 350r / min, and the ball milling time is 3h;
[0069] 3) Screening the red mud after ball milling, the specific screening conditions are: the test sieve number is 200 meshes, and the particle size of the red mud powder after screening is less than 75 μm;
[0070] 4) The screened red mud is subjected to a roasting activation treatment, and the specific roasting conditions are: a roasting temperature of 600° C. and a roasting time of 2 h to stimulate the intrinsic activity of the red mud.
[0071] The preparation method of the mineral admixture is:
[0072] 1) Weigh carbide slag powder and modified red mud according to a set ratio, and mix them in a mixer. The specific mixing conditions are: the mixer speed is 100r / min, the mixing time is 5h, and after the mixing is uniform, a modified mineral admixture is obtained.
[0073] The anti-corrosion component is prepared by mixing ultrafine mica powder, basalt fiber powder and EVA rubber powder in a weight ratio of 1:2:0.8;
[0074] The accelerating coagulant component is prepared by mixing sodium aluminate, sodium carbonate and limestone powder in a weight ratio of 1:2:1.5;
[0075] The preparation method of the above-mentioned composite accelerating coagulant anti-corrosion material is specifically as follows: modified mineral admixtures, anti-corrosion components, reinforcing agents, expansion agents and accelerating coagulant components are weighed in sequence according to the set ratio, and mixing is carried out in a mixer. The specific mixing conditions are: the mixer speed is 100r / min, the mixing time is 10h, and after the mixing is uniform, a composite accelerating coagulant anti-corrosion material is obtained.
[0076] Example 3
[0077] The present embodiment provides a composite accelerating coagulant anti-corrosion material, which is made of the following raw materials in parts by weight: 55 parts of mineral admixture, 16 parts of anti-corrosion component, 10 parts of silica fume, 15 parts of accelerating coagulant component, and 4 parts of magnesium oxide.
[0078] The mineral admixture is prepared by mixing carbide slag fine powder and modified red mud in a weight ratio of 1:4.
[0079] The preparation method of the carbide slag fine powder is:
[0080] 1) The weighed carbide slag is dried in a drying oven. The specific drying conditions are: drying temperature is 140°C, drying time is 2.5h, and drying the carbide slag until constant weight is obtained;
[0081] 2) ball milling the dried carbide slag, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is 200r / min, and the ball milling time is 5h;
[0082] 3) The carbide slag after ball milling is screened. The specific screening conditions are: the test mesh number is 200 meshes, the particle size of the carbide slag powder after screening is less than 75 μm, and it has good dispersibility and surface activity.
[0083] The preparation method of the modified red mud is:
[0084] 1) The weighed red mud is dried in a drying oven. The specific drying conditions are: drying temperature is 105° C., drying time is 3 h, and the red mud is dried until constant weight is reached;
[0085] 2) ball milling the dried red mud, the specific ball milling conditions are: using a planetary ball mill, the ball mill speed is 300r / min, and the ball milling time is 4h;
[0086] 3) Screening the red mud after ball milling, the specific screening conditions are: the test sieve number is 200 meshes, and the particle size of the red mud powder after screening is less than 75 μm;
[0087] 4) The screened red mud is subjected to a roasting activation treatment, and the specific roasting conditions are: a roasting temperature of 500° C. and a roasting time of 2 h to stimulate the intrinsic activity of the red mud.
[0088] The preparation method of the mineral admixture is:
[0089] 1) Carbide slag fine powder and modified red mud are weighed according to the set weight ratio, and mixed in a mixer. The specific mixing conditions are: the mixer speed is 80r / min, the mixing time is 6h, and after the mixing is uniform, a modified mineral admixture is obtained.
[0090] The preservative is prepared by mixing ultrafine mica powder, basalt fiber powder and EVA rubber powder in a weight ratio of 1:2:1.2;
[0091] The accelerating coagulant component is prepared by mixing sodium aluminate, sodium carbonate and limestone powder in a weight ratio of 1:1.5:1.5;
[0092] The preparation method of the above-mentioned composite accelerating coagulant anti-corrosion material is specifically as follows: modified mineral admixtures, anti-corrosion components, reinforcing agents, expansion agents and accelerating coagulant components are weighed in sequence according to the set weight ratio, and mixing is carried out in a mixer. The specific mixing conditions are: the mixer speed is 80r / min, the mixing time is 12h, and after the mixing is uniform, a composite accelerating coagulant anti-corrosion material is obtained.
[0093] Comparative Example 1
[0094] The only difference between Comparative Example 1 and Example 1 is that no preservative component is added in Comparative Example 1, and the preparation methods and contents of the remaining raw materials are consistent with those in Example 1.
[0095] Comparative Example 2
[0096] The only difference between Comparative Example 2 and Example 2 is that no accelerating component is added in Comparative Example 2, and the preparation method and content of the remaining raw materials are consistent with those in Example 2.
[0097] Comparative Example 3
[0098] The only difference between Comparative Example 3 and Example 3 is that no reinforcing agent is added in Comparative Example 3, and the preparation methods and contents of the remaining raw materials are consistent with those in Example 3.
[0099] Comparative Example 4
[0100] The only difference between Comparative Example 4 and Example 1 is that no swelling agent is added in Comparative Example 4, and the preparation methods and contents of the remaining raw materials are consistent with those in Example 1.
[0101] Comparative Example 5
[0102] The rest is the same as in Example 1, except that the EVA rubber powder in the raw material is completely replaced by basalt fiber powder.
[0103] Comparative Example 6
[0104] The rest is the same as in Example 1, except that all the sodium carbonate in the raw material is replaced by limestone powder.
[0105] Comparative Example 7
[0106] The rest is the same as Example 1, except that the modified red mud in the raw material is completely replaced by fine powder of calcium carbide slag.
[0107] Application Examples
[0108] The anti-corrosion materials provided in the above embodiments or comparative examples are used to replace part of the cement or mineral admixture to prepare shotcrete, and are added together with cement, coarse aggregate, fine aggregate, fly ash, silica fume, polycarboxylic acid high-performance water reducer, aluminum sulfate-based fluorine-free and alkali-free quick-setting agent and water into a forced mixer for mixing and stirring to obtain shotcrete, and the mixing time is not less than 120 seconds.
[0109] Specifically, the raw materials of shotcrete are: cement, coarse aggregate, fine aggregate, fly ash, silica fume, polycarboxylic acid high-performance water reducing agent, anticorrosive materials in the embodiments or comparative examples, BASF SA type aluminum sulfate series fluorine-free and alkali-free quick setting agent and water. Among them, the cement is Conch PO42.5 grade cement, the coarse aggregate is 5-10mm single-grade limestone crushed stone, and the apparent density is 2.819g / cm 3 , mud content is 0.2%; the fine aggregate is river sand with a fineness modulus of 2.8 and an apparent density of 2.592g / cm 3 The mud content is 0.3%; the fly ash is secondary fly ash, with a specific surface area of 408.1m 2 / kg; the density of silica fume is 2.209g / cm 3 , SiO2 content ≥90%; the polycarboxylic acid high-performance water-reducing agent adopts HLP-MH240 produced by Ningbo Conch Material Technology Co., Ltd., with a solid content of 40%, a water reduction rate of 32%, and the dosage is adjusted according to the slump (210±10) mm.
[0110] kg / m 3 The proportion of each raw material in shotcrete is shown in Table 1. The amount of anti-corrosion material is 6% or 10% of the mass of cementitious material, the amount of BASF SA type aluminum sulfate-based fluorine-free and alkali-free liquid accelerator is 7% or 6% of the mass of cementitious material, and the sand ratio is 50%.
[0111] Table 1
[0112]
[0113] The construction method of shotcrete is: wet mixing method is used for spraying construction. According to the designed mix ratio, the weighed cement, silica fume, fly ash, river sand, crushed stone, anti-corrosion materials, polycarboxylic acid high-performance water reducing agent and water are added into the forced mixer in sequence. After being mixed evenly, they are loaded into the sprayer. High-pressure air is used to deliver the concrete to the nozzle to mix with the accelerator, and then the concrete is sprayed onto the surface of the tunnel surrounding rock at high speed.
[0114] According to the requirements of Chinese industry standard JGJ / T372-2016 "Technical Code for Application of Shotcrete", the setting time of cement paste mixed with aluminum sulfate-based fluorine-free and alkali-free liquid quick-setting agent and composite accelerating anti-corrosion material was tested. At the same time, the penetration method was used to test the compressive strength of shotcrete at a hydration age of 1d. After curing for 7d under standard conditions, the shotcrete specimens were prepared from the concrete slab by cutting method. The compressive strength test used a 100mm×100mm×100mm specimen, which was cured to 28d under standard conditions. The compressive strength test was carried out according to the requirements of Chinese national standard GB / T50081 "Standard Test Method for Mechanical Properties of Ordinary Concrete". In addition, the above concrete specimens were systematically evaluated for their sulfate corrosion resistance using corrosion resistance coefficient tests and dry-wet cycle tests in accordance with the methods specified in GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete". At the same time, the chloride ion diffusion capacity of the concrete was measured to evaluate the concrete's resistance to chloride ion penetration. The cement brand used in the following experiments is Conch Cement, model PO42.5.
[0115] The performance test results of each embodiment, weight ratio and control group are shown in Table 2. The control group is a concrete sample with only aluminum sulfate-based fluorine-free and alkali-free liquid quick-setting agent added but no anti-corrosion material added, and other raw materials and dosages are the same.
[0116] Table 2 Performance test statistical results
[0117]
[0118] It can be clearly seen from Table 1 that the composite accelerating anti-corrosion material provided by the present invention can significantly enhance the sulfate corrosion resistance and chloride ion permeability resistance of shotcrete. In Example 1, the corrosion resistance coefficient of the concrete is 1.21, the sulfate corrosion resistance grade is KS150 and above, and the 28d electrical flux is 772C. According to the statistical results of the performance tests of the control group and Examples 1-3, without affecting the working performance of the shotcrete, the introduction of the anti-corrosion material can effectively reduce the dosage of the aluminum sulfate-based fluorine-free and alkali-free quick-setting agent, while improving the compressive strength of the cement mortar at each hydration age, and significantly enhancing the sulfate erosion resistance and chloride ion permeability of the shotcrete, extending the service life of the tunnel structure; according to the statistical results of the performance tests of Example 1 and Comparative Example 1, the anti-corrosion component can play a key role in resisting aluminum sulfate erosion and inhibiting chloride ion penetration; according to the statistical results of the performance tests of Example 2 and Comparative Example 2, the introduction of the accelerating coagulation component in the preservative can shorten the setting time of the cement paste, and promote the early strength development of the cement, effectively avoiding the problem of poor construction effect caused by the large amount of mineral admixtures replacing the cementitious material; according to the statistical results of the performance tests of Example 3 and Comparative Example 3, the reinforcing agent helps to optimize the pore structure inside the concrete, while improving the compactness of the concrete, achieving an effective improvement in the compressive strength at each hydration age, and can further enhance the sulfate erosion resistance and chloride ion permeability of the shotcrete to a certain extent; by implementing According to the statistical results of the performance tests of Example 1 and Comparative Example 4, the expansive agent can produce volume expansion in the early stage of concrete coagulation and hardening, inhibit the formation and extension of microcracks in the concrete, and thus help to improve the mechanical strength of the concrete, and can also effectively enhance the ability of the shotcrete to resist sulfate and chloride ion corrosion and degradation; according to the statistical results of the performance tests of Example 1 and Comparative Example 5, replacing all the EVA rubber powder in the anti-corrosion component with basalt fiber powder will significantly weaken the sulfate corrosion resistance and chloride ion permeability resistance of the shotcrete, which is not conducive to the long-term service of the tunnel structure ... According to the statistical results of the performance tests of Example 6, replacing all the sodium carbonate in the accelerating component with limestone powder will lead to a prolonged setting time of the cement slurry and relatively reduce the early strength of the concrete; according to the statistical results of the performance tests of Example 1 and Comparative Example 7, replacing all the modified red mud in the mineral admixture with fine carbide slag powder will lead to an excessively high content of fine carbide slag powder in the cementitious material, causing a large amount of Ca(OH)2 in the cement liquid phase to precipitate, significantly reducing the later strength of the shotcrete, and also causing certain negative impacts on the concrete's resistance to sulfate erosion and chloride ion permeability.
[0119] The detailed description of a composite accelerating anti-corrosion material and a preparation method with reference to the above-mentioned embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A composite accelerating anti-corrosion material, characterized in that: The composite accelerating coagulation anticorrosive material comprises the following raw materials by weight: 45-55 parts of mineral admixture, 16-25 parts of anticorrosive component, 8-12 parts of reinforcing agent, 10-15 parts of accelerating coagulation component, and 4-8 parts of expansion agent; The mineral admixture is composed of carbide slag fine powder and modified red mud in a weight ratio of 1:2.5-4; the modified red mud is obtained by drying, ball milling, screening and roasting red mud, and the roasting condition is 500-600°C for 1-2h; The anti-corrosion component is composed of ultrafine mica powder, basalt fiber powder and EVA rubber powder in a weight ratio of 1:1.5~2:0.8~1.2; The accelerating coagulant component is composed of aluminate, carbonate and limestone powder in a weight ratio of 1:1.5~2:1.5~2.5; the carbonate is any one or more of sodium carbonate, potassium carbonate or lithium carbonate; The reinforcing agent is silica fume.
2. The composite accelerating coagulant anticorrosive material according to claim 1, characterized in that: The particle size of the carbide slag fine powder is less than 75 μm.
3. The composite accelerating coagulant anticorrosive material according to claim 1, characterized in that: The expansion agent is any one or both of magnesium oxide and calcium oxide.
4. The composite accelerating coagulant anticorrosive material according to claim 1, characterized in that: The composite accelerating coagulation anticorrosive material partially replaces cement or mineral admixture when used, and the admixture amount is 6-10% of the mass of the cementitious material.
5. A method for preparing a composite accelerating anti-corrosion material according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: uniformly mixing the raw materials in the formula amount.
6. Use of the composite accelerating anti-corrosion material as claimed in claim 1 in shotcrete.
Citation Information
Patent Citations
Low-dosage high-early-strength alkali-free liquid accelerator and preparation method thereof
CN111333362A
Sulfate-erosion-resistant preservative, sprayed concrete and preparation method of sulfate-erosion-resistant preservative
CN113735489A
Modified concrete expansive agent
CN106348643A
Quick setting agent for spraying, spraying material, and spray construction method using the same
JP2011001244A