A nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material and preparation method thereof
The preparation of nitrogen-phosphorus double-doped three-dimensional porous carbon materials solves the problems of high cost and poor selectivity of existing carbon-based materials, achieves efficient removal of heavy metal ions in water, and provides a low-cost, simple preparation solution. , suitable for heavy metal pollution treatment.
Patent Information
- Application Number
- CN202310487257.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing carbon-based adsorption materials have high costs, difficulty in preparation, and poor selectivity when removing heavy metal ions from water. Moreover, the hydrophobic structure of unmodified surface functional groups has a low removal rate of ions in water, and cannot effectively solve the problem of heavy metal pollution.
Nitrogen and phosphorus double-doped three-dimensional porous carbon materials are used to generate nitrogen and phosphorus double-doped polymers through the polymerization reaction of melamine and phytic acid. They are prepared in one step by combining sodium alginate and cobalt ions to form carbon with rich pore structure and large specific surface area. The material is calcined at high temperature and etched to form a porous structure, and the doping amount of nitrogen and phosphorus elements is controlled to improve the adsorption performance.
A low-cost, simple preparation of nitrogen-phosphorus double-doped three-dimensional porous carbon material with high specific surface area and porous structure has been achieved, which significantly improves the removal rate of heavy metal ions, especially the removal effect in aqueous solution. It is suitable for Heavy metal separation.
Smart Images

Figure CN116492984B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon-based adsorption materials, and in particular to a nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material and a preparation method thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] With the rapid development of industry and agriculture, heavy metal pollution is becoming increasingly serious. Heavy metals are not easily degraded and can enter organisms through the food chain, posing a great threat to human health and the living environment. At present, the main methods for treating heavy metals are chemical precipitation, ion exchange, membrane separation, electrochemical method and adsorption. In comparison, adsorption has the characteristics of simple operation and low cost, and is considered to be one of the most effective methods for heavy metal separation.
[0004] Adsorption is the separation of heavy metals using solid materials with high specific surface area. The separation effect mainly depends on the specific surface area, pore structure and functional groups on the surface of the adsorbent. Current adsorbents can be divided into natural adsorption materials, biological adsorption materials and synthetic materials according to their sources.
[0005] Natural materials include inorganic materials such as zeolite, kaolin, diatomaceous earth, and organic materials such as wood fiber, sawdust, rice husks, chitosan and its modified materials. They are widely available and easy to obtain, but have disadvantages such as small adsorption capacity and poor selectivity.
[0006] Biological adsorption materials such as bacteria, fungi, Bacillus, yeast, etc. have high treatment efficiency and less secondary pollution, but the adsorption capacity is not high and the strain selection is time-consuming.
[0007] Among synthetic materials, porous materials and nanomaterials have high specific surface area and adjustable pore size and have received extensive attention. Activated carbon fiber, graphene, carbon nanotubes, porous carbon materials, etc. have excellent separation performance. However, the current carbon-based materials have high cost and are difficult to prepare. In addition, unmodified carbon nanotubes, graphene activated carbon, etc. have few surface functional groups and present a hydrophobic structure. The removal rate of ions in water is not high and the selectivity is poor. Therefore, it is necessary to modify or dope the carbon material to improve its interaction with heavy metal ions in aqueous solution. Existing doped carbon materials are mainly used as electrode materials to prepare electrochemical sensors for pollutant removal; or polyacrylonitrile, polypyrrole, polyaniline, polythiophene, etc. are used as carbon and nitrogen precursors, which are costly. Summary of the invention
[0008] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material and a preparation method thereof. The nitrogen-phosphorus dual-doped three-dimensional porous carbon material provided by the present invention is simple to prepare, the raw materials are cheap and readily available, it has a rich pore structure and a large specific surface area, and its doping amount can be effectively controlled, so it is suitable for heavy metal separation.
[0009] In order to achieve the above object, the present invention provides the following technical solutions:
[0010] In a first aspect of the present invention, a method for preparing a nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material is provided, comprising the following steps:
[0011] The melamine and phytic acid are polymerized in a solution to obtain a nitrogen-phosphorus dual-doped polymer, wherein the mass ratio of melamine to phytic acid is 3-7:2-4;
[0012] The nitrogen-phosphorus dual-doped polymer and the sodium alginate solution are uniformly mixed to obtain a mixed solution, wherein the mass percentage of the sodium alginate solution is 2%-5%, and the mass ratio of the nitrogen-phosphorus dual-doped polymer to the sodium alginate is 0.05-0.5:1;
[0013] The mixed solution is added dropwise to the cobalt ion solution, and stirring is continued during the adding process to form gel particles;
[0014] After washing, the gel particles were frozen in liquid nitrogen and then freeze-dried;
[0015] The freeze-dried particles were calcined in an inert atmosphere at a temperature of 450-550°C for a time of 0.5-2 h;
[0016] The calcined product is ground into powder, etched in an acid solution to remove cobalt particles, and then the material is washed and dried to obtain a nitrogen-phosphorus dual-doped three-dimensional porous carbon material.
[0017] Melamine and phytic acid undergo polymerization to form a macromolecular polymer, which is then dispersed in a sodium alginate solution as a nitrogen and phosphorus source to achieve uniform doping.
[0018] In some embodiments, during the polymerization reaction of melamine and phytic acid, the phytic acid solution is added dropwise to the melamine solution in a dropwise manner to ensure the uniformity of the reaction.
[0019] Preferably, the concentration of the melamine solution is 0.2-0.6 mol·L -1 ; The mass fraction of phytic acid solution is 60-75%.
[0020] In some embodiments, the concentration of the cobalt ion solution is 1-3 mol / L.
[0021] In some embodiments, the acid solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 2-6 mol / L.
[0022] Preferably, in order to remove the metal cobalt particles during the etching process, the powder obtained by grinding the calcined product is placed in a hydrochloric acid solution, and the hydrochloric acid solution is heated to 65-75° C. and reacted for 10-15 hours.
[0023] In some embodiments, the calcination temperature is 470-520° C., and the calcination time is 0.7-1.2 h.
[0024] Preferably, the heating rate during the calcination process is 2-4°C / min.
[0025] In some embodiments, the inert atmosphere is an argon atmosphere.
[0026] In a second aspect, the present invention provides a nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material prepared by the preparation method.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1) The present invention selects melamine, phytic acid and sodium alginate as nitrogen and phosphorus sources, which is simple to prepare and the raw materials are cheap and readily available;
[0029] 2) The present invention adds a polymer containing nitrogen and phosphorus elements to a precursor solution, and through the chelation of the precursor solution and metal ions, a carbon-based material with dual element doping can be obtained in a one-step method. And by adjusting the amount of polymer added, the doping amount of nitrogen and phosphorus elements can be effectively regulated, which helps to achieve quantitative doping of heteroelements. At the same time, the introduced metal ions generate metal nanoparticles in situ during the high-temperature heating process, and a porous structure can be obtained after etching it later, thereby increasing the specific surface area of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0031] Figure 1 The scanning electron microscope image (a) and transmission electron microscope image (b) of the nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material prepared in Example 1.
[0032] Figure 2 This is a bar graph showing the removal rates of various heavy metal ions by the nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material prepared in Example 1. DETAILED DESCRIPTION
[0033] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0034] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0035] Example 1
[0036] The preparation of nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material includes the following steps:
[0037] (1) Prepare 0.4 mol·L -1 100 mL of melamine solution was added and stirred by magnetic heating in a water bath to fully dissolve the melamine and obtain a uniform and transparent melamine solution.
[0038] (2) At room temperature, 5 mL of phytic acid (70% by mass) solution was added dropwise to the above solution. With the addition of phytic acid, white flocculent precipitates were generated in the solution. The polymer precipitates were collected by centrifugal washing.
[0039] (3) Disperse 0.2 g of the precipitate prepared in step (2) into 100 mL of a 2% sodium alginate solution and stir for 10 h at room temperature to mix the mixture thoroughly. Since the sodium alginate solution has a certain viscosity, the stirring time should be appropriately extended to obtain a uniform mixed solution.
[0040] (4) Configuration with 1 mol L -1 200 mL of cobalt nitrate solution was added and a uniformly dispersed cobalt ion solution was obtained by magnetic stirring at room temperature.
[0041] (5) 100 mL of the mixed solution of polymer and sodium alginate in step (3) is added dropwise to the cobalt ion solution in step (4) through a peristaltic pump to form gel particles. During the dropwise addition process, magnetic stirring is required at a low speed in order to evenly disperse the cobalt ions in the solution.
[0042] (6) The obtained gel particles were repeatedly rinsed with deionized water, rapidly frozen with liquid nitrogen, and then transferred to a freeze dryer for drying.
[0043] (7) The dried particles were collected and placed in a quartz boat, and then transferred to a tube furnace for heating under inert gas protection (500°C, 1 h, heating rate 3°C / min, argon atmosphere). After heating was completed, they were naturally cooled to room temperature and taken out.
[0044] (6) Grind the heated composite material into powder and then disperse it into 2 mol L -1 The metal cobalt ions are etched in a hydrochloric acid solution. In order to fully etch the metal cobalt element, the solution is heated to 70°C and the reaction is carried out for 12 hours, with condensation and reflux during the heating process.
[0045] (7) After the reaction is completed, the product in step (6) is fully centrifuged and washed with deionized water until the solution is neutral, and then transferred to a forced air drying oven for drying to obtain a nitrogen and phosphorus doped three-dimensional porous carbon material (the nitrogen and phosphorus doping ratio is 1%).
[0046] The scanning electron microscopy and transmission electron microscopy images of the prepared nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material are shown in Figure 1 As shown, the structure of the adsorption material is a three-dimensional structure formed by interlaced carbon nanobelts, and the metal cobalt particles are etched to form a porous structure with a size of about 5nm, in which the elements nitrogen and phosphorus are evenly distributed in the carbon material.
[0047] Weigh 0.05 g of the prepared nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material and put it into 50 mL of heavy metal solution at room temperature for static adsorption experiment. The heavy metal ion is Cu 2+ , Ni 2+ , Zn 2+ ,Cr 2+ , Pb 2+ The initial concentration was 0.1 mmol / L. After 12 hours of adsorption, the supernatant was centrifuged and filtered. The concentration of heavy metal ions in the solution before and after adsorption was tested by ICP-AES, and the removal rate was calculated. Figure 2 As shown, it can be seen that the adsorption material has a good effect on Cu 2+ The removal rate of Ni is 80%. 2+ The removal rate of Zn was 83%. 2+ The removal rate of Pb was 82%. 2+ The removal rate of Cr 2+ The removal rate is 88%.
[0048] Example 2
[0049] The preparation of nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material includes the following steps:
[0050] (1) Prepare 0.4 mol·L -1 100 mL of melamine solution was added and stirred by magnetic heating in a water bath to fully dissolve the melamine and obtain a uniform and transparent melamine solution.
[0051] (2) At room temperature, 5 mL of phytic acid (70% by mass) solution was added dropwise to the above solution. With the addition of phytic acid, white flocculent precipitates were generated in the solution. The polymer precipitates were collected by centrifugal washing.
[0052] (3) Disperse 1 g of the above-prepared precipitate into 100 mL of 2% sodium alginate solution and stir for 10 h at room temperature to mix the mixture thoroughly. Since the sodium alginate solution has a certain viscosity, the stirring time should be appropriately extended to obtain a uniform mixture.
[0053] (4) Configuration with 1 mol L -1 200 mL of cobalt nitrate solution was added and a uniformly dispersed cobalt ion solution was obtained by magnetic stirring at room temperature.
[0054] (5) 100 mL of the mixed solution of polymer and sodium alginate was added dropwise into the cobalt ion solution through a peristaltic pump to form gel particles. During the dropwise addition process, magnetic stirring was required at a low speed in order to evenly disperse the cobalt ions in the solution.
[0055] (6) The obtained gel particles were repeatedly rinsed with deionized water, rapidly frozen with liquid nitrogen, and then transferred to a freeze dryer for drying.
[0056] (7) The dried particles were collected and placed in a quartz boat, and then transferred to a tube furnace for heating under inert gas protection (500°C, 1 h, heating rate 3°C / min, argon atmosphere). After heating was completed, they were naturally cooled to room temperature and taken out.
[0057] (6) Grind the heated composite material into powder and then disperse it into 2 mol L -1 The metal cobalt ions are etched in a hydrochloric acid solution. In order to fully etch the metal cobalt element, the solution is heated to 70°C and the reaction is carried out for 12 hours, with condensation and reflux during the heating process.
[0058] (7) After the reaction is completed, the above product is fully centrifuged and washed with deionized water until the solution is neutral, and then transferred to a forced air drying oven for drying to obtain a nitrogen and phosphorus doped three-dimensional porous carbon material (the nitrogen and phosphorus doping ratio is 3%).
[0059] Example 3
[0060] The preparation of nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material includes the following steps:
[0061] (1) Prepare 0.6 mol·L -190 mL of melamine solution was added and stirred by magnetic heating in a water bath to fully dissolve the melamine and obtain a uniform and transparent melamine solution.
[0062] (2) At room temperature, 5 mL of phytic acid (mass fraction 65%) solution was added dropwise to the above solution. With the addition of phytic acid, white flocculent precipitates were generated in the solution. The polymer precipitates were collected by centrifugal washing.
[0063] (3) Disperse 1 g of the above-prepared precipitate into 100 mL of 4% sodium alginate solution and stir for 10 h at room temperature to mix the mixture thoroughly. Since the sodium alginate solution has a certain viscosity, the stirring time should be appropriately extended to obtain a uniform mixture.
[0064] (4) Configuration with 2 mol L -1 200 mL of cobalt nitrate solution was added and a uniformly dispersed cobalt ion solution was obtained by magnetic stirring at room temperature.
[0065] (5) 100 mL of the mixed solution of polymer and sodium alginate was added dropwise into the cobalt ion solution through a peristaltic pump to form gel particles. During the dropwise addition process, magnetic stirring was required at a low speed in order to evenly disperse the cobalt ions in the solution.
[0066] (6) The obtained gel particles were repeatedly rinsed with deionized water, rapidly frozen with liquid nitrogen, and then transferred to a freeze dryer for drying.
[0067] (7) The dried particles were collected and placed in a quartz boat, and then transferred to a tube furnace for heating under inert gas protection (500°C, 1 h, heating rate 3°C / min, argon atmosphere). After heating was completed, they were naturally cooled to room temperature and taken out.
[0068] (6) Grind the heated composite material into powder and then disperse it into 2 mol L -1 The metal cobalt ions are etched in a hydrochloric acid solution. In order to fully etch the metal cobalt element, the solution is heated to 75°C and the reaction is carried out for 10 hours, with condensation and reflux during the heating process.
[0069] (7) After the reaction is completed, the product is fully centrifuged and washed with deionized water until the solution is neutral, and then transferred to a forced air drying oven for drying to obtain a nitrogen and phosphorus dual-element doped three-dimensional porous carbon material.
[0070] Weigh 0.05 g of the nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material prepared in Example 1-3 and put it into 50 mL of heavy metal solution at room temperature for a static adsorption experiment. The heavy metal ion is Cu 2+ , Ni 2+, Zn 2+ ,Cr 2+ , Pb 2+ The initial concentration was 0.1 mmol / L. After 12 hours of adsorption, the supernatant was centrifuged and filtered. The concentration of heavy metal ions in the solution before and after adsorption was tested by ICP-AES, and the removal rate was calculated. See Table 1.
[0071] Table 1 Removal rate of various metal elements by adsorption materials prepared in Examples 1-3
[0072]
[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material, characterized in that: The steps include: The melamine and phytic acid are polymerized in a solution to obtain a nitrogen-phosphorus dual-doped polymer, wherein the mass ratio of melamine to phytic acid is 3-7:2-4; The nitrogen-phosphorus dual-doped polymer and the sodium alginate solution are uniformly mixed to obtain a mixed solution, wherein the mass percentage of the sodium alginate solution is 2%-5%, and the mass ratio of the nitrogen-phosphorus dual-doped polymer to the sodium alginate is 0.05-0.5:1; The mixed solution is added dropwise to the cobalt ion solution, and stirring is continued during the adding process to form gel particles; After washing, the gel particles were frozen in liquid nitrogen and then freeze-dried; The freeze-dried particles were calcined in an inert atmosphere at a temperature of 450-550°C for a time of 0.5-2 h; The calcined product is ground into powder, etched in an acid solution to remove cobalt particles, and then the material is washed and dried to obtain a nitrogen-phosphorus dual-doped three-dimensional porous carbon material.
2. The method for preparing the nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 1, characterized in that: During the polymerization reaction of melamine and phytic acid, the phytic acid solution is added dropwise into the melamine solution.
3. The method for preparing the nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 2, characterized in that: The concentration of the melamine solution is 0.2-0.6 mol·L -1 ; The mass fraction of phytic acid solution is 60-75%.
4. The method for preparing the nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 1, characterized in that: The concentration of the cobalt ion solution is 1-3 mol / L.
5. The method for preparing the nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 1, characterized in that: The acid solution is a hydrochloric acid solution, and the concentration of the hydrochloric acid solution is 2-6 mol / L.
6. The method for preparing the nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 5, characterized in that: During the etching process, the powder ground from the calcined product is placed in a hydrochloric acid solution, the hydrochloric acid solution is heated to 65-75° C., and the reaction is carried out for 10-15 hours.
7. The method for preparing the nitrogen-phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 1, characterized in that: The calcination temperature is 470-520° C., and the calcination time is 0.7-1.2 h.
8. The method for preparing the nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 7, characterized in that: The heating rate during the calcination process is 2-4°C / min.
9. The method for preparing the nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material according to claim 1, characterized in that: The inert atmosphere is an argon atmosphere.
10. A nitrogen and phosphorus dual-doped three-dimensional porous carbon heavy metal adsorption material, characterized in that: Prepared by the preparation method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Nitrogen and cobalt double-doped porous carbon composite bifunctional oxygen catalyst and preparation method and application thereof
CN107604375A
Carbon-doped transition metal oxide composite material and preparation method and application thereof
CN109148901A