A magnetic humic acid resin adsorbent and preparation method thereof

Through the preparation of magnetic humic acid resin adsorbents, the ternary composite structure of nano-ferric-phenolic resins is used to solve the problems of poor selectivity and difficulty in recycling of existing adsorbents, and efficient and economical large-scale sewage treatment is achieved, which is suitable for industrial applications.

CN116492993BActive Publication Date: 2024-12-03CHINA UNIV OF MINING & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310467807.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-12-03
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The existing water treatment adsorbents have poor selectivity and difficulty in recycling. Commonly used adsorbents such as activated carbon have poor stability in acidic environments and have a long treatment cycle, making it difficult to achieve efficient and economical large-scale wastewater treatment.

Method used

The preparation method of magnetic humic acid resin adsorbent is adopted, and the nano-ferrous mixture solution is combined with phenolic resin and humic acid to form a ternary composite structure of nano-ferrous resin, and the rich oxygen-containing functional groups of humic acid and nano-ferrous Magnetic properties improve adsorption selectivity and material regeneration ability.

Benefits of technology

It realizes high selectivity and high efficiency heavy metal ion adsorption, short adsorption equilibrium time, high material stability, suitable for large-scale sewage treatment, and significantly reduces the treatment cost through multiple regeneration, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116492993B_ABST
    Figure CN116492993B_ABST
Patent Text Reader

Abstract

The present invention relates to a magnetic humic acid resin adsorbent and a preparation method thereof, which are used to solve the problems of poor selectivity and difficult recovery of existing water treatment adsorbents. The preparation method of the magnetic humic acid resin adsorbent of the present invention comprises the following steps: S100: preparing an iron-ferrous mixed solution; S200: adding a humic acid solution, ammonia water, and a phenolic resin to the iron-ferrous mixed solution obtained in step S100 in sequence, and reacting at 80-110°C for 2.5-4h; S300: adding a solution containing calcium ions to the liquid after the reaction in step S200, stirring and cooling to room temperature, collecting precipitation, rinsing the precipitation to neutrality, and drying to obtain a magnetic humic acid resin adsorbent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water treatment, and in particular to a magnetic humic acid resin adsorbent and a preparation method thereof. Background Art

[0002] Industrial wastewater has a complex composition and contains a large number of toxic and harmful substances. It not only contains highly toxic heavy metal ions, but also contains high concentrations of organic pollutants, making it difficult to treat. At present, the main methods for treating wastewater are chemical precipitation, ion exchange, physical and chemical adsorption, and biological treatment. Among them, the chemical method generally requires the addition of a large amount of chemical reagents, which determines that there will be secondary pollution after chemical treatment, such as the generation of a large amount of waste residue. There is currently no better disposal method for these waste residues, so there is a huge negative impact on its application in engineering and sustainable development; the ion exchange method has low energy consumption, simple operation, and good treatment effect, but the treatment cost is relatively high; and the adsorption method has received widespread attention due to its price advantage, simple operation and high efficiency.

[0003] Commonly used adsorbents such as activated carbon, alumina, zeolite molecular sieves, etc. have high adsorption capacity, stable structure, and wide application range, but most of them are single-use and have long processing cycles, that is, a long time to reach equilibrium, generally requiring about 20 hours, and subsequent recovery is difficult; at the same time, they are easily affected by the acidity of wastewater and have poor adsorption selectivity. Summary of the invention

[0004] In view of the above analysis, the embodiments of the present invention aim to provide a magnetic humic acid resin adsorbent and a preparation method thereof, so as to solve the problems of poor selectivity and difficult recovery of existing water treatment adsorbents.

[0005] In one aspect, the present invention provides a method for preparing a magnetic humic acid resin adsorbent, comprising the following steps:

[0006] S100: preparing a ferrous-ferrous mixed solution;

[0007] S200: adding humic acid solution, ammonia water and phenolic resin to the ferrous-ferrous mixed solution obtained in step S100 in sequence, and reacting at 80-110° C. for 2.5-4 hours;

[0008] S300: adding a solution containing calcium ions to the liquid after the reaction in step S200, stirring and cooling to room temperature, collecting precipitates, washing the precipitates to neutrality, and drying to obtain a magnetic humic acid resin adsorbent.

[0009] Furthermore, in step S100:

[0010] The iron-ferrous mixed solution contains Fe 3+ , Fe 2+ A solution of Fe 3+with Fe 2+ The molar ratio is 1:1 to 2:1;

[0011] The ferrous-ferrous mixed solution is prepared by dissolving FeCl3·6H2O and FeSO4·7H2O in water.

[0012] Furthermore, in step S200:

[0013] The concentration of the humic acid solution is 0.01 to 0.015 g / mL;

[0014] The ratio of the mass of the humic acid to the sum of the mass of FeCl3·6H2O and FeSO4·7H2O is 1:25 to 1:15;

[0015] The mass fraction of the ammonia water is 25%, and the volume ratio of the ammonia water to the humic acid solution is 5:1;

[0016] The mass ratio of the phenolic resin to humic acid is 1:1.

[0017] Further, in the step S300: the concentration of calcium ions in the calcium ion-containing solution is 1 mol / L;

[0018] The precipitate is collected by a permanent magnet;

[0019] The precipitate is washed with deionized water until the pH value is neutral, and dried at 90-120°C.

[0020] Furthermore, the phenolic resin is a micro-mesoporous phenolic resin, and the preparation method of the micro-mesoporous phenolic resin comprises the following steps:

[0021] S201: Preparation of carbon precursor;

[0022] Phenol, formaldehyde and sodium hydroxide are sequentially added into a container to undergo polycondensation reaction to obtain a translucent brown-red product that is completely soluble in water, and then dehydrated under reduced pressure to obtain a water-soluble phenolic resin adhesive with a solid content in the range of 70 to 80% as a precursor;

[0023] S202: Preparation of micro-mesoporous phenolic resin;

[0024] Ethylene glycol and FeCl2 are sequentially added to the precursor obtained in step S201, mixed evenly and then solidified. The solidified sample is carbonized at high temperature under an inert atmosphere, naturally cooled, washed and dried to obtain a micro-mesoporous phenolic resin.

[0025] Further, in the step S201, the mass ratio of phenol to formaldehyde is 1:3;

[0026] The mass of the sodium hydroxide is 5% of the total mass of phenol and formaldehyde.

[0027] Furthermore, the step S201 includes the following steps:

[0028] S201-1: Place phenol in a container and heat until the solid melts into liquid, then add sodium hydroxide for the first time and stir to react at a constant temperature of 50°C for 20 minutes;

[0029] S201-2: Add formaldehyde to the container for the first time, continue stirring and reacting at 60° C. for 50 minutes, then add sodium hydroxide for the second time, raise the temperature to 70° C., and maintain stirring and reacting at 70° C. for 20 minutes;

[0030] S201-3: Add formaldehyde to the container for the second time, continue stirring at 90° C. for 30 minutes, and finally obtain a translucent brown-red product that is completely soluble in water;

[0031] S201-4: dehydrating the product obtained in step S201-3 under reduced pressure to obtain a water-soluble phenolic resin adhesive having a solid content in the range of 70 to 80% as a precursor;

[0032] The mass ratio of the first added sodium hydroxide to the second added sodium hydroxide is 7:3;

[0033] The mass ratio of the first added formaldehyde to the second added formaldehyde is 19:5.

[0034] Furthermore, in step S202, the mass ratio of the precursor, ethylene glycol, and FeCl2 is 100:100:3.

[0035] Furthermore, the magnetic humic acid resin adsorbent can be regenerated after being saturated with heavy metal ions, and the regeneration method comprises the following steps:

[0036] Step 1: Soak the magnetic humic acid resin adsorbent that has been saturated with heavy metal ions in a 0.1 mol / L HCl solution for 30 to 60 minutes, and shake it every 5 minutes to ensure sufficient desorption;

[0037] Step 2: After desorption, rinse the resin with ultrapure water until the HCl solution is completely rinsed and then dry;

[0038] Step 3: Repeat steps 1 and 2 3 to 5 times.

[0039] On the other hand, the present invention provides a magnetic humic acid resin adsorbent, which can be prepared at least according to the above-mentioned preparation method, and the magnetic humic acid resin adsorbent comprises:

[0040] A carrier, wherein the carrier is a phenolic resin;

[0041] The load includes humic acid and Fe3O4.

[0042] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0043] (1) The preparation method of the present invention has an easy process and simple operation, can easily realize batch preparation, and is suitable for industrial production; the synthetic materials are simple and easy to obtain, the price is cheap, and the synthetic conditions are relatively mild;

[0044] (2) The present invention creatively combines phenolic resin, humic acid, etc. to prepare a new type of adsorbent, and the adsorbent has a simple production process, high adsorption, high selectivity and short adsorption equilibrium time, and can be regenerated multiple times and has high stability;

[0045] (3) The adsorbent of the present invention has a ternary system of humic acid-nano iron-phenolic resin with high interface assembly properties. The system has high adsorption capacity and high selectivity for lead ions in different solution environments, can quickly reach adsorption equilibrium, and is easy to separate and recover materials, which is suitable for large-scale sewage treatment applications.

[0046] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be achieved and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0048] Figure 1 is a SEM-EDS image of a phenolic resin in a specific embodiment;

[0049] Figure 2 is a SEM-EDS image of a magnetic humic acid resin adsorbent in a specific embodiment;

[0050] Figure 3 The specific embodiment of Example 2 is the Pd 2+ Adsorption curve diagram. DETAILED DESCRIPTION

[0051] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0052] In the description of the embodiments of the present invention, it should be noted that, unless otherwise clearly specified and limited, the term "connected" should be understood in a broad sense, for example, it can be a fixed connection, or a detachable connection, or an integral connection, which can be a mechanical connection, or an electrical connection, which can be a direct connection, or can be indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0053] The terms "top", "bottom", "above", "lower", and "on" used throughout the description are relative to the relative positions of components of a device, such as the relative positions of the top and bottom substrates within a device. It is understood that devices are multifunctional regardless of their orientation in space.

[0054] The common working surface of the present invention can be a plane or a curved surface, can be inclined, or can be horizontal. For the convenience of description, the embodiment of the present invention is placed on a horizontal plane and used on the horizontal plane, and "high and low" and "up and down" are defined in this way.

[0055] Embodiment 1

[0056] This embodiment discloses a method for preparing a magnetic humic acid resin adsorbent, comprising the following steps:

[0057] S100: preparing a ferrous-ferrous mixed solution;

[0058] S200: adding humic acid solution, ammonia water and phenolic resin to the ferrous-ferrous mixed solution obtained in step S100 in sequence, and reacting at 80-110° C. for 2.5-4 hours;

[0059] S300: adding a solution containing calcium ions to the liquid after the reaction in step S200, stirring and cooling to room temperature, collecting precipitates, washing the precipitates to neutrality, and drying to obtain a magnetic humic acid resin adsorbent.

[0060] The preparation method of the present invention combines phenolic resin, humic acid and the like to prepare a magnetic humic acid resin adsorbent, wherein the phenolic resin has thermal stability and acid resistance, and can improve the acid resistance of the adsorbent of the present invention; the humic acid, as a natural polymer compound, has a huge reserve and rich oxygen-containing functional groups, and can simultaneously form coordination bonds with various forms of heavy metals, and can improve the adsorption selectivity of the adsorbent of the present invention for heavy metals.

[0061] In step S100, the iron-ferrous mixed solution contains Fe 3+ , Fe 2+ A solution of Fe 3+ with Fe 2+ The molar ratio of Fe is 1:1 to 2:1, and Fe2+ The concentration range of is 0.12 to 0.19 mol / L. For example, the molar ratio is 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1. Preferably, the iron-ferrous mixed solution is prepared by dissolving FeCl3·6H2O and FeSO4·7H2O in water. For example, in the prepared iron-ferrous mixed solution, the concentration of FeCl3 is 0.178 mol / L, and the concentration of FeSO4 is 0.122 mol / L, that is, Fe 3+ with Fe 2+ The molar ratio is 1.46:1.

[0062] In step S200, in order to obtain uniform nanoparticles, a coprecipitation method is used, the principle of which is Fe 2+ +2Fe 3+ +8OH - →Fe3O4+4H2O, thus obtaining superparamagnetic ferroferric oxide particles. Humic acid, as a natural polymer compound, has abundant oxygen-containing functional groups and can simultaneously form coordination bonds with various forms of heavy metals. Humic acid (represented by HA) mainly wraps Fe3O4 nanoparticles through ligand exchange and hydrophobic interaction. The active sites on the HA-Fe3O4 surface are conducive to the adsorption of heavy metals.

[0063] The humic acid solution is prepared by dissolving humic acid in water, and the concentration of the humic acid solution is 0.01-0.015 g / mL. Exemplarily, the concentration of the humic acid solution is 0.01 g / mL, 0.011 g / mL, 0.012 g / mL, 0.013 g / mL, 0.014 g / mL, and 0.015 g / mL.

[0064] The ratio of the mass of the humic acid to the sum of the masses of FeCl3·6H2O and FeSO4·7H2O is 1:25 to 1:15, that is, m(humic acid):(m(FeCl3·6H2O)+m(FeSO4·7H2O))=1:25 to 1:15, preferably, m(humic acid):(m(FeCl3·6H2O)+m(FeSO4·7H2O))=1:20.5. It should be noted that m(humic acid) refers to the mass of humic acid used to prepare the humic acid solution, and m(FeCl3·6H2O) and m(FeSO4·7H2O) refer to the mass of FeCl3·6H2O and FeSO4·7H2O used to prepare the ferrous-ferrous mixed solution.

[0065] The humic acid can be purchased or directly extracted from lignite. Preferably, the content of fulvic acid in the humic acid is ≥ 90%. In this embodiment, the humic acid was purchased from Aladdin with a CAS number of 1415-93-6.

[0066] The mass fraction of the ammonia water is 25%, and the volume ratio of the ammonia water to the humic acid solution is 5:1.

[0067] The mass ratio of the phenolic resin to the humic acid is 1:1, that is, m (phenolic resin): m (humic acid) = 1:1.

[0068] Preferably, the reaction temperature of step S200 is controlled by an oil bath. This is because the constant temperature oil bath can fully and effectively heat the liquid sample to be heated, so as to achieve the purpose of mixing and sufficient reaction at a certain temperature. Preferably, the stirrer can be placed directly in the pot to directly stir the oil in the pot. Under the continuous stirring action of the oil, the temperature uniformity of each point in the pot is ensured, and the temperature control accuracy of the oil bath and the volatility of the oil temperature are improved.

[0069] Further preferably, the reaction is carried out at 90-95° C. for 3-3.5 h, that is, humic acid solution, ammonia water and phenolic resin are sequentially added to the ferrous-ferrous mixed solution, and the reaction is carried out at 90-95° C. in an oil bath for 3-3.5 h.

[0070] According to a preferred embodiment of the present invention, the phenolic resin is a micro-mesoporous phenolic resin, and the preparation method of the micro-mesoporous phenolic resin comprises the following steps:

[0071] S201: Preparation of carbon precursor;

[0072] Phenol, formaldehyde and sodium hydroxide are sequentially added into a container to undergo polycondensation reaction to obtain a translucent brown-red product that is completely soluble in water, and then dehydrated under reduced pressure to obtain a water-soluble phenolic resin adhesive with a solid content in the range of 70 to 80% as a precursor;

[0073] S202: Preparation of micro-mesoporous phenolic resin;

[0074] Ethylene glycol and FeCl2 are sequentially added to the precursor obtained in step S201, mixed evenly and then solidified. The solidified sample is carbonized at high temperature under an inert atmosphere, naturally cooled, washed and dried to obtain a micro-mesoporous phenolic resin.

[0075] In the step S201, the mass ratio of phenol to formaldehyde is 1:3. The sodium hydroxide is a catalyst, and its mass is 5% of the total mass of phenol and formaldehyde.

[0076] Preferably, sodium hydroxide is added in two portions, and the water-soluble phenolic resin adhesive is synthesized by a two-step alkali catalysis method. In this case, step S201 includes the following steps:

[0077] S201-1: Place phenol in a container and heat until the solid melts into liquid, then add sodium hydroxide for the first time and stir to react at a constant temperature of 50°C for 20 minutes;

[0078] S201-2: Add formaldehyde to the container for the first time, continue stirring and reacting at 60° C. for 50 minutes, then add sodium hydroxide for the second time, raise the temperature to 70° C., and maintain stirring and reacting at 70° C. for 20 minutes;

[0079] S201-3: Add formaldehyde to the container for the second time, continue stirring at 90° C. for 30 minutes, and finally obtain a translucent brown-red product that is completely soluble in water;

[0080] S201-4: Dehydrate the product obtained in step S201-3 under reduced pressure to obtain a water-soluble phenolic resin adhesive with a solid content in the range of 70 to 80% as a precursor.

[0081] Preferably, the mass ratio of the sodium hydroxide added before and after is 7:3, that is, the mass ratio of the sodium hydroxide added for the first time to the sodium hydroxide added for the second time is 7:3.

[0082] Preferably, the mass ratio of the formaldehyde added for the first time to the formaldehyde added for the second time is 19:5.

[0083] The vacuum degree of the reduced pressure dehydration is -0.085 to -0.095 MPa, and the dehydration temperature is 50°C.

[0084] In step S202, ethylene glycol is used as a solvent and a pore-forming agent, and FeCl2 is used as a catalyst. The mass ratio of the precursor, ethylene glycol, and FeCl2 is 100:100:3.

[0085] Preferably, the precursor, ethylene glycol, and FeCl2 react in a reactor, and the reactor is equipped with a magnetic stirrer, a temperature detector, and a condenser, so that the three (i.e., the precursor, ethylene glycol, and FeCl2) are stirred evenly at room temperature, and then maintained at 85-95°C for 5-6h (preferably, at 90°C for 6h). After the reaction is completed, the temperature is raised to 180-200°C and maintained for 8h (preferably, the temperature is raised to 190°C and maintained for 8h) to obtain a solidified sample.

[0086] The conditions for high-temperature carbonization are as follows: the inert atmosphere is a nitrogen atmosphere, the carbonization temperature is controlled at 800-1100° C. (preferably, 900° C.), the heating rate is controlled at 5° C. / min-10° C. / min, and the carbonization time is 0.5-1.0 h.

[0087] Preferably, deionized water is used for washing at room temperature for 1.5 to 2 hours to remove residual iron salts so as to obtain clean micro-mesoporous phenolic resin. Acid washing can also be used to increase the pore size of the phenolic resin.

[0088] Preferably, the drying is carried out in a blast oven at a drying temperature of 80 to 90° C. (preferably 80° C.) and a drying time of 6 to 8 hours.

[0089] The specific surface area of ​​the micro-mesoporous phenolic resin obtained by the above method is 50-600 m 2 / g, and the average pore size is distributed in the range of 1.59-4.25nm. The pore size of the obtained micro-mesoporous phenolic resin is distributed in the micro-mesoporous range, and the pores are rich and uniform, and the quality and performance stability are good.

[0090] The above-mentioned preparation method of micro-mesoporous phenolic resin can obtain a new type of phenolic resin carbon material with relatively uniform micro-mesoporous diameter and high specific surface area, and the synthetic materials required for the preparation method are simple and easy to obtain, cheap, the synthesis conditions are relatively mild, the operation is simple, and it is green and environmentally friendly.

[0091] In step S300, the solution containing calcium ions can be any solution containing Ca 2+ In this embodiment, the solution containing calcium ions is a calcium chloride solution, and the concentration of calcium chloride is 1 mol / L.

[0092] In order to load as much Ca ions as possible, an excess of calcium ion-containing solution is generally used in step S300. For example, the volume ratio of the calcium ion-containing solution to the ferrous-ferrous mixed solution is 1:10 to 1:5.

[0093] Calcium has greater selectivity and affinity for heavy metal lead. Adding calcium can enhance the adsorption effect of heavy metals, that is, increase the selectivity of the adsorbent for heavy metal lead.

[0094] The collection and precipitation method can be filtering, vacuum filtration, etc. Preferably, a permanent magnet is used to collect the precipitation. Since magnetic ferroferric oxide is generated in the precipitation, the permanent magnet can be used to collect the precipitation. On the one hand, more humic acid can be combined as active sites to adsorb heavy metals; on the other hand, paramagnetism can be used to achieve rapid and efficient separation of the adsorbent, achieving an effect of one plus one being greater than two.

[0095] The room temperature refers to 25°C±5°C.

[0096] The precipitate is washed with deionized water until the pH value is neutral, and dried at 90-120° C. Preferably, it is dried in a vacuum oven, and the drying temperature is preferably 100-105° C., and illustratively, the vacuum degree in the vacuum oven is -0.085 MPa. Preferably, the dried precipitate is ground to 100-200 mesh to obtain a magnetic humic acid resin adsorbent.

[0097] The magnetic humic acid resin adsorbent of the present invention can be regenerated after being saturated with adsorption, and the regeneration method comprises the following steps:

[0098] Step 1: Soak the magnetic humic acid resin adsorbent that has been saturated with heavy metal ions in a 0.1 mol / L HCl solution for 30 to 60 minutes, and shake it every 5 minutes to ensure sufficient desorption;

[0099] Step 2: After desorption, the resin is rinsed with ultrapure water until the HCl solution is completely rinsed (i.e., until the rinsed liquid is neutral, pH = 7), and then dried (drying temperature is 70-80°C);

[0100] Step 3: Repeat step 1 and step 2 3 to 5 times. Exemplarily, repeat step 1 and step 2 4 times.

[0101] In the step 1, hydrochloric acid is generally used for pickling, and the pickling rate of hydrochloric acid is relatively high. If dilute sulfuric acid is used for pickling, it will react with the previous calcium ions and destroy the adsorbent structure, which is not desirable.

[0102] [Example 1] A method for preparing a magnetic humic acid resin adsorbent comprises the following steps:

[0103] S100: dissolving 4.8 g of FeCl3·6H2O and 3.4 g of FeSO4·7H2O in 100 mL of water to prepare a ferrous-ferrous mixed solution;

[0104] S200: 40 mL of 0.01 g / mL humic acid solution, 8 mL of 25% ammonia water, and 0.4 g of phenolic resin are sequentially added to the iron-ferrous mixed solution obtained in step S100, and reacted in an oil bath at 90° C. for 3 h;

[0105] S300: Add 10 mL of 1 mol / L calcium chloride solution to the liquid after the reaction in step S200, stir for 30 min, cool to 25° C., collect the precipitate with a permanent magnet, rinse the precipitate to neutrality, dry it in a vacuum oven at 90° C., and then grind it to 100-200 mesh to obtain a magnetic humic acid resin adsorbent.

[0106] [Example 2] A method for preparing a magnetic humic acid resin adsorbent comprises the following steps:

[0107] S100: 6.1 g of FeCl3·6H2O and 4.3 g of FeSO4·7H2O were dissolved in 100 mL of water to prepare a ferrous-ferrous mixed solution;

[0108] S200: 50 mL of 0.01 g / mL humic acid solution, 10 mL of 25% ammonia water, and 0.5 g of phenolic resin are sequentially added to the ferrous-ferrous mixed solution obtained in step S100, and reacted in an oil bath at 92° C. for 3 h;

[0109] S300: Add 15 mL of 1 mol / L calcium chloride solution to the liquid after the reaction in step S200, stir for 30 min, cool to 25° C., collect the precipitate with a permanent magnet, rinse the precipitate to neutrality, dry it in a vacuum oven at 90° C., and then grind it to 100-200 mesh to obtain a magnetic humic acid resin adsorbent.

[0110] [Example 3] A method for preparing a magnetic humic acid resin adsorbent comprises the following steps:

[0111] S100: Dissolve 7.2 g of FeCl3·6H2O and 5.1 g of FeSO4·7H2O in 100 mL of water to prepare a ferrous-ferrous mixed solution;

[0112] S200: 60 mL of 0.01 g / mL humic acid solution, 12 mL of 25% ammonia water, and 0.6 g of phenolic resin are sequentially added to the ferrous-ferrous mixed solution obtained in step S100, and reacted in an oil bath at 94° C. for 3 h;

[0113] S300: Add 20 mL of 1 mol / L calcium chloride solution to the liquid after the reaction in step S200, stir for 30 min, cool to 25° C., collect the precipitate with a permanent magnet, rinse the precipitate to neutrality, dry it in a vacuum oven at 90° C., and then grind it to 100-200 mesh to obtain a magnetic humic acid resin adsorbent.

[0114] The magnetic humic acid resin adsorbent obtained in the above example has a good effect on Pb 2+ The relationship between the adsorption effect of the solution, the number of regeneration times and the adsorption amount is shown in Table 1-2.

[0115] Adsorption experiment: In order to study the adsorption effect of magnetic humic acid resin adsorbent on heavy metals, 50mL of prepared heavy metal solution was measured, pH=3 or pH=5, a certain mass of magnetic humic acid resin adsorbent was added, and it was oscillated in a constant temperature water bath oscillating box for 180min. When the adsorption reached saturation, the filtrate was filtered to determine the heavy metal ion concentration and calculate the removal rate.

[0116] Table 1 - Magnetic humic acid resin adsorbent for Pb 2+ The adsorption results

[0117]

[0118] It can be seen from Table 1 that when the pH value is 3, Pb 2+ The solution ion removal rate is over 84%; at a pH of 5, Pb 2+ The solution ion removal rate is more than 90%. The adsorption capacity of the magnetic humic acid resin adsorbent of the present invention for heavy metal lead under acidic solution conditions is evaluated using the Langmuir and Reundlich equations. Through the fitting under acidic solution and the calculation of isotherm parameters, it is found that the Langmuir equation can better describe the adsorption of lead ions by the magnetic humic acid resin. The maximum adsorption capacity of the magnetic humic acid resin adsorbent at pH = 3 and 5 is calculated to be 352.51 and 465.12 mg / g respectively.

[0119] From Table 1 and Figure 3 It can be seen that the magnetic humic acid resin adsorbent of the present invention has a good effect on Pb 2+ The adsorption equilibrium time is 20 to 30 minutes, and the adsorption kinetic equilibrium time is faster when the pH is low.

[0120] A regeneration experiment was conducted on Example 2. It can be seen from Table 2 that for solutions with pH = 3 and 5, as the number of cycles increases, the removal rates drop to 90% and 94% respectively, and the removal rate changes slightly, which shows that the magnetic humic acid resin adsorbent has good reproducibility and stability.

[0121] Table 2 - Relationship between regeneration times and removal rate

[0122]

[0123] Embodiment 2

[0124] This embodiment discloses a magnetic humic acid resin adsorbent, which can at least be prepared by the preparation method provided in the first embodiment.

[0125] The magnetic humic acid resin adsorbent comprises:

[0126] The carrier is a phenolic resin having a specific surface area of ​​50 to 600 m 2 / g, the average pore size distribution is 1.59~4.25nm;

[0127] The load includes humic acid and Fe3O4.

[0128] The structure of the magnetic humic acid resin adsorbent is a ternary composite structure of humic acid-nano iron-phenolic resin.

[0129] SEM-EDS was used to characterize the phenolic resin and magnetic humic acid resin adsorbents. Figure 1 It can be seen that the phenolic resin has a smooth surface and rich pore structure. Figure 2 It can be seen that the magnetic humic acid resin adsorbent retains the inherent morphology of phenolic resin and a relatively rich void structure. Compared with phenolic resin, the iron content in the magnetic humic acid resin adsorbent is increased, and the carbon and oxygen are evenly distributed, which shows that the structure of the magnetic humic acid resin adsorbent is a ternary composite structure of humic acid-nano iron-phenolic resin.

[0130] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a magnetic humic acid resin adsorbent, It is characterized in that The following steps are involved: S100: preparing a ferrous-ferrous mixed solution; S200: adding humic acid solution, ammonia water and phenolic resin to the ferrous-ferrous mixed solution obtained in step S100 in sequence, and reacting at 80-110° C. for 2.5-4 hours; S300: adding a solution containing calcium ions to the liquid after the reaction in step S200, stirring and cooling to room temperature, collecting precipitates, washing the precipitates to neutrality, and drying them to obtain a magnetic humic acid resin adsorbent; The phenolic resin is a micro-mesoporous phenolic resin, and the preparation method of the micro-mesoporous phenolic resin comprises the following steps: S201: Preparation of carbon precursor; Phenol, formaldehyde and sodium hydroxide are sequentially added into a container to undergo polycondensation reaction to obtain a translucent brown-red product that is completely soluble in water, and then dehydrated under reduced pressure to obtain a water-soluble phenolic resin adhesive with a solid content in the range of 70 to 80% as a precursor; S202: Preparation of micro-mesoporous phenolic resin; Ethylene glycol, FeCl 2 After being uniformly mixed, the mixture is solidified, and the solidified sample is carbonized at high temperature in an inert atmosphere, cooled naturally, washed, and dried to obtain a micro-mesoporous phenolic resin.

2. The preparation method according to claim 1, It is characterized in that In step S100: The iron-ferrous mixed solution contains Fe 3+ , Fe 2+ A solution of Fe 3+ with Fe 2+ The molar ratio is 1:1 to 2:1; The ferrous-ferrous mixed solution is composed of FeCl 3 6H 2 O, FeSO 4 7H 2 O is prepared by dissolving in water.

3. The preparation method according to claim 2, It is characterized in that In step S200: The concentration of the humic acid solution is 0.01 to 0.015 g / mL; The mass of humic acid and FeCl 3 6H 2 O, FeSO 4 7H 2 The sum ratio of the mass of O is 1:25 to 1:15; The mass fraction of the ammonia water is 25%, and the volume ratio of the ammonia water to the humic acid solution is 5:1; The mass ratio of the phenolic resin to humic acid is 1:

1.

4. The preparation method according to claim 3, It is characterized in that In the step S300: the concentration of calcium ions in the solution containing calcium ions is 1 mol / L; The precipitate is collected by a permanent magnet; The precipitate is washed with deionized water until the pH value is neutral, and dried at 90-120°C.

5. The preparation method according to claim 1, It is characterized in that In the step S201, the mass ratio of phenol to formaldehyde is 1:3; The mass of the sodium hydroxide is 5% of the total mass of phenol and formaldehyde.

6. The preparation method according to claim 5, It is characterized in that The step S201 comprises the following steps: S201-1: Place phenol in a container and heat until the solid melts into liquid, then add sodium hydroxide for the first time and stir to react at a constant temperature of 50°C for 20 minutes; S201-2: Add formaldehyde to the container for the first time, continue stirring and reacting at 60° C. for 50 minutes, then add sodium hydroxide for the second time, raise the temperature to 70° C., and maintain stirring and reacting at 70° C. for 20 minutes; S201-3: Add formaldehyde to the container for the second time, continue stirring at 90° C. for 30 minutes, and finally obtain a translucent brown-red product that is completely soluble in water; S201-4: dehydrating the product obtained in step S201-3 under reduced pressure to obtain a water-soluble phenolic resin adhesive having a solid content in the range of 70 to 80% as a precursor; The mass ratio of the first added sodium hydroxide to the second added sodium hydroxide is 7:3; The mass ratio of the first added formaldehyde to the second added formaldehyde is 19:

5.

7. The preparation method according to claim 1, It is characterized in that In the step S202, the mass ratio of the precursor, ethylene glycol, and FeCl2 is 100:100:

3.

8. A magnetic humic acid resin adsorbent, It is characterized in that At least it can be prepared by the preparation method according to any one of claims 1 to 7, and the magnetic humic acid resin adsorbent comprises: A carrier, wherein the carrier is a phenolic resin; The load includes humic acid, Fe 3 O 4 .

9. A method for regenerating the magnetic humic acid resin adsorbent as claimed in claim 8, It is characterized in that The regeneration method comprises the following steps: Step 1: Soak the magnetic humic acid resin adsorbent that has been saturated with heavy metal ions in a 0.1 mol / L HCl solution for 30 to 60 minutes, and shake it every 5 minutes to ensure sufficient desorption; Step 2: After desorption, rinse the resin with ultrapure water until the HCl solution is completely rinsed and then dry; Step 3: Repeat steps 1 and 2 3 to 5 times.

Citation Information

Patent Citations

  • Magnetic phenol formaldehyde-humic acid resin and preparation method thereof

    CN103611513A

  • Method for preparing magnetic adsorbent for methylene blue wastewater treatment

    CN106040185A

  • Magnetic activated carbon mixture containing carbon spheres and preparation method of mixture

    CN107774232A

  • Preparation method and application of polyethyleneimine modified magnetic bamboo powder material

    CN110898817A

  • Preparation method and application of artificial humic acid-functionalized colloid-like magnetic charcoal

    CN112827475A