A kind of diethanol monoisopropanolamine cement grinding aid and preparation method thereof
By using diethanol monoisopropanolamine and stable components in cement aids, the problems of early strength and late strength in cement are solved, and the effects of cost reduction and strength balance are achieved.
Patent Information
- Application Number
- CN202310439890.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-23
AI Technical Summary
While the existing abrasive agents increase the early strength of cement, they lead to the late strength of cement inverted, and the cost of alcohol amine materials is high, which affects economicality.
Use diethanol monoisopropanolamine cement aid, combined with stable components such as gel resin, sodium hexametaphosphate and nano-silica powder, and form stable components through the use of colloid molding agent and gelatin solution. Improve early strength of cement and reduce ettringite formation and reduce late fracture risk.
It effectively improves the early strength of cement, while reducing the adverse effects of late strength, reducing costs, and is simple and convenient to operate.
Smart Images

Figure BDA0004193538160000051 
Figure BDA0004193538160000061 
Figure BDA0004193538160000062
Abstract
Description
Technical Field
[0001] The present application relates to the field of cement admixtures, and more specifically, to a diethanol monoisopropanolamine cement grinding aid and a preparation method thereof. Background Art
[0002] Grinding aid is a cement admixture added to cement mill to aid grinding. It can significantly improve grinding efficiency and reduce unit cement energy consumption. At present, cement plants’ demand for grinding aid is not only to improve cement grinding efficiency, but also to pay more attention to the effect of grinding aid on cement strength enhancement.
[0003] In the current grinding aid ratio, amine materials such as triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, etc. are mainly used to improve the strength of cement. With the increasing requirements for early and late strength of cement, the dosage of amine materials has also been increasing, approaching the upper limit of the optimal use range of amine materials. At the same time, the cost of amine materials is relatively high, which directly leads to the high cost of grinding aids.
[0004] In order to reduce the cost of grinding aids, sodium thiocyanate is usually added to replace part of the amine materials to improve the early compressive strength of cement. However, as the amount of potassium thiocyanate added increases, the cement hydration in the later stage produces a large amount of calcium sulfoaluminate, which causes the cement volume to expand. When the cement is used for concrete mixing, the cracks in the hardened concrete increase, which leads to a reduction in the late compressive strength. Summary of the invention
[0005] In order to improve the reinforcing effect on the early strength of cement and reduce the adverse effects on the late strength of cement, the present application provides a diethanol monoisopropanolamine cement grinding aid and a preparation method thereof.
[0006] In the first aspect, the present application provides a diethanol monoisopropanolamine cement grinding aid, adopting the following technical scheme: a diethanol monoisopropanolamine cement grinding aid, which comprises the following raw materials in parts by weight: 60 to 80 parts of diethanol monoisopropanolamine, 10 to 20 parts of triethanolamine, 10 to 20 parts of sodium thiocyanate, and 15 to 30 parts of a stabilizing component, wherein the stabilizing component comprises a stabilizer, an absorbent and a densifier, and the weight ratio of the stabilizer, absorbent and densifier is 3 to 9:6 to 10:1.
[0007] By adopting the above technical scheme, the stabilizing component is prepared from the stabilizer, the absorbent and the densifier. After the three are mixed, the stabilizer and the absorbent play the role of the main structure, and the densifier is in the gap to play a reinforcing role. The stabilizer allows the stabilizing component to maintain good dispersion in the grinding aid. When the grinding aid is used, the stabilizing component is also evenly dispersed in the cement, and the absorbent is evenly distributed during the grinding process. Sodium thiocyanate improves the early strength of cement in the early stage of cement hydration. In the late stage of cement hydration, the absorbent adsorbs and binds excess sulfite ions, reduces the formation of calcium sulfonate, thereby reducing the possibility of cement being cracked by calcium sulfonate, and further reduces the adverse effects on the late strength of cement.
[0008] Preferably, the stabilizer is a gel-type resin.
[0009] By adopting the above technical solution, the gel-type resin is embedded in the main body to become a part of the main body structure, thereby improving the dispersibility of the stabilizing component and reducing the possibility of stratification between the stabilizing component and other components.
[0010] Preferably, the absorbent comprises sodium hexametaphosphate and a colloid forming agent, and the weight ratio of the sodium hexametaphosphate to the colloid forming agent is 5 to 9:1.
[0011] By adopting the above technical solution, during the absorbent molding process, the colloid molding agent provides water for the gelation of sodium hexametaphosphate on the one hand, and improves the gelation stability of sodium hexametaphosphate on the other hand, thereby making the combination of the stabilizer and sodium hexametaphosphate more stable.
[0012] Preferably, the colloid forming agent is a mixed solution of forming glue and water, and the mass fraction concentration of the mixed solution is 5%.
[0013] By adopting the above technical solution, the molding glue is first dissolved in water, thereby promoting the gelation of sodium hexametaphosphate and improving its gel stability.
[0014] Preferably, the molding glue is one of carrageenan, gelatin, β-cyclodextrin or konjac flour.
[0015] By adopting the above technical solution, water-soluble glue is used as the molding glue, so it is easy to combine with sodium hexametaphosphate, thereby effectively improving the stability of sodium hexametaphosphate.
[0016] Preferably, the densifying agent comprises nano-silicon dioxide powder and calcium carbonate powder, and the weight ratio of the nano-silicon dioxide powder to the calcium carbonate powder is 3:1.
[0017] By adopting the above technical solution, nano-silicon dioxide powder and calcium carbonate powder are used as compacting agents, which can fill the internal and structural gaps of the stabilizing components on the one hand, and effectively improve the strength of the cement in the later stage of cement hydration on the other hand, thereby reducing the possibility of cement cracking by calcium sulfoxide.
[0018] Preferably, the stabilizing component is prepared by the following steps: mixing the gel-type resin, sodium hexametaphosphate and a densifying agent uniformly, using a colloid forming agent as a binder, and preparing particles by disk granulation, the particle size D 90 =1.5 mm, thereby producing a stable component.
[0019] By adopting the above technical scheme, the gel-type resin, sodium hexametaphosphate and a densifier are used as powders and the colloid forming agent is used as a binder to obtain stable component particles, which is simple and convenient to operate.
[0020] In the second aspect, the present application provides a method for preparing a diethanol monoisopropanolamine cement grinding aid, using the following technical solution:
[0021] A method for preparing a diethanol monoisopropanolamine cement grinding aid comprises the following steps: diethanol monoisopropanolamine, triethanolamine, sodium thiocyanate and a stabilizing component are stirred and mixed evenly to obtain the cement grinding aid.
[0022] By adopting the above technical solution, the cement grinding aid can be prepared by mixing the temperature component with other components, and the operation is simple.
[0023] In summary, this application has the following beneficial effects:
[0024] 1. Since the present application adopts gel-type resin, sodium hexametaphosphate and a densifier to stir and mix evenly, and uses a colloid forming agent as a binder to prepare a stable component, on the one hand, the combination stability of the stable component and other components is improved, and on the other hand, the absorbent obtained after cement grinding absorbs and combines excess sulfite ions, thereby reducing the formation of calcium sulfonate.
[0025] 2. In the present application, nano-silicon dioxide powder and calcium carbonate powder are preferably used as compacting agents. In the later stage of cement hydration, the strength of cement is effectively improved, so that the possibility of cement cracking by ettringite is reduced.
[0026] 3. The method of the present application can prepare cement grinding aid by simple mixing, and the operation is simple. DETAILED DESCRIPTION
[0027] In this application, the concentration of diethanol monoisopropanolamine is 85%, industrial grade, purchased from the market; the concentration of triethanolamine is 85%, industrial grade, purchased from the market; the concentration of sodium thiocyanate liquid is 55%, industrial grade, purchased from the market; the gel-type resin is Dow cation exchange resin, gel acid type 001X7, particle size 0.4mm, purchased from the market; sodium hexametaphosphate is a white odorless crystalline powder purchased from the market; gelatin is purchased from the market, the particle size of nano-silicon dioxide powder is 30nm, purchased from the market; the particle size of calcium carbonate powder is 2500 mesh, purchased from the market.
[0028] The present application is further described in detail below in conjunction with embodiments.
[0029] Preparation Example
[0030] Preparation Example 1
[0031] This preparation example discloses a stabilizing component, which is prepared by the following steps:
[0032] 3kg of gel-type resin, 5kg of sodium hexametaphosphate, 0.75kg of nano-silicon dioxide powder and 0.25kg of calcium carbonate powder were taken and stirred and mixed evenly, and then 1kg of gelatin solution was used as a binder to obtain a granular stable component with a particle size of 1.5mm through disc granulation.
[0033] Preparation Example 2
[0034] This preparation example discloses a stabilizing component, which is prepared by the following steps:
[0035] 6 kg of gel-type resin, 7 kg of sodium hexametaphosphate, 0.75 kg of nano-silicon dioxide powder and 0.25 kg of calcium carbonate powder were taken and stirred and mixed evenly, and then 1 kg of gelatin solution was used as a binder to obtain a granular stable component with a particle size of 1.5 mm through disc granulation.
[0036] Preparation Example 3
[0037] This preparation example discloses a stabilizing component, which is prepared by the following steps:
[0038] 9 kg of gel-type resin, 9 kg of sodium hexametaphosphate, 0.75 kg of nano-silicon dioxide powder and 0.25 kg of calcium carbonate powder were taken and stirred and mixed evenly, and then 1 kg of gelatin solution was used as a binder to obtain a granular stable component with a particle size of 1.5 mm through disc granulation.
[0039] Preparation Example 4
[0040] This preparation example discloses a stabilizing component, which is prepared by the following steps:
[0041] 7 kg of sodium hexametaphosphate, 0.75 kg of nano-silicon dioxide powder and 0.25 kg of calcium carbonate powder were taken and stirred and mixed evenly, and then 1 kg of gelatin solution was used as a binder to obtain a granular stable component with a particle size of 1.5 mm through disc granulation.
[0042] Preparation Example 5
[0043] This preparation example discloses a stabilizing component, which is prepared by the following steps:
[0044] 6 kg of gel-type resin and 7 kg of sodium hexametaphosphate were taken and stirred and mixed evenly, and then 1 kg of gelatin solution was used as a binder, and a granular stable component with a particle size of 1.5 mm was obtained by disc granulation.
[0045] Example
[0046] Example 1
[0047] This embodiment discloses a cement grinding aid, which is prepared by the following steps:
[0048] 60 kg of diethanol monoisopropanolamine, 10 kg of triethanolamine, 10 kg of sodium thiocyanate and 15 kg of the stabilizing component prepared in Preparation Example 1 were stirred and mixed uniformly to prepare a cement grinding aid.
[0049] Example 2
[0050] This embodiment discloses a cement grinding aid, which is prepared by the following steps:
[0051] 70 kg of diethanol monoisopropanolamine, 15 kg of triethanolamine, 15 kg of sodium thiocyanate and 20 kg of the stabilizing component prepared in Preparation Example 2 were stirred and mixed uniformly to prepare a cement grinding aid.
[0052] Example 3
[0053] This embodiment discloses a cement grinding aid, which is prepared by the following steps:
[0054] 80 kg of diethanol monoisopropanolamine, 20 kg of triethanolamine, 20 kg of sodium thiocyanate and 30 kg of the stabilizing component prepared in Preparation Example 3 were stirred and mixed uniformly to prepare a cement grinding aid.
[0055] Example 4
[0056] This embodiment discloses a cement grinding aid, which is prepared by the following steps:
[0057] 70 kg of diethanol monoisopropanolamine, 15 kg of triethanolamine, 15 kg of sodium thiocyanate and 20 kg of the stabilizing component prepared in Preparation Example 1 were stirred and mixed uniformly to prepare a cement grinding aid.
[0058] Example 5
[0059] This embodiment discloses a cement grinding aid, which is prepared by the following steps:
[0060] 70 kg of diethanol monoisopropanolamine, 15 kg of triethanolamine, 15 kg of sodium thiocyanate and 20 kg of the stabilizing component prepared in Preparation Example 3 were stirred and mixed uniformly to prepare a cement grinding aid.
[0061] Comparative Example
[0062] Comparative Example 1
[0063] This comparative example discloses a cement grinding aid, which differs from Example 2 in that:
[0064] The stabilizing component is prepared in Preparation Example 4.
[0065] Comparative Example 2
[0066] This comparative example discloses a cement grinding aid, which differs from Example 2 in that:
[0067] The stabilizing component is prepared in Preparation Example 5.
[0068] Comparative Example 3
[0069] This comparative example discloses a cement grinding aid, which differs from Example 2 in that:
[0070] The stabilizing component was replaced by 14 kg of gel-type resin, 4.5 kg of nano-silicon dioxide powder and 1.5 kg of calcium carbonate powder.
[0071] Comparative Example 4
[0072] This comparative example discloses a cement grinding aid, which differs from Example 2 in that:
[0073] The stabilizing component was replaced by 20 kg of gel-type resin.
[0074] Comparative Example 5
[0075] This comparative example discloses a cement grinding aid, which differs from Example 2 in that:
[0076] The stabilizing component was replaced by 15 kg of nano-silicon dioxide powder and 5 kg of calcium carbonate powder.
[0077] Comparative Example 6
[0078] This comparative example discloses a cement grinding aid, which differs from Example 2 in that:
[0079] The stabilizing component was replaced with 17.5 kg of sodium hexametaphosphate and 2.5 kg of gelatin solution.
[0080] Comparative Example 7
[0081] This comparative example discloses a cement grinding aid, which differs from Example 2 in that:
[0082] No stabilizing ingredients added.
[0083] Table 1 Examples and Comparative Examples Raw Materials (kg)
[0084]
[0085]
[0086] Performance testing
[0087] The performance of the grinding aids obtained in the embodiments and comparative examples was tested, and the specific contents are as follows:
[0088] First, the components of cement are selected. The weight percentage (%) of the components of cement is clinker: mineral powder: slag: gypsum = 75:15:5:5. All components are crushed and passed through a 5 mm sieve.
[0089] Each time of grinding, the grinding time is 30 minutes, the grinding time is 5 minutes, the grinding temperature is 115°C, and the amount of grinding aid added is 0.04% of the weight of cement.
[0090] The fineness of the ground cement was tested, and the 80 μm sieve residue and 45 μm sieve residue of Example 2 and Comparative Example 7 were tested respectively. The specific test data are shown in Table 2.
[0091] The compressive strength of the cement in the embodiment or comparative example after grinding was tested, and the 3d and 28d compressive strengths were tested respectively with reference to GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)". The specific test data are shown in Table 2.
[0092] Table 2 Performance test data table
[0093]
[0094]
[0095] The grinding aid prepared in Example 2 was tested with reference to JC / T 667-2004 "Cement Grinding Aids". Specific test items and data are shown in Table 3.
[0096] Table 3 Cement grinding aid test data
[0097]
[0098] It can be seen from Example 2, Example 4 and Example 5 and Table 2 that the corresponding cement grinding aid is prepared by adjusting the amount of each component added, and after being mixed with cement and ground, the compressive strength of cement is effectively improved.
[0099] It can be seen from Example 2, Comparative Example 1, Comparative Example 4 and Comparative Example 7 and Table 2 and Table 3 that the gel-type resin is used as an intermediate connecting component between the reinforcing component and components such as diethanol monoisopropanolamine and triethanolamine, thereby improving the dispersion uniformity of the reinforcing component in the grinding aid, so that the reinforcing component is evenly dispersed in the cement with the use of the cement grinding aid, thereby effectively improving the reinforcement effect on the late strength of the cement.
[0100] It can be seen from Example 2, Comparative Example 2, Comparative Example 5 and Comparative Example 7 and Table 2 and Table 3 that the addition of nano-silicon dioxide powder and calcium carbonate powder improves the compactness and structural stability of the reinforcement component on the one hand, so that the reinforcement component can be evenly dispersed in the cement during the cement doping grinding aid process, and on the other hand, after uniform dispersion and crushing, it effectively enhances the strength and deformation resistance of cement soil and reduces the generation of cracks.
[0101] It can be seen from Example 2, Comparative Example 3, Comparative Example 6 and Comparative Example 7 and Table 2 and Table 3 that sodium hexametaphosphate can be used as a sulfite ion absorbent to absorb and bind excess sulfite ions, and at the same time, it is combined with gelatin solution, gel-type resin, nano-silicon dioxide powder and calcium carbonate powder to form a whole, so that the reinforcement component is evenly dispersed in the cement grinding aid, and then effectively evenly dispersed in the cement, thereby enhancing the late strength of the cement.
[0102] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A diethanol monoisopropanolamine cement grinding aid, It is characterized in that The method comprises the following raw materials in parts by weight: 60-80 parts of diethanol monoisopropanolamine, 10-20 parts of triethanolamine, 10-20 parts of sodium thiocyanate, and 15-30 parts of a stabilizing component, wherein the stabilizing component comprises a stabilizer, an absorbent and a densifier, and the weight ratio of the stabilizer, the absorbent and the densifier is 3-9:6-10:1; The stabilizer is a gel-type resin; The absorbent comprises sodium hexametaphosphate and a colloid forming agent, wherein the weight ratio of the sodium hexametaphosphate to the colloid forming agent is 5 to 9:1; the colloid forming agent is a mixed solution of forming glue and water, wherein the mass fraction concentration of the mixed solution is 5%, and the forming glue is one of carrageenan, gelatin, β-cyclodextrin or konjac flour; The densifying agent comprises nano silicon dioxide powder and calcium carbonate powder, and the weight ratio of the nano silicon dioxide powder to the calcium carbonate powder is 3:
1.
2. The preparation method of the diethanol monoisopropanolamine cement grinding aid according to claim 1, Features: The following steps are involved: The cement grinding aid can be prepared by stirring and mixing diethanol monoisopropanolamine, triethanolamine, sodium thiocyanate and a stabilizing component.
3. The preparation method of diethanol monoisopropanolamine cement grinding aid according to claim 2, Features: The stabilizing component is prepared by the following steps: the gel-type resin, sodium hexametaphosphate and a densifying agent are stirred and mixed evenly, a colloid forming agent is used as a binder, and particles are prepared by disc granulation, and the particle size D90 is 1.5 mm, thereby preparing the stabilizing component.