A kind of anti-aging flame-retardant polypropylene material and preparation method thereof
By using titanium dioxide/aluminum hydroxide composite particles and metal organic framework materials to optimize the anti-aging flame retardant composite particles, the problem of insufficient flame retardant performance of polypropylene materials is solved, and its flame retardant durability and mechanical properties are improved.
Patent Information
- Application Number
- CN202310437225.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-23
AI Technical Summary
The existing polypropylene materials ignore the modification of anti-aging properties during the flame retardant modification process, resulting in the breakage of their molecular chains and reducing the durability of their flame retardant properties.
Titanium dioxide/aluminum hydroxide composite particles are used as functional additives to coat titanium dioxide through aluminum hydroxide to form a core-shell structure, and combine metal organic framework materials to optimize the structure of anti-aging flame retardant composite particles to improve compatibility with polypropylene materials. and flame retardant properties.
It improves the flame retardant durability and mechanical properties of polypropylene materials, enhances the antioxidant effect, and extends the stability of flame retardant performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to polypropylene materials, and more specifically, to an anti-aging flame-retardant polypropylene material and a preparation method thereof. Background Art
[0002] Polypropylene is one of the most widely used general-purpose plastics. It can be used in a wide temperature range and has the characteristics of light density, excellent processing performance, stable physical and chemical properties, and low price. In addition, its molecular chain is composed entirely of carbon and hydrogen elements, which is easy to recycle and conforms to the environmental protection concept of "carbon neutrality". Although polypropylene has excellent performance, its shortcomings such as poor impact resistance at low temperatures, poor weather resistance, and easy combustion have greatly limited its application range. Therefore, PP needs to be chemically and physically modified to improve its flame retardancy and weather resistance.
[0003] At present, the flame retardant modification of polypropylene mainly includes two methods: physical blending flame retardants and coating surface treatment. Among them, physical blending flame retardants are widely used in the flame retardant modification of polypropylene plastics due to their easy processing and low cost, and coating surface treatment is mostly used for the flame retardant modification of polypropylene non-woven fabrics and polypropylene foams.
[0004] In view of the above-mentioned related technologies, the inventors believe that the existing polypropylene materials often only process their flame retardant properties during the flame retardant modification process, while ignoring the effect of anti-aging performance modification on the flame retardant properties. Since the aging of polypropylene plastic will cause the main chain of its molecular chain to break, it is more easily ignited, thereby reducing the durability of its flame retardant properties. Summary of the invention
[0005] In order to overcome the defects of poor flame retardancy and durability of existing polypropylene materials, the present application provides an anti-aging flame retardant polypropylene material and a preparation method thereof, which adopts the following technical scheme:
[0006] In the first aspect, the present application provides an anti-aging flame-retardant polypropylene material, which adopts the following technical solution:
[0007] An anti-aging flame-retardant polypropylene material comprises the following substances in parts by weight:
[0008] Copolymer polypropylene 65-80 parts;
[0009] Homopolymer polypropylene 20-30 parts;
[0010] 1 to 3 parts of lubricant;
[0011] Functional additives 2.5-3.0 parts;
[0012] The functional additive comprises anti-aging flame-retardant composite particles, and the anti-aging flame-retardant composite particles comprise titanium dioxide / aluminum hydroxide composite particles.
[0013] By adopting the above technical scheme, the technical scheme of the present application optimizes the components of the anti-aging flame-retardant polypropylene material, and replaces the flame retardant and anti-aging agent in the traditional functional additives with the composite particles prepared by the present application. Since the present application coats the aluminum hydroxide particles on the surface of titanium dioxide, on the one hand, the aluminum hydroxide can be effectively dispersed into the interior of the polypropylene material to form a good dispersion effect, and give it good flame retardant properties inside the polypropylene material; on the other hand, the titanium dioxide / aluminum hydroxide composite particles with a composite structure have good anti-aging properties. Since the aluminum hydroxide coats the titanium dioxide, the lattice defects of the titanium dioxide are compensated, the photochemical active points thereof are shielded, and the quality of the titanium dioxide is improved, thereby further improving the flame retardant and durable properties of the polypropylene material.
[0014] Furthermore, the anti-aging flame-retardant composite particles are also provided with a porous supporting matrix, and at least a part of the titanium dioxide / aluminum hydroxide composite particles are arranged on the surface of the supporting matrix so that the anti-aging flame-retardant composite particles form a core-shell structure.
[0015] By adopting the above technical scheme, the technical scheme of the present application further optimizes the structure of the anti-aging and flame-retardant composite particles, and further improves the compatibility of the anti-aging and flame-retardant composite particles with the polypropylene material by selecting a load matrix and titanium dioxide / aluminum hydroxide composite particles to form a core-shell structure, so that the prepared polypropylene material has good structural strength and mechanical properties, thereby further improving the antioxidant effect and flame retardant durability of the polypropylene material.
[0016] Furthermore, the supporting matrix of the porous structure is an aluminum-based metal organic framework material.
[0017] Furthermore, the aluminum-based metal organic framework material is made by the following scheme:
[0018] Aluminum nitrate and DMF were mixed and stirred, and 2-methylimidazole was added, and the mixture was stirred and mixed, and the mixture was placed in a hydrothermal reactor for heat preservation and reaction;
[0019] The heat-insulated reaction product is collected and mixed with N,N-dimethylformamide, centrifuged and dried to obtain an intermediate product;
[0020] The intermediate product is placed in a muffle furnace, heated, kept warm for calcination, and then naturally cooled to room temperature to prepare the aluminum-based metal organic framework material.
[0021] By adopting the above technical solution, the loading matrix material of the porous structure is adjusted to address the defect of poor compatibility between traditional inorganic porous materials and organic materials, and a metal organic framework material is selected. Since the organic ligands in the aluminum-based metal organic framework material interact more strongly with the polymer molecular chain and have better affinity with the polymer chain, the antioxidant and flame retardant prepared in the present application can form a more stable dispersed structure in the polypropylene material, thereby improving the durability of the polypropylene material.
[0022] On this basis, the metal organic framework material used in the technical solution of the present application can adsorb carbon residue to form a dense structural layer on the surface of its pore structure during the combustion of polypropylene material, thereby graphitizing the carbon residue and promoting the conversion of amorphous carbon into a graphite structure, thereby enhancing the strength of the carbon layer, making the carbon layer denser and more stable, playing a better barrier role during the combustion process, reducing heat transfer, and thus improving the flame retardancy of the composite material.
[0023] Furthermore, the anti-aging flame-retardant composite particles are also provided with a bonding layer between the bonding layer, the supporting matrix of the porous structure and the titanium dioxide / aluminum hydroxide composite particles.
[0024] By adopting the above technical scheme, the technical scheme of the present application optimizes the structure of the anti-aging flame-retardant composite particles and improves the bonding performance between the titanium dioxide / aluminum hydroxide composite particles and the porous structured loading matrix through the design of the bonding layer, thereby further improving the flame retardant stability of the polypropylene material.
[0025] Furthermore, the anti-aging flame-retardant composite particles are prepared by the following scheme:
[0026] After mixing sodium aluminate with sulfuric acid, collect the aluminum-based mixed solution;
[0027] After the aluminum-based mixed liquid and the titanium sol are stirred and mixed, they are placed in a spray drying device;
[0028] After the surface of the porous support matrix is impregnated with nickel hydroxide sol, the surface is coated with spray-dried particles, and after natural drying, it is placed in a vacuum freeze-drying device and dried to prepare the anti-aging flame-retardant composite particles.
[0029] By adopting the above technical scheme, the technical scheme of the present application optimizes the preparation method of anti-aging flame-retardant composite particles. Different from the traditional coating method, the present application adopts a spray drying coating method to improve the uniformity and stability of the coating; secondly, the present application uses nickel hydroxide sol to perform surface treatment on the porous structure load matrix. Since the dried nickel hydroxide forms an effective aerogel coating layer on the surface of the load matrix, it serves as a flame retardant synergistic material for titanium dioxide / aluminum hydroxide composite particles, further improving the flame retardancy and durability of the polypropylene material.
[0030] In a second aspect, the present application provides a method for preparing an anti-aging flame-retardant polypropylene material, comprising the following preparation steps:
[0031] Premixing treatment: homopolymer polypropylene, lubricant and functional additives are stirred and mixed, and the premix is collected;
[0032] Pre-modification treatment: After the premix is mixed with the cross-linking agent, it is melt-extruded for micro-cross-linking treatment, and the micro-cross-linked material is collected;
[0033] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material can be prepared.
[0034] By adopting the above technical solution, the technical solution of the present application further optimizes the technical solution of flame retardant modification of polypropylene materials, and through the technical solution of double mixing, improves the modification efficiency and reduces the modification cost.
[0035] Further, the cross-linking agent includes at least one of DVB or PETA.
[0036] By adopting the above technical scheme, the technical scheme of the present application optimizes the components in the flame retardant modification of polypropylene materials, and by adding materials that can undergo micro-cross-linking during the modification process of polypropylene materials, the melt strength of the polypropylene material is further improved, so that it has good mechanical properties and flame retardant modification properties.
[0037] In summary, the present application includes at least one of the following beneficial technical effects:
[0038] First, the technical solution of the present application optimizes the components of the anti-aging flame-retardant polypropylene material, and replaces the flame retardant and anti-aging agent in the traditional functional additives with the composite particles prepared by the present application. Since the present application coats the aluminum hydroxide particles on the surface of titanium dioxide, on the one hand, the aluminum hydroxide can be effectively dispersed into the interior of the polypropylene material to form a good dispersion effect, and give it good flame retardant properties inside the polypropylene material; on the other hand, the titanium dioxide / aluminum hydroxide composite particles with a composite structure have good anti-aging properties. Since the aluminum hydroxide coats the titanium dioxide, the lattice defects of the titanium dioxide are compensated, its photochemical active points are shielded, and the quality of the titanium dioxide is improved, thereby further improving the flame retardant and durable properties of the polypropylene material.
[0039] Second, the technical solution of the present application further optimizes the structure of the anti-aging and flame-retardant composite particles. By selecting a load matrix and titanium dioxide / aluminum hydroxide composite particles to form a core-shell structure, the compatibility of the anti-aging and flame-retardant composite particles with polypropylene materials is further improved, so that the prepared polypropylene material has good structural strength and mechanical properties, thereby further improving the antioxidant effect and flame retardant durability of the polypropylene material.
[0040] Third, in view of the defect of poor compatibility between traditional inorganic porous materials and organic materials, the present application adjusts the load matrix material of the porous structure and selects metal organic framework materials. Since the organic ligands in the aluminum-based metal organic framework materials interact more strongly with the polymer molecular chains and have better affinity with the polymer chains, the antioxidants and flame retardants prepared in the present application can form a more stable dispersed structure in the polypropylene material, thereby improving the durability of the polypropylene material.
[0041] On this basis, the metal organic framework material used in the technical solution of the present application can adsorb carbon residue to form a dense structural layer on the surface of its pore structure during the combustion of polypropylene material, thereby graphitizing the carbon residue and promoting the conversion of amorphous carbon into a graphite structure, thereby enhancing the strength of the carbon layer, making the carbon layer denser and more stable, playing a better barrier role during the combustion process, reducing heat transfer, and thus improving the flame retardancy of the composite material. DETAILED DESCRIPTION
[0042] The present application is further described in detail below with reference to the embodiments.
[0043] Preparation Example 1
[0044] Take 10g of sodium aluminate and 2kg of 10% sulfuric acid, stir and mix them, adjust the pH to 6.0 with 1% sodium hydroxide solution, stir and mix with 15% solid content titanium dioxide sol, and spray dry to prepare the titanium dioxide / aluminum hydroxide composite particles 1.
[0045] Preparation Example 2
[0046] Take 12g of sodium aluminate and 2.5kg of 10% sulfuric acid, stir and mix them, adjust the pH to 6.0 with 1% sodium hydroxide solution, stir and mix with 16.5% solid content titanium dioxide sol, and spray dry to prepare the titanium dioxide / aluminum hydroxide composite particles 2.
[0047] Preparation Example 3
[0048] Take 15g of sodium aluminate and 3kg of 10% sulfuric acid, stir and mix them, adjust the pH to 6.0 with 1% sodium hydroxide solution, stir and mix with 18% solid content titanium dioxide sol, and spray dry to prepare the titanium dioxide / aluminum hydroxide composite particles 3.
[0049] Preparation Example 4
[0050] Take 0.7 g of aluminum nitrate and 50 g of DMF, stir and mix, then add 0.17 g of 2-methylimidazole, continue to stir and mix, place in a hydrothermal reactor, and keep the reaction at 140° C. for 24 hours;
[0051] The heat-insulated reaction product was collected and mixed with N,N-dimethylformamide, centrifuged and dried at 60° C. to prepare an intermediate product;
[0052] The intermediate product is placed in a muffle furnace, heated to 580° C. at a rate of 2° C. / min, calcined at this temperature, and then naturally cooled to room temperature, thereby preparing the aluminum-based metal organic framework material 1.
[0053] Preparation Example 5
[0054] Take 0.75g aluminum nitrate and 65g DMF and stir and mix, then add 0.19g 2-methylimidazole, continue to stir and mix, place in a hydrothermal reactor, and keep the temperature at 145°C for 24h;
[0055] The heat-insulated reaction product was collected and mixed with N,N-dimethylformamide, centrifuged and dried at 65°C to obtain an intermediate product;
[0056] The intermediate product is placed in a muffle furnace, heated to 600° C. at a rate of 2° C. / min, and naturally cooled to room temperature after calcination to obtain the aluminum-based metal organic framework material 2.
[0057] Preparation Example 6
[0058] Take 0.8 g of aluminum nitrate and 80 g of DMF, stir and mix, then add 0.20 g of 2-methylimidazole, continue to stir and mix, place in a hydrothermal reactor, and keep the temperature at 150° C. for 24 hours;
[0059] The heat-insulated reaction product was collected and mixed with N,N-dimethylformamide, centrifuged and dried at 70° C. to obtain an intermediate product;
[0060] The intermediate product is placed in a muffle furnace, heated to 620° C. at a rate of 2° C. / min, calcined at this temperature, and then naturally cooled to room temperature, thereby preparing the aluminum-based metal organic framework material 3.
[0061] Preparation Example 7
[0062] Take 10g of sodium aluminate and 2kg of 10% sulfuric acid, stir and mix, adjust the pH to 6.0 with 1% sodium hydroxide solution, stir and mix with 15% solid content titanium dioxide sol, and collect the coating liquid;
[0063] The surface of the aluminum-based metal organic framework material 1 is coated with a spray-dried coating liquid, and after natural drying, it is placed in a vacuum freeze-drying device and dried to prepare the anti-aging flame-retardant composite particles 1.
[0064] Preparation Example 8
[0065] Take 10g of sodium aluminate and 2kg of 10% sulfuric acid, stir and mix, adjust the pH to 6.0 with 1% sodium hydroxide solution, stir and mix with 15% solid content titanium dioxide sol, and collect the coating liquid;
[0066] The surface of the aluminum-based metal organic framework material 2 is coated with a spray-dried coating liquid, and after natural drying, it is placed in a vacuum freeze-drying device and dried to prepare the anti-aging flame-retardant composite particles 2.
[0067] Preparation Example 9
[0068] Take 10g of sodium aluminate and 2kg of 10% sulfuric acid, stir and mix, adjust the pH to 6.0 with 1% sodium hydroxide solution, stir and mix with 15% solid content titanium dioxide sol, and collect the coating liquid;
[0069] The surface of the aluminum-based metal organic framework material 3 is coated with a spray-dried coating liquid, and after natural drying, it is placed in a vacuum freeze-drying device and dried to prepare the anti-aging flame-retardant composite particles 3.
[0070] Preparation Example 10
[0071] Take 10g of sodium aluminate and 2kg of 10% sulfuric acid, stir and mix, adjust the pH to 6.0 with 1% sodium hydroxide solution, stir and mix with 15% solid content titanium dioxide sol, and collect the coating liquid;
[0072] The surface of the aluminum-based metal organic framework material 2 is impregnated with nickel hydroxide sol with a solid content of 5%, and after vacuum freeze drying, the surface is coated with a spray drying coating liquid, and after natural drying, it is placed in a vacuum freeze drying device and dried to prepare the anti-aging flame retardant composite particles 4. Example 1
[0073] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolypropylene, 1kg lubricant EBS and 2.5kg titanium dioxide / aluminum hydroxide composite particles 1.
[0074] Premixing treatment: homopolymerized polypropylene, lubricant and titanium dioxide / aluminum hydroxide composite particles 1 are stirred and mixed, and the premix is collected;
[0075] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0076] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 1 can be prepared. Example 2
[0077] An anti-aging flame-retardant polypropylene material comprises: 72kg copolymer polypropylene, 25kg homopolypropylene, 2kg lubricant EBS and 2.7kg titanium dioxide / aluminum hydroxide composite particles 1.
[0078] Premixing treatment: homopolymerized polypropylene, lubricant and titanium dioxide / aluminum hydroxide composite particles 1 are stirred and mixed, and the premix is collected;
[0079] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0080] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 2 can be prepared. Example 3
[0081] An anti-aging flame-retardant polypropylene material comprises: 80kg copolymer polypropylene, 30kg homopolypropylene, 3kg lubricant EBS and 3.0kg titanium dioxide / aluminum hydroxide composite particles 1.
[0082] Premixing treatment: homopolymerized polypropylene, lubricant and titanium dioxide / aluminum hydroxide composite particles 1 are stirred and mixed, and the premix is collected;
[0083] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0084] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 3 can be prepared. Example 4
[0085] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolypropylene, 1kg lubricant EBS and 2.5kg titanium dioxide / aluminum hydroxide composite particles 2.
[0086] Premixing treatment: homopolymerized polypropylene, lubricant and titanium dioxide / aluminum hydroxide composite particles 2 are stirred and mixed, and the premix is collected;
[0087] Pre-modification treatment: After mixing the premix with the cross-linking agent DVB, set the temperature of sections 1 to 5 of the single-screw extruder barrel to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-cross-linking treatment, and collect the micro-cross-linked material; mixed co-extrusion: After mixing the copolymerized polypropylene and the micro-cross-linked material, melt extrude them to prepare the anti-aging flame-retardant polypropylene material 4. Example 5
[0088] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolypropylene, 1kg lubricant EBS and 2.5kg titanium dioxide / aluminum hydroxide composite particles 3.
[0089] Premixing treatment: homopolymerized polypropylene, lubricant and titanium dioxide / aluminum hydroxide composite particles 3 are stirred and mixed, and the premix is collected;
[0090] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0091] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 5 can be prepared. Example 6
[0092] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolypropylene, 1kg lubricant EBS and 2.5kg anti-aging flame-retardant composite particles 1.
[0093] Premixing treatment: homopolymer polypropylene, lubricant and anti-aging flame retardant composite particles 1 are stirred and mixed, and the premix is collected;
[0094] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0095] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 6 can be prepared. Example 7
[0096] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolypropylene, 1kg lubricant EBS and 2.5kg anti-aging flame-retardant composite particles 2.
[0097] Premixing treatment: homopolymer polypropylene, lubricant and anti-aging flame retardant composite particles 2 are stirred and mixed, and the premix is collected;
[0098] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0099] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 7 can be prepared. Example 8
[0100] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolymer polypropylene, 1kg lubricant EBS and 2.5kg anti-aging flame-retardant composite particles 3.
[0101] Premixing treatment: homopolymer polypropylene, lubricant and anti-aging flame retardant composite particles 3 are stirred and mixed, and the premix is collected;
[0102] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0103] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 8 can be prepared. Example 9
[0104] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolymer polypropylene, 1kg lubricant EBS and 2.5kg anti-aging flame-retardant composite particles 4.
[0105] Premixing treatment: homopolymer polypropylene, lubricant and anti-aging flame retardant composite particles 4 are stirred and mixed, and the premix is collected;
[0106] Pre-modification treatment: after mixing the premix with the crosslinking agent DVB, set the temperatures of the single screw extruder barrel sections 1 to 5 to 160°C, 180°C, 190°C, 190°C and 180°C, control the extruder screw speed to 50r / min, melt extrude and perform micro-crosslinking treatment, and collect the micro-crosslinked material;
[0107] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 9 can be prepared. Example 10
[0108] An anti-aging flame-retardant polypropylene material comprises: 65kg copolymer polypropylene, 20kg homopolymer polypropylene, 1kg lubricant EBS and 2.5kg anti-aging flame-retardant composite particles 4.
[0109] Premixing treatment: homopolymer polypropylene, lubricant and anti-aging flame retardant composite particles 4 are stirred and mixed, and the premix is collected;
[0110] Pre-modification treatment: after the premix is mixed with the cross-linking agent PETA, the mass of PETA is controlled to be 20% of the mass of the premix, the temperatures of the 1st to 5th sections of the single-screw extruder barrel are set to 160°C, 180°C, 190°C, 190°C and 180°C, the screw speed of the extruder is controlled to be 50r / min, and the melt extrusion is micro-cross-linked to collect the micro-cross-linked material;
[0111] Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material 10 can be prepared.
[0112] Comparative Example 1
[0113] Compared with Example 1, the functional additive in this comparative example uses a mixture of 2.0 kg of aluminum hydroxide and 0.5 kg of titanium dioxide to replace the anti-aging flame-retardant composite particles 1 used in Example 1.
[0114] Comparative Example 2
[0115] Compared with Example 1, in this comparative example 2, no anti-aging flame-retardant composite particles 1 or other flame retardants and antioxidants are added.
[0116] Performance Testing
[0117] The polypropylene prepared in Examples 1 to 10 and Comparative Examples 1 to 2 was injection molded into standard brick specimens, which were subjected to light aging treatment and then tested for flame retardancy.
[0118] Light aging flame retardant performance test: place the standard sample in Atlas Ci4000 xenon lamp aging box, the black mark temperature is (100±3)°C, the temperature of the aging box sample room is (65±3)°C, the humidity is 20%±10%, and the irradiation intensity (420nm) is 1.2W / m 2 After aging for 72 hours, the initial flame retardant performance and the flame retardant performance after aging were tested. The specific test results are shown in the following table:
[0119] Table 1 Performance test
[0120]
[0121] Combining the technical solutions and performance test tables of Examples 1 to 5 and Comparative Examples 1 to 2, it can be seen that the flame retardant properties of the polypropylene material prepared by optimizing the components of the anti-aging flame-retardant composite particles in this embodiment did not show a significant decrease in the flame retardant properties during the flame retardant properties test after aging, indicating that the technical solution of the present application can effectively disperse the composite particles prepared in the present application into the interior of the polypropylene material by replacing the flame retardant and anti-aging agent in the traditional functional additives with the composite particles prepared in the present application, thereby forming a good dispersion effect, giving the polypropylene material good flame retardant properties, and improving the flame retardant and durable properties of the polypropylene material.
[0122] Further comparison is made with the data of Examples 6 to 8 and Examples 1 to 5. Since the flame retardant properties of Examples 6 to 8 are significantly improved by optimizing the anti-aging flame retardant composite particles, and at the same time, on this basis, the anti-aging effect is improved, and the flame retardant properties are partially reduced after aging, indicating that the technical solution of the present application selects a load matrix and titanium dioxide / aluminum hydroxide composite particles to form a core-shell structure, which further improves the compatibility of the anti-aging flame retardant composite particles with the polypropylene material, so that the prepared polypropylene material has good structural strength and mechanical properties, thereby further improving the antioxidant effect and flame retardant durability of the polypropylene material.
[0123] Finally, by comparing Examples 9 to 10 with Examples 6 to 8, their flame retardant properties are significantly improved after aging, indicating that the technical solution of the present application further improves the flame retardant stability of the polypropylene material by optimizing the structure of the anti-aging flame retardant composite particles and improving the bonding performance between the titanium dioxide / aluminum hydroxide composite particles and the porous structure of the load matrix through the design of the bonding layer.
[0124] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An anti-aging flame-retardant polypropylene material, characterized in that: include: Copolymer polypropylene 65-80 parts; Homopolymer polypropylene 20-30 parts; 1 to 3 parts of lubricant; Functional additives 2.5-3.0 parts; The functional additive comprises anti-aging flame-retardant composite particles, and the anti-aging flame-retardant composite particles comprise titanium dioxide / aluminum hydroxide composite particles; The anti-aging flame-retardant composite particles are also provided with a porous structured loading matrix, and at least a portion of the titanium dioxide / aluminum hydroxide composite particles are arranged on the surface of the loading matrix so that the anti-aging flame-retardant composite particles form a core-shell structure; the loading matrix of the porous structure is an aluminum-based metal organic framework material; the aluminum-based metal organic framework material is made by the following scheme: Aluminum nitrate and DMF were mixed and stirred, and 2-methylimidazole was added, and the mixture was stirred and mixed, and the mixture was placed in a hydrothermal reactor for heat preservation and reaction; The heat-insulated reaction product is collected and mixed with N,N-dimethylformamide, centrifuged and dried to obtain an intermediate product; The intermediate product is placed in a muffle furnace, heated, kept warm for calcination, and then naturally cooled to room temperature to prepare the aluminum-based metal organic framework material; The anti-aging flame-retardant composite particles are also provided with a bonding layer, between the bonding layer and the porous structure support matrix and the titanium dioxide / aluminum hydroxide composite particles; The anti-aging flame-retardant composite particles are prepared by the following scheme: After mixing sodium aluminate with sulfuric acid, collect the aluminum-based mixed solution; After the aluminum-based mixed liquid and the titanium sol are stirred and mixed, they are placed in a spray drying device; After the surface of the porous support matrix is impregnated with nickel hydroxide sol, the surface is coated with spray-dried particles, and after natural drying, it is placed in a vacuum freeze-drying device and dried to prepare the anti-aging flame-retardant composite particles.
2. The method for preparing the anti-aging flame-retardant polypropylene material according to claim 1, characterized in that: The method comprises the following preparation steps: Premixing treatment: homopolymer polypropylene, lubricant and functional additives are stirred and mixed, and the premix is collected; Pre-modification treatment: After the premix is mixed with the cross-linking agent, it is melt-extruded for micro-cross-linking treatment, and the micro-cross-linked material is collected; Mixed co-extrusion: After the copolymerized polypropylene and the slightly cross-linked material are mixed and melt-extruded, the anti-aging flame-retardant polypropylene material can be prepared.
3. The method for preparing an anti-aging flame-retardant polypropylene material according to claim 2, characterized in that: The cross-linking agent includes at least one of DVB or PETA.