A back silver paste for N-type crystalline silicon solar cell and a preparation method thereof
By adding covalent functional graphene to the back silver paste, the problems of insufficient dispersion, poor adhesion ability and high resistivity in the prior art are solved, and higher photoelectric conversion efficiency and better weather resistance are achieved sex.
Patent Information
- Application Number
- CN202310567384.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-19
AI Technical Summary
The back silver paste in the prior art lacks dispersion, poor adhesion ability, difficulty in reducing resistivity and poor weather resistance, which cannot meet the needs of efficient photoelectric conversion and stable performance.
Covalent functional graphene is prepared by reacting graphene oxide with bis(4-aminophenoxy)dimethylsilane to enhance graphene by strengthening graphene graphene. The dispersion and adhesion ability of enes form conductive channels other than Ag-Si, reducing battery resistance.
It effectively reduces the battery's resistance, improves the photoelectric conversion efficiency, enhances the adhesion ability and weather resistance of silver paste, and meets the requirements of high performance and stability.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to a back silver paste for an N-type crystalline silicon solar cell and a preparation method thereof. Background Art
[0002] Solar energy is the source of the earth's energy. It is widely distributed and easy to obtain. It is an inexhaustible clean energy. In the context of the increasing depletion of non-renewable energy sources such as coal and oil, the development of solar energy is imminent. Solar cells came into being and became the most direct and effective means of developing and utilizing solar energy. Among them, silicon-based solar energy has become the most mature and widely commercialized solar cell solution.
[0003] According to the doping type of the substrate, silicon-based solar cells are divided into P-type crystalline silicon solar cells and N-type crystalline silicon solar cells. Compared with P-type crystalline silicon solar cells, N-type crystalline silicon solar cells have higher conversion efficiency and impurity tolerance, and basically no light-induced degradation. Since N-type crystalline silicon has a longer minority carrier lifetime than P-type crystalline silicon, N-type crystalline silicon cells can usually be made into double-sided PERC cells to increase the output power of the cell, and the increase is generally more than 20%.
[0004] Bifacial PERC solar cells are a special type of silicon-based solar cells. Their main feature is that one or more layers of passivation film structures are additionally plated on the front and back of the solar cell on the basis of silver paste. The back electrode formed after the back silver paste printed on the back of the cell is sintered plays the role of collecting current. The conductive silver paste used on the back of the solar cell is usually composed of three parts: silver powder, glass powder, and organic carrier. The silver powder mainly plays a conductive role; the organic carrier mainly plays a role in dispersing the silver powder, and some of its components also have the function of improving the printing performance of the silver paste; the glass powder mainly etches the reflective film on the surface of the silicon wafer and promotes the silver powder to form an ohmic contact with the silicon wafer. Therefore, the composition and properties of the conductive silver paste directly affect the performance of the solar cell, such as the photoelectric conversion efficiency. The key to obtaining high-performance and stable conductive silver paste lies in the preparation of silver powder and glass powder and the mixing of the two in the organic carrier.
[0005] However, as the demand for solar cells continues to grow, the back silver paste in the existing technology is gradually unable to meet the performance requirements of solar cells such as photoelectric conversion efficiency due to its insufficient dispersibility, poor adhesion, difficulty in reducing resistivity and poor weather resistance.
[0006] Therefore, there is an urgent need for a silver paste for the back side of N-type crystalline silicon solar cells that has good dispersibility and strong adhesion, can reduce battery resistance, improve photoelectric conversion efficiency, and improve grid line weather resistance after being printed on the electrode surface. Summary of the invention
[0007] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide a back silver paste for N-type crystalline silicon solar cells and a preparation method thereof, which has good dispersibility and strong adhesion, can reduce battery resistance, improve photoelectric conversion efficiency, and improve grid line weather resistance after being printed on the electrode surface.
[0008] Technical solution:
[0009] A back silver paste for an N-type crystalline silicon solar cell, comprising silver powder, an organic carrier, glass powder and covalently functionalized graphene;
[0010] The covalently functionalized graphene is prepared by reacting graphene oxide with bis(4-aminophenoxy)dimethylsilane.
[0011] The addition of covalently functionalized graphene in the present invention can effectively reduce the resistance of the battery, thereby improving the photoelectric conversion efficiency of the battery. When the silver paste is printed on the electrode surface, the covalently functionalized graphene can be deposited in the glass layer to form a conductive channel other than Ag-Si, so that more electrons on the surface of the N-type silicon are effectively separated through the conductive channel; the covalently functionalized graphene can make the electrons in the N-type silicon migrate to the silver grid surface at a very fast speed, which is conducive to reducing the recombination of electrons and holes; the sheet structure of the covalently functionalized graphene can well fill the gaps between the silver powder particles, improve the adhesion of the silver paste, and make the grid line surface formed by the paste after printing and sintering relatively smooth and dense.
[0012] Furthermore, the silver powder is selected from one or more of spherical silver powder, flaky silver powder and dendritic silver powder.
[0013] Furthermore, the organic carrier comprises a high molecular polymer, a dispersant and an organic solvent.
[0014] Furthermore, the mass ratio of the high molecular weight polymer, the dispersant and the organic solvent is (5-10): (3-5): (80-90);
[0015] The high molecular polymer is selected from one of ethyl cellulose, cellulose acetate propionate, cellulose acetate butyrate, polyvinyl formal, polyvinyl butyral, epoxy resin, phenolic epoxy resin or acrylic resin;
[0016] The dispersant is selected from one of sorbitan ester, alkylphenol polyoxyethylene ether or fatty amine polyoxyethylene ether;
[0017] The organic solvent is selected from one of butyl carbitol, butyl carbitol acetate, terpineol, dimethyl adipate, dimethyl glutarate, benzyl benzoate, ethylene glycol phenyl ether or propylene glycol phenyl ether.
[0018] Furthermore, the glass powder comprises, by weight: 1-10 parts of Bi2O3, 5-20 parts of TeO2, 1-3 parts of SiO2, 1-5 parts of B2O3, 1-5 parts of ZnO and 1-3 parts of Al2O3; the particle size of the glass powder is: 0.2 μm≤D 50 ≤3.0μm; the softening temperature of the glass powder is 200-500℃.
[0019] Furthermore, the preparation of the covalently functionalized graphene comprises the following steps:
[0020] (1) ultrasonically dispersing graphene oxide in N,N-dimethylformamide to obtain a graphene dispersion;
[0021] (2) adding graphene dispersion and bis(4-aminophenoxy)dimethylsilane into a reactor, adding hydrazine hydrate after ultrasonic treatment for 0.5-1 hour, stirring evenly and transferring to a reactor;
[0022] (3) The reaction vessel is heated to 100-110° C. and reacted for 2-3 hours, followed by suction filtration, washing, and drying to obtain the covalently functionalized graphene.
[0023] Furthermore, the mass ratio of the graphene oxide to bis(4-aminophenoxy)dimethylsilane is 1:3-5.
[0024] The invention generates covalently functionalized graphene by reacting oxygen-containing functional groups on the surface of graphene oxide with amino groups of bis(4-aminophenoxy)dimethylsilane, thereby replacing oxygen-containing functional groups on the surface of graphene oxide, thereby enhancing the interaction between graphene sheets, and expanding the steric hindrance between graphene sheets through benzene rings, thereby enhancing the dispersibility of graphene. On the one hand, the problem of easy aggregation of graphene is alleviated, and on the other hand, the graphene can be evenly dispersed in silver paste to reduce battery resistance.
[0025] The covalently functionalized graphene added to the silver paste of the present invention contains silicon-oxygen bonds and silicon methyl groups, which can improve the weather resistance of the gate lines.
[0026] Furthermore, the weight proportions of the components are 80-95 parts of silver powder, 5-15 parts of organic carrier, 1-5 parts of glass powder and 0.1-1 parts of covalently functionalized graphene.
[0027] Furthermore, the average fineness of the conductive silver paste is ≤10 μm.
[0028] Any one of the above methods for preparing a back silver paste for an N-type crystalline silicon solar cell comprises the following steps:
[0029] (1) weighing silver powder, organic carrier, glass powder and covalently functionalized graphene in proportion, adding them into a double planetary mixer, and stirring at a speed of 100-150 rpm for 30-50 minutes to prepare a slurry;
[0030] (2) The slurry is placed in a three-roll grinder, and ground for 10-15 times at a grinding speed of 300-500 rpm and a pressure of 0.8-1 MPa, so that the average fineness of the slurry is ≤10 μm to obtain the back silver paste for N-type crystalline silicon solar cells.
[0031] Beneficial effects:
[0032] (1) Adding covalently functionalized graphene to the silver paste on the back of the N-type crystalline silicon solar cell provided by the present invention can effectively reduce the resistance of the battery, thereby improving the photoelectric conversion efficiency of the battery. When the silver paste is printed on the electrode surface, the covalently functionalized graphene can be deposited in the glass layer to form a conductive channel other than Ag-Si, so that more electrons on the surface of the N-type silicon are effectively separated through the conductive channel; the covalently functionalized graphene can make the electrons in the N-type silicon migrate to the silver grid surface at a very fast speed, which is conducive to reducing the recombination of electrons and holes; the sheet structure of the covalently functionalized graphene can well fill the gaps between the silver powder particles, improve the adhesion of the silver paste, and make the grid line surface formed by the paste after printing and sintering relatively smooth and dense.
[0033] (2) Covalently functionalized graphene is added to the silver paste on the back side of an N-type crystalline silicon solar cell provided by the present invention. The oxygen-containing functional groups on the surface of graphene oxide react with the amino groups of bis(4-aminophenoxy)dimethylsilane to generate covalently functionalized graphene, which replaces the oxygen-containing functional groups on the surface of graphene oxide, thereby enhancing the interaction between graphene sheets and expanding the steric hindrance between graphene sheets through benzene rings, thereby enhancing the dispersibility of graphene. On the one hand, the problem of easy aggregation of graphene is alleviated, and on the other hand, the graphene can be evenly dispersed in the silver paste to reduce the battery resistance.
[0034] (3) The covalently functionalized graphene added to the silver paste on the back side of the N-type crystalline silicon solar cell provided by the present invention contains silicon-oxygen bonds and silicon methyl groups, which can improve the weather resistance of the grid lines. DETAILED DESCRIPTION
[0035] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0036] Graphene oxide was 796034 purchased from Merck; commercially available silver paste was RS8900 back silver paste purchased from Hangzhou Zhengyin Electronic Materials Co., Ltd.; and the remaining reagents and equipment were conventional reagents and equipment in the technical field.
[0037] Preparation of covalently functionalized graphene-1
[0038] Covalently functionalized graphene-1 was prepared by the following steps:
[0039] (1) ultrasonically dispersing 100 mg of graphene oxide in 100 mL of N,N-dimethylformamide to prepare a graphene dispersion;
[0040] (2) Add 100 mL of graphene dispersion and 400 mg of bis(4-aminophenoxy)dimethylsilane into the reactor, add 1 mL of hydrazine hydrate after 150 W ultrasonic treatment for 1 hour, stir evenly and transfer to the reactor;
[0041] (3) The reaction kettle was heated to 110° C. and reacted for 2 hours, then filtered, washed, and dried to obtain the covalently functionalized graphene-1.
[0042] Preparation of covalently functionalized graphene-2
[0043] The preparation is basically the same as that of covalently functionalized graphene-1, except that bis(4-aminophenoxy)dimethylsilane is replaced by an equal amount of 3,3'-diaminobenzidine.
[0044] Preparation of covalently functionalized graphene-3
[0045] The preparation is basically the same as that of covalently functionalized graphene-1, except that bis(4-aminophenoxy)dimethylsilane is replaced by an equal amount of dodecyl primary amine.
[0046] Organic carrier preparation
[0047] The organic carrier was prepared by the following steps:
[0048] By weight, 10 parts of ethyl cellulose, 5 parts of sorbitan ester and 90 parts of sorbitan ester were weighed and mixed, and then dispersed on a dispersant for 1 hour to prepare the organic carrier.
[0049] Glass powder preparation
[0050] The glass powder was prepared by the following steps:
[0051] According to the weight percentage, 5 parts of Bi2O3, 10 parts of TeO2, 2 parts of SiO2, 3 parts of B2O3, 3 parts of ZnO and 2 parts of Al2O3 were weighed, mixed evenly and placed in a high-temperature muffle furnace for heating, the temperature was controlled at 1000℃, and the temperature was kept for 1 hour. The melted glass powder particles were quenched with ionized water and ball milled for 5 hours to obtain a particle size of 0.2μm≤D 50 Glass powder ≤3.0μm.
[0052] Example 1
[0053] The back silver paste for N-type crystalline silicon solar cells was prepared by the following steps:
[0054] (1) 80 parts by weight of spherical silver powder, 10 parts by weight of organic carrier, 3 parts by weight of glass powder and 0.5 parts by weight of covalently functionalized graphene-1 were added into a double planetary mixer and stirred at a speed of 120 rpm for 40 minutes to prepare a slurry;
[0055] (2) The slurry was placed in a three-roll mill and ground for 15 passes at a grinding speed of 300 rpm and a pressure of 0.8 MPa to obtain the back silver paste for N-type crystalline silicon solar cells after the average fineness of the slurry was ≤10 μm.
[0056] Example 2
[0057] The method is basically the same as Example 1, except that the raw materials are changed to 85 parts of flaky silver powder, 5 parts of organic carrier, 1 part of glass powder and 0.5 parts of covalently functionalized graphene-1.
[0058] Example 3
[0059] The method is basically the same as Example 1, except that the raw materials are changed to 90 parts of dendritic silver powder, 15 parts of organic carrier, 5 parts of glass powder and 0.5 parts of covalently functionalized graphene-1.
[0060] Comparative Example 1
[0061] Commercially available silver paste.
[0062] Comparative Example 2
[0063] The method is basically the same as Example 1, except that the covalently functionalized graphene-1 is not added.
[0064] Comparative Example 3
[0065] The method is basically the same as Example 1, except that the covalently functionalized graphene-1 is replaced by an equal amount of graphene oxide.
[0066] Comparative Example 4
[0067] The method is basically the same as Example 1, except that the covalently functionalized graphene-1 is replaced by an equal amount of covalently functionalized graphene-2.
[0068] Comparative Example 5
[0069] The method is basically the same as Example 1, except that the covalently functionalized graphene-1 is replaced by an equal amount of covalently functionalized graphene-3.
[0070] Performance Testing
[0071] Resistance and photoelectric conversion efficiency detection: The back silver pastes prepared in Examples 1-3 and Comparative Examples 1-5 were printed on the front surface of the N-type PERC cell for testing, and the IV curve was detected using a TMC-PV1A solar cell tester to test the cell grid line resistance and photoelectric conversion efficiency.
[0072] Gate line resistance (Ω) Photoelectric conversion efficiency (%) Example 1 0.413 25.4 Example 2 0.411 25.5 Example 3 0.413 25.5 Comparative Example 1 0.651 23.3 Comparative Example 2 0.617 23.5 Comparative Example 3 0.531 24.3 Comparative Example 4 0.445 24.6 Comparative Example 5 0.493 24.5
[0073] According to the comparison of the test results of Examples 1-3 with Comparative Examples 1 and 2, it can be seen that the back silver paste for N-type crystalline silicon solar cells provided by the present invention has better dispersibility than the back silver paste in the prior art and can effectively reduce the grid line resistance, thereby making the battery have a higher photoelectric conversion efficiency.
[0074] According to the comparison of the test results of Examples 1-3 and Comparative Examples 3-5, it can be seen that the addition of covalently functionalized graphene prepared by the reaction of graphene oxide and bis(4-aminophenoxy)dimethylsilane to the back silver paste for N-type crystalline silicon solar cells provided by the present invention can effectively improve the dispersibility of the silver paste, reduce the battery resistance, and improve the photoelectric conversion efficiency; and the benzene rings, silicon-oxygen bonds, and silicon-methyl structures in its structure improve the dispersibility of graphene, thereby reducing the battery resistance and improving the battery photoelectric conversion efficiency.
[0075] Reliability test: The reliability of solar cells is verified through the double 85 test. Specifically, the cell with the back electrode welded is placed in a humid test chamber at 85°C and 85% humidity for 1000 hours to test the attenuation of its photoelectric conversion efficiency.
[0076] attenuation(%) Example 1 0.7 Example 2 0.6 Example 3 0.7 Comparative Example 1 4.6 Comparative Example 2 3.9 Comparative Example 3 2.7 Comparative Example 4 1.9 Comparative Example 5 2.2
[0077] According to the comparison of the test results of Examples 1-3 with Comparative Examples 1 and 2, it can be seen that the silver paste for the back side of an N-type crystalline silicon solar cell provided by the present invention has stronger weather resistance than the silver paste in the prior art.
[0078] According to the comparison of the test results of Examples 1-3 and Comparative Examples 3-5, it can be seen that the covalently functionalized graphene added to the silver paste on the back side of the N-type crystalline silicon solar cell provided by the present invention can improve the adhesion ability of the silver paste, and the silicon-oxygen bonds and silicon-methyl structures in its structure can significantly improve the weather resistance of the silver paste.
[0079] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A silver paste for the back side of an N-type crystalline silicon solar cell, characterized in that: It contains silver powder, organic carrier, glass powder and covalently functionalized graphene; The covalently functionalized graphene is prepared by reacting graphene oxide with bis(4-aminophenoxy)dimethylsilane; The silver powder is selected from one or more of spherical silver powder, flaky silver powder and dendritic silver powder; The organic carrier comprises a high molecular polymer, a dispersant and an organic solvent; The preparation of the covalently functionalized graphene comprises the following steps: (1) ultrasonically dispersing graphene oxide in N,N-dimethylformamide to obtain a graphene dispersion; (2) Adding graphene dispersion and bis(4-aminophenoxy)dimethylsilane into a reactor, adding hydrazine hydrate after ultrasonic treatment for 0.5-1 hour, stirring evenly and transferring to a reactor; (3) The reaction vessel is heated to 100-110° C., reacted for 2-3 hours, and then filtered, washed, and dried to obtain the covalently functionalized graphene.
2. The back silver paste for N-type crystalline silicon solar cells according to claim 1, characterized in that: The mass ratio of the high molecular polymer, dispersant and organic solvent is (5-10): (3-5): (80-90); The high molecular polymer is selected from one of ethyl cellulose, cellulose acetate propionate, cellulose acetate butyrate, polyvinyl formal, polyvinyl butyral, epoxy resin, phenolic epoxy resin or acrylic resin; The dispersant is selected from one of sorbitan ester, alkylphenol polyoxyethylene ether or fatty amine polyoxyethylene ether; The organic solvent is selected from one of butyl carbitol, butyl carbitol acetate, terpineol, dimethyl adipate, dimethyl glutarate, benzyl benzoate, ethylene glycol phenyl ether or propylene glycol phenyl ether.
3. The back silver paste for N-type crystalline silicon solar cells according to claim 1, characterized in that: In terms of weight, the glass powder comprises: 1-10 parts of Bi2O3, 5-20 parts of TeO2, 1-3 parts of SiO2, 1-5 parts of B2O3, 1-5 parts of ZnO and 1-3 parts of Al2O3.
4. The back silver paste for N-type crystalline silicon solar cells according to claim 1, characterized in that: The mass ratio of the graphene oxide to bis(4-aminophenoxy)dimethylsilane is 1:3-5.
5. The back silver paste for N-type crystalline silicon solar cells according to claim 1, characterized in that: The weight proportions of the components are 80-95 parts of silver powder, 5-15 parts of organic carrier, 1-5 parts of glass powder and 0.1-1 parts of covalently functionalized graphene.
6. The back silver paste for N-type crystalline silicon solar cells according to claim 1, characterized in that: The average fineness of the silver paste is ≤10 μm.
7. The method for preparing the back silver paste for N-type crystalline silicon solar cells according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Weighing silver powder, organic carrier, glass powder and covalently functionalized graphene in proportion, adding them into a double planetary mixer, and stirring at a speed of 100-150 rpm for 30-50 minutes to prepare a slurry; (2) The slurry is placed in a three-roll grinder and ground for 10-15 times at a grinding speed of 300-500 rpm and a pressure of 0.8-1 MPa to obtain the back silver paste for N-type crystalline silicon solar cells after the average fineness of the slurry is ≤10 μm.
Citation Information
Patent Citations
Graphene-based organic carrier and preparation method thereof as well as electronic paste and preparation method thereof