A AgSbSe2-based nanomaterial and its preparation method and application
Sn-doped AgSbSe2 nanocrystals prepared by colloid synthesis and surface chemical treatment methods solve the problem of Sn2+ easy oxidation, significantly improve the thermoelectric performance, and achieve efficient thermoelectric material preparation.
Patent Information
- Application Number
- CN202310515505.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-05-09
AI Technical Summary
Sn2+ ions are easily oxidized into high-valent state Sn4+ in AgSbSe2-based materials, resulting in a decrease in conductivity and limiting the improvement of thermoelectric performance.
Sn-doped AgSbSe2 nanocrystals were prepared by colloid synthesis method and two-step surface chemical treatment method. Sn4+ was reduced to Sn2+ through NaBH4 solution, and low-temperature annealing was performed in a nitrogen-hydrogen mixed atmosphere to ensure the stability of Sn2+.
It effectively inhibits the oxidation of Sn2+, improves the thermoelectric performance of AgSbSe2-based materials, improves the thermoelectric superiority zT, and has a simple process, low cost and high yield.
Smart Images

Figure CN116514070B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nano material preparation, and in particular to an AgSbSe2-based nano thermoelectric material and a preparation method and application thereof. Background Art
[0002] Thermoelectric conversion technology can realize the direct conversion between heat and electricity. It has broad application prospects in the fields of IoT self-powered power supply, deep space exploration and solid-state refrigeration, and is an important green clean energy technology. IV-VI2 ternary chalcogenide semiconductors have attracted more and more attention due to their excellent functional properties. AgSbTe2 has low intrinsic thermal conductivity (0.6-0.7Wm -1 K -1 ) and high Seebeck coefficient (300μVK -1 AgSbTe2 is widely studied as a promising low-medium temperature thermoelectric material. However, when the temperature is lower than 633K, AgSbTe2 will slowly decompose into secondary phases, and the scarcity of Te has hindered the practical application of AgSbTe2-based materials. Therefore, many researchers have turned their research targets to AgSbSe2-based materials that do not contain Te and are more stable.
[0003] AgSbSe2 crystals have a cubic rock salt structure similar to NaCl. Although Ag and Sb are thought to randomly occupy Na sites, careful characterization shows ordered domains of the two elements. This ordered structure and the possible existence of mixed phases and densely disordered defects have a significant impact on the electronic band structure near the band gap. AgSbSe2 is an indirect narrow bandgap semiconductor (0.03–0.10 eV) and is intrinsically p-type. Its valence band structure includes multiple flat valleys, resulting in high effective mass and high Seebeck coefficient. In addition, due to the 5s 2 The presence of lone pairs of electrons exhibits strong anharmonicity, which strengthens the phonon-phonon interaction and leads to extremely low lattice thermal conductivity. However, the carrier concentration of AgSbSe2 at room temperature is low (10 16 –10 18 cm -3 ), low electrical conductivity limits the improvement of its thermoelectric figure of merit zT. Therefore, its thermoelectric performance can be optimized by increasing the carrier concentration.
[0004] Usually, alivalent doping of AgSbSe2 is an effective strategy to increase the carrier concentration. 3+ Ions, such as Pb 2+ 、Cd 2+ 、Zn 2+ , Ca 2+ Mg 2+ , Ba 2+ , Mn 2+、Na + and Ag + A large amount of research work has proved the effectiveness of this method. Through simulation calculation of crystals, it is found that Sn 2+ The conductivity of AgSbSe2 can be improved without excessively affecting its Seebeck coefficient, thereby improving the overall thermoelectric performance. 2+ Ions are extremely unstable and their doping usually results in AgSb 1-x Sn x There are high-valence Sn in the Se2 lattice 4+ , resulting in a sharp drop in electrical conductivity, hindering the improvement of the thermoelectric figure of merit zT. Therefore, how to effectively stabilize Sn 2+ , that is, to inhibit its oxidation to high-valent Sn 4+ , thereby increasing Sn 2+ The thermoelectric performance of doped AgSbSe2 materials has become a key issue that needs to be solved urgently. Summary of the invention
[0005] The purpose of the present invention is to provide a AgSbSe2-based nano thermoelectric material and a preparation method and application thereof, which can inhibit Sn 2+ Ion oxidation, the prepared AgSbSe2-based materials have higher thermoelectric properties.
[0006] In one aspect of the present invention, the present invention provides a method for preparing AgSbSe2-based nanomaterials. According to an embodiment of the present invention, the preparation method comprises the following steps:
[0007] Step 1: Synthesis of AgSbSe2-based nanocrystals by colloidal synthesis
[0008] The powders of AgNO3, SbCl3, SnCl2 and Se are reacted in the atomic ratio of Ag:Sb:Sn:Se=1:(1-x):x:2, where 0<x≤0.03, and then added to a three-necked flask containing a mixed solution of oleylamine and oleic acid, stirred at room temperature under nitrogen protection, and then vacuumed at 80-100°C for 30min-60min, then heated to 110-120°C and nitrogen was introduced, and the temperature was quickly raised to 200-240°C for reaction. At this time, the Se source precursor was injected into the reaction solution, and the reaction was kept warm for at least 30min after the temperature returned to 220°C. After the reaction, the reaction solution was cooled to room temperature in a water bath, centrifuged and washed, and Sn-doped AgSbSe2-based (AgSb 1-x Sn x Se2) nanocrystals;
[0009] Step 2: Preparation of AgSbSe2-based nanomaterials using a two-step surface chemical treatment method
[0010] Sn-doped AgSbSe2-based nanocrystals were dispersed in chloroform, then mixed with NaBH4 solution for phase exchange treatment, shaken and centrifuged, and then chloroform and NaBH4 solution were added again and stirred at room temperature; the product was washed to remove excess NaBH4 and vacuum dried; in order to ensure that Sn 4+ In order to completely reduce and prevent possible surface oxidation during sample processing before hot pressing and sintering, the dried AgSbSe2-based nanomaterial powder treated with NaBH4 solution was placed in a tubular furnace for annealing. A nitrogen-hydrogen mixed reducing gas was introduced into the tubular furnace to obtain Sn-doped AgSbSe2-based nanothermoelectric material powder with surface chemical treatment.
[0011] The NaBH4 solution will Sn 4+ Restore to Sn 2+ The reaction mechanism is:
[0012] 4Sn 4+ +BH4 - +3H2O→4Sn 2+ +10H + +BO3 3-
[0013] Standard electrode potential (E θ )for:
[0014] Therefore, the redox potential (ΔE θ )for:
[0015] The Gibbs free energy of the reaction (Δ r G θ )Change: Δ r G θ =–zFΔE θ ≈–984 kJ mol -1 <0, where z is the number of electrons transferred in the chemical reaction, and F is the Faraday constant (96485 J·V -1 ·mol -1 ), the reaction will proceed largely spontaneously according to thermodynamics.
[0016] In addition, the method for preparing a AgSbSe2-based nanomaterial according to the above embodiment of the present invention may also have the following additional technical features:
[0017] In some embodiments of the present invention, in step 1, washing is performed three times using chloroform and anhydrous ethanol.
[0018] In some embodiments of the present invention, in step 1, the volume ratio of oleylamine to oleic acid is ≥5:1.
[0019] In some embodiments of the present invention, in step 1, the preparation method of the Se source precursor is as follows: weigh Se powder and transfer it to a mixed solution of oleylamine and n-dodecyl mercaptan, and stir it continuously under nitrogen protection at room temperature until the selenium powder is completely dissolved to obtain a selenium source precursor, wherein the concentration of the Se source precursor is 0.5 mol·L -1 , the volume ratio of oleylamine and n-dodecyl mercaptan is 1:1.
[0020] In some embodiments of the present invention, in step 1, the single-phase AgSbSe2-based nanocrystals have a cubic rock salt structure of NaCl.
[0021] In some embodiments of the present invention, in step 2, the NaBH4 solution is prepared by dissolving NaBH4 in an ethanol aqueous solution, wherein the ethanol aqueous solution is a mixed solution of 95% ethanol by volume and 5% deionized water by volume, and the concentration of the NaBH4 ethanol aqueous solution is 20.0 mmol·L -1 .
[0022] In some embodiments of the present invention, in step 2, the annealing treatment is as follows: keep the temperature at 250°C for 10 to 12 hours, and the heating rate is 5 to 10°C min -1 The nitrogen-hydrogen mixed gas consists of 95% N2 by volume and 5% H2 by volume.
[0023] In another aspect of the present invention, the present invention provides a Sn-doped AgSbSe2-based nanomaterial prepared according to the preparation method of the AgSbSe2-based nanomaterial.
[0024] The AgSbSe2 nanocrystals prepared in the present invention have a size of about 17±2 nanometers and can be dispersed in chloroform to form a stable dark brown dispersion system. By replacing SbCl3 with SnCl2 at a certain doping ratio in the cationic precursor solution, the Sn element is introduced into the product. The size distribution and morphology of the prepared nanocrystals doped with Sn do not change significantly.
[0025] The Sn-doped AgSbSe2-based nanocrystals prepared by the present invention have good thermoelectric properties. When x=0.02, the highest thermoelectric figure of merit zT reaches 1.37 at 666K, and can be used as a potential thermoelectric material with certain application value.
[0026] In another aspect of the present invention, a thermoelectric material is provided. According to an embodiment of the present invention, the thermoelectric material is obtained by hot pressing and sintering the AgSbSe2-based nanomaterial to densify it.
[0027] In addition, a thermoelectric material according to the above embodiment of the present invention may also have the following additional technical features:
[0028] In some embodiments of the present invention, the hot pressing sintering densification is carried out at a pressure of 60 to 70 MPa and a temperature of 360 to 380° C. for 20 to 30 minutes.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1) The present invention adopts an efficient material surface chemical treatment strategy, which can effectively inhibit the Sn on the surface of Sn-doped AgSbSe2-based nanocrystals. 2+ The oxidation and reduction of the high-valent Sn on the surface of the nanocrystals 4+ , increasing Sn 2+ The doping efficiency is greatly optimized, the thermoelectric performance is simple to operate and the repeatability is good.
[0031] 2) The present invention uses a scalable hot injection synthesis method to synthesize Sn-doped AgSb in large quantities through a one-step one-pot reaction. 1- x Sn x Se2 nanocrystals. Secondly, the present invention realizes the removal of organic ligands on the surface of nanocrystals and the removal of high-valent Sn 4+ Reduction, and further stabilization of Sn by low temperature annealing in a reducing atmosphere 2+ .
[0032] 3) The present invention significantly optimizes the thermoelectric properties of the material through the coordinated regulation of surface chemistry and energy band engineering. The high-performance Sn-doped AgSbSe2 nanomaterial finally obtained has the potential to be used as a thermoelectric material and has certain value.
[0033] 4) The present invention adopts a lower reaction temperature (low energy consumption), lower raw material cost (no need for ultra-high purity raw materials), and a simple and easy preparation method. AgSbSe2-based high-quality nanomaterials with a yield of more than 95% can be prepared in a short time. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a transmission electron microscope image (TEM) of the pure phase AgSbSe2 nanocrystal synthesized in Comparative Example 1 of the present invention;
[0035] Figure 2 The AgSb doped with different amounts of Sn in Examples 1-3 of the present invention 1-x Sn x Transmission electron microscopy (TEM) images of Se2 nanocrystals, from top to bottom: AgSb 0.97 Sn 0.03 Se2, AgSb 0.98 Sn 0.02 Se2 and AgSb 0.99 Sn0.01 Se2;
[0036] Figure 3 The AgSb synthesized in Examples 1-3 and Comparative Example 1 of the present invention is 1-x Sn x X-ray diffraction patterns (XRD) of Se2 (x = 0, 0.01, 0.02, 0.03) nanocrystals;
[0037] Figure 4 AgSb in Example 2 of the present invention 0.98 Sn 0.02 X-ray photoelectron spectroscopy (XPS) of Sn3d in untreated and untreated Se2 samples, where the treated samples refer to AgSb 0.98 Sn 0.02 Se2 nanocrystal samples were treated by two-step surface chemical method to obtain AgSb 0.98 Sn 0.02 Se2 nanomaterials, the untreated sample refers to AgSb without two-step surface chemical treatment 0.98 Sn 0.02 Se2 nanomaterials;
[0038] Figure 5 The AgSb after hot pressing and sintering densification in Example 4 of the present invention 1-x Sn x X-ray diffraction patterns (XRD) of bulk samples of Se2 (x = 0, 0.01, 0.02 and 0.03) thermoelectric materials;
[0039] Figure 6 The AgSb after hot pressing and sintering densification in Example 4 of the present invention 0.98 Sn 0.02 Cross-sectional scanning electron microscope image (SEM) of Se2 bulk sample;
[0040] Figure 7 The AgSbSe2 (pure sample) and AgSbSe2 (pure sample) after sintering and densification in Example 4 of the present invention are 0.98 Sn 0.02 Se2 (untreated), AgSb 0.98 Sn 0.02 The relationship between the conductivity of three different thermoelectric materials, AgSbSe2 (after treatment) and temperature, where the pure sample refers to the nano thermoelectric material after sintering and densification of the AgSbSe2 nanomaterial subjected to two-step surface chemical treatment in Comparative Example 1, and the untreated sample refers to the AgSbSe2 nanomaterial subjected to two-step surface chemical treatment in Example 2. 0.98 Sn 0.02 The nano thermoelectric material after sintering and densification of Se2 nanocrystals, the treated sample refers to the AgSb treated with two-step surface chemical treatment in Example 2. 0.98Sn 0.02 Nano thermoelectric materials after sintering and densification of Se2 nanomaterials;
[0041] Figure 8 The AgSbSe2 (pure sample after treatment) and AgSbSe2 after sintering and densification in Example 4 of the present invention are 0.98 Sn 0.02 Se2 (untreated), AgSb 0.98 Sn 0.02 The relationship between the thermoelectric figure of merit zT of three different thermoelectric materials Se2 (after treatment) and temperature, where the pure sample refers to the nano thermoelectric material after sintering and densification of the AgSbSe2 nanomaterial subjected to two-step surface chemical treatment in Comparative Example 1, and the untreated sample refers to the AgSbSe2 nanomaterial subjected to two-step surface chemical treatment in Example 2. 0.98 Sn 0.02 The nano thermoelectric material after sintering and densification of Se2 nanocrystals, the treated sample refers to the AgSb treated with two-step surface chemical treatment in Example 2. 0.98 Sn 0.02 Nano thermoelectric material after sintering and densification of Se2 nanomaterials. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] An AgSbSe2-based 1-x Sn x Se2, x = 0.01) nano material preparation method, comprising the following steps:
[0045] Step 1: Synthesis of AgSbSe2-based nanocrystals by colloidal synthesis
[0046] a. Preparation of selenium source precursor: 70 mmol of Se powder was dissolved in 70 mL of oleylamine and 70 mL of n-dodecyl mercaptan, and the mixture was cycled three times under vacuum and nitrogen atmosphere at room temperature with continuous magnetic stirring until the selenium powder was completely dissolved.
[0047] b. Simultaneously, 35 mmol of AgNO3, 34.65 mmol of SbCl3, and 0.35 mmol of SnCl2 were added to a three-necked flask containing a mixed solution of 490 mL of oleylamine (OLA) and 70 mL of oleic acid (OA), and the mixture was continuously stirred with magnetic stirring. After keeping the mixture at room temperature for 30 min, the mixture was evacuated at 80°C for 1 hour to remove low-boiling impurities, and then heated to 120°C, nitrogen was introduced, and the temperature was rapidly raised to 220°C to obtain a cationic solution.
[0048] c. Rapidly inject 140mL of the selenium source precursor prepared in step a into the cationic solution of step b. After injection, the reaction solution changes from transparent yellow-brown to dark brown. At this time, the temperature drops to about 170°C. After the temperature rises to 220°C, keep reacting for 30 minutes, and then quickly cool in a water bath. Use chloroform to disperse the colloidal solution, and add anhydrous ethanol to precipitate the prepared nanocrystals. Centrifugal washing is performed 3 times, and the centrifugal speed and time are 8000rpm and 5 minutes respectively, to obtain AgSb 0.09 Sn 0.01 Se2 nanocrystals are dispersed in chloroform for later use.
[0049] Step 2: Prepare high-performance AgSbSe2-based nano-thermoelectric blocks using a two-step surface chemical treatment method
[0050] d. Prepare 100 mL of 20 mmol / L -1 NaBH4 solution, weigh 76mg of NaBH4 and dissolve it in 100mL of ethanol aqueous solution (ethanol 95ml, water 5mL), then mix it with the chloroform solution (150mL) of the nanocrystals (about 5g) synthesized in step c at a volume ratio of 3:1, shake for 1-2 minutes to exchange and remove the organic ligands on the surface of the nanocrystals, centrifuge and wash, add a certain amount of new chloroform and NaBH4 solution again and stir for 30min. Finally, wash the nanocrystals with anhydrous ethanol to remove excess NaBH4, and store the nanopowder in a glove box after vacuum drying.
[0051] e. Take a certain amount of the nanocrystalline powder dried in step d, introduce a mixed reducing gas of 95% N2 and 5% H2 into a tube furnace, and heat it at 10℃·min -1 The sample was heated to 250°C at a heating rate of 100 °C and annealed at 250°C for 12 hours. After annealing, the sample was quickly transferred to a glove box for storage to obtain the surface-treated AgSb 0.09 Sn 0.01 Se2 nanomaterials.
[0052] Example 2
[0053] An AgSbSe2-based 1-x Sn xSe2, x = 0.02) nanomaterial preparation method, the difference between this embodiment and embodiment 1 is that in step b, SbCl3 is 34.3mmol, SnCl2 is 0.70mmol, and step c obtains AgSb 0.98 Sn 0.02 Se2 nanocrystals, step e to obtain AgSb 0.98 Sn 0.02 Se2 nanomaterials. The remaining steps are the same as those in Example 1.
[0054] Depend on Figure 4 As shown, after treatment, it refers to AgSb 0.98 Sn 0.02 Se2 nanocrystal samples were treated by two-step surface chemical method to obtain AgSb 0.98 Sn 0.02 Se2 nanomaterials, untreated refers to AgSb without two-step surface chemical treatment 0.98 Sn 0.02 X-ray photoelectron spectroscopy (XPS) of Se2 nanocrystals, Sn3d, Sn 4+ :Sn 2+ The ratio decreased more than 3-fold, from 19.4% in the untreated samples to 6.2% in the treated samples.
[0055] Example 3
[0056] An AgSbSe2-based 1-x Sn x Se2, x = 0.03) nanomaterial preparation method, the difference between this embodiment and embodiment 1 is that in step b, SbCl3 is 33.95mmol, SnCl2 is 1.05mmol, and step c obtains AgSb 0.97 Sn 0.03 Se2 nanocrystals, step e to obtain AgSb after surface chemical treatment 0.98 Sn 0.02 Se2 nanomaterials. The remaining steps are the same as those in Example 1.
[0057] Comparative Example 1
[0058] An AgSbSe2-based 1-x Sn x Se2, x = 0) nanomaterial preparation method, the difference between this embodiment and embodiment 1 is that in step b, SbCl3 is 35mmol, SnCl2 is 0mmol, step c obtains AgSbSe2 nanocrystals, and step e obtains AgSbSe2 nanomaterial after surface treatment. The remaining steps are the same as in embodiment 1.
[0059] The morphology of the obtained samples was characterized by using a German Zeiss field emission scanning electron microscope Auriga Zeiss (SEM) and a transmission electron microscope ZEISSLIBRA120 (TEM). The sample phase was characterized by a German Bruker AXSD8ADVANCE X-ray diffractometer (XRD); the chemical valence state of Sn3d without and after surface chemical treatment was analyzed by a Swedish VGscientificESA X-ray photoelectron spectrometer (XPS).
[0060] like Figure 1 As shown, the morphology of the AgSbSe2 nanocrystals prepared in Comparative Example 1 is mainly uniform and monodispersed spherical, with a size of about 17±2 nanometers.
[0061] Depend on Figure 2 As shown, the three different Sn concentrations in Examples 1-3 have little effect on the size distribution and morphology of the nanocrystals.
[0062] Depend on Figure 3 As shown, the XRD analysis shows a cubic phase structure, which is consistent with the peaks of pure phase AgSbSe2, and no impurity peaks appear.
[0063] Example 4
[0064] An AgSbSe2-based nano thermoelectric material:
[0065] In a glove box, the AgSbSe2-based (AgSb 1- x Sn x Se2, x = 0, 0.01, 0.02 and 0.03) nanomaterials were poured into a graphite mold with an inner liner of 0.20 mm carbon paper and a diameter of 8.6 mm, and sintered using a commercial hot pressing system under nitrogen protection. The nanopowders were hot pressed and sintered at 360 ° C for 30 min under a pressure of 70 MPa to densify them into mm × 1.5 mm disc.
[0066] The AgSb without two-step surface chemical treatment in Example 2 0.98 Sn 0.02 Se2 nanomaterials are densified into nano-thermoelectric blocks under the same hot pressing and sintering conditions.
[0067] Table 1. Different nano thermoelectric blocks AgSb prepared in Example 4 1-x Sn x Density table of Se2
[0068]
[0069] The block density obtained in Example 4 is within the theoretical density (6.60 g·cm -3 ) is between 93% and 96%.
[0070] The performance and structural morphology of the sintered samples and their cross sections were characterized by the formula ZT=TσS 2 κ -1 (where T is the absolute thermodynamic temperature; S is the Seebeck coefficient; σ is the electrical conductivity; κ is the thermal conductivity; where κ = λC p ρ,λ are thermal diffusion coefficients, C p is the specific heat, ρ is the bulk density) and the thermoelectric figure of merit zT is calculated.
[0071] The sample phase was characterized by using a German Bruker AXSD8ADVANCE X-ray diffractometer (XRD); the AgSb2O3 densified by hot pressing after surface chemical treatment was characterized by using a German Zeiss field emission scanning electron microscope (SEM). 0.98 Sn 0.02 The cross-sectional structure and morphology of Se2 block were characterized. The conductivity (σ) and Seebeck coefficient (S) of the sample were tested using the German Lindsay Seebeck coefficient / resistance analysis system LSR-3; the Hall carrier concentration and Hall mobility of the sample were tested using the American Quantum Science Hall Effect Test System PPMS-9T; the thermal diffusion coefficient of the sample was measured using the German Lindsay laser thermal conductivity meter LFA-1000; and the specific heat of the sample was measured using the German Netzsch differential scanning calorimeter DSC 404F3.
[0072] like Figure 5 As shown, the XRD half-peak width of the sample after hot pressing sintering becomes narrower and the diffraction peak is sharper, indicating that the sample has better crystallinity and larger grains.
[0073] like Figure 6 As shown, after hot pressing sintering, AgSb 0.98 Sn 0.02 The Se2 bulk samples are large grains ranging from several hundred nanometers to micrometers, with a small amount of nanostructured pores.
[0074] like Figure 7 As shown, the sample with surface chemical treatment has higher conductivity, followed by the sample without surface treatment, and the surface treated but pure phase AgSbSe2 has the lowest conductivity.
[0075] like Figure 8 As shown in the figure, the maximum zT value of the treated pure sample AgSbSe2 reaches 0.58 at 664K, while the untreated AgSb 0.98 Sn 0.02The maximum zT value of Se2 reaches 1.14 at 667K, while the treated AgSb 0.98 Sn 0.02 The maximum zT value of Se2 reaches 1.37 at 666K, which is the highest zT value of AgSbSe2-based thermoelectric materials.
[0076] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. AgSbSe 2 Method for preparing nanomaterials, It is characterized in that The following steps are involved: Step 1: Synthesis of AgSbSe by colloidal synthesis 2 Nanocrystals AgNO 3 、SbCl 3 SnCl 2 The powder of Se is reacted with the powder according to the atomic ratio of Ag:Sb:Sn:Se=1:(1-x):x:2, wherein 0<x≤0.03, and then added into a mixed solution containing oleylamine and oleic acid, stirred at room temperature under nitrogen protection, and then vacuumed at 80-100°C for 30-60min, then heated to 110-120°C and introduced with nitrogen, and rapidly heated to 200-240°C for reaction, and the Se source precursor is injected into the reaction solution, and the reaction is kept warm for more than 30min after the temperature rises to 220°C, and after the reaction is completed, the reaction solution is cooled to room temperature in a water bath, and centrifuged and washed to prepare Sn-doped AgSbSe 2 Base nanocrystals; Step 2: Preparation of AgSbSe by two-step surface chemical treatment 2 Nanomaterials Sn-doped AgSbSe 2 The nanocrystals were dispersed in chloroform and then reacted with NaBH 4 The solution was mixed, vortexed, centrifuged, and then chloroform and NaBH were added again. 4 The solution was stirred at room temperature; the product was washed to remove excess NaBH 4 , vacuum drying; take the dried AgSb 1-x Sn x Se 2 The nanocrystals were annealed in a tube furnace, and a nitrogen-hydrogen mixed reducing gas was introduced into the tube furnace to obtain AgSbSe with surface chemical treatment. 2 Based on nano thermoelectric material powder.
2. The AgSbSe according to claim 1 2 Method for preparing nanomaterials, Features: In the step 1, washing is performed three times with chloroform and anhydrous ethanol.
3. The AgSbSe according to claim 1 2 Method for preparing nanomaterials, Features: In step 1, the volume ratio of oleylamine to oleic acid is ≥5:
1.
4. The AgSbSe according to claim 1 2 Method for preparing nanomaterials, Features: In step 1, the Se source precursor is prepared as follows: Se powder is weighed and transferred to a mixed solution of oleylamine and n-dodecyl mercaptan, and the mixture is stirred continuously under nitrogen protection at room temperature until the Se powder is completely dissolved to obtain a Se source precursor, wherein the concentration of the Se source precursor is 0.5 mol·L -1 , the volume ratio of oleylamine and n-dodecyl mercaptan is 1:
1.
5. The AgSbSe according to claim 1 2 Method for preparing nanomaterials, Features: In step 1, the single-phase AgSbSe 2 The base nanocrystals have a cubic rock-salt structure of NaCl.
6. The AgSbSe according to claim 1 2 Method for preparing nanomaterials, Features: In step 2, NaBH 4 The solution is NaBH 4 Dissolved in ethanol aqueous solution, ethanol aqueous solution is a mixed solution of 95% ethanol and 5% deionized water. 4 The concentration of ethanol aqueous solution is 20.0mmol·L -1 .
7. The AgSbSe according to claim 1 2 Method for preparing nanomaterials, Features: In step 2, the annealing treatment is as follows: the temperature is kept at 250°C for 10 to 12 hours, the heating rate is 5 to 10°C / min, and the nitrogen-hydrogen mixed gas is composed of 95% N 2 and 5% by volume H 2 composition.
8. An AgSbSe according to any one of claims 1 to 7 2 AgSbSe prepared by the preparation method of base nanomaterials 2 Based nanomaterials.
9. A thermoelectric material, Features: The AgSbSe 2 The thermoelectric material is obtained by hot pressing and sintering the base nanomaterial to densify it.
10. A thermoelectric material according to claim 9, Features: The hot pressing sintering densification is carried out at a pressure of 60 to 70 MPa and a temperature of 360 to 380° C. for 20 to 30 minutes.