Crystallization and purification method of electronic grade ammonium cerium nitrate

Through multiple processes of multi-stage cooling crystallization and water washing and drying, combined with a slow-then-fast cooling curve and an appropriate stirring speed, the problem of insufficient impurity content in cerium ammonium nitrate crystals in the existing technology has been solved, and the production of high-purity cerium ammonium nitrate has been achieved. Preparation, meeting SEMI G1 standards and improving crystallization efficiency and purity.

CN116514156BActive Publication Date: 2024-10-01HUBEI THREE GORGES LAB +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310388376.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-01
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

The existing technology cannot effectively prepare high-purity cerium ammonium nitrate crystals that meet the SEMI G1 standard of the International Semiconductor Equipment and Materials Association, and there is insufficient research on impurity removal during the crystallization process, resulting in a metal impurity content that cannot be less than 100 ppb.

Method used

Using a multi-stage cooling crystallization method, through multiple cooling crystallizations and water washing and drying of the cerium ammonium nitrate solution, combined with a slow-then-fast cooling curve and appropriate stirring speed and crystal growth time, high-purity purification and gradual separation of cerium ammonium nitrate are achieved Metal impurities, the content of all metal impurities is less than 100ppb.

Benefits of technology

It realizes the preparation of high-purity electronic grade products of cerium ammonium nitrate, meets the SEMI G1 standard, improves the crystallization efficiency and purity, reduces the adsorption of impurities on the crystal surface, and is suitable for the preparation of integrated circuit etching solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116514156B_ABST
    Figure CN116514156B_ABST
Patent Text Reader

Abstract

The present invention provides an electronic-grade ammonium cerium nitrate crystallization and purification method, and the ammonium cerium nitrate solution is prepared by adding a crude ammonium cerium nitrate product to water, heating and dissolving to obtain an ammonium cerium nitrate solution; primary crystallization: adding crystal seeds to the ammonium cerium nitrate solution, and performing cooling and crystallization during the stirring process, and after reaching the final temperature, the crystal is grown at a constant temperature; washing and drying: after the crystallization is completed, the slurry is filtered, washed, and vacuum-dried to obtain ammonium cerium nitrate crystals of a certain particle size; the obtained ammonium cerium nitrate crystals are repeatedly crystallized 2-3 times to obtain an electronic-grade ammonium cerium nitrate product. The present invention uses multi-stage cooling crystallization to purify ammonium cerium nitrate, avoiding the problem that the evaporation crystallization removes the solvent while the metal impurities remain in the crystal in the existing patent, and the mother liquor containing the metal impurities is separated from the crystal for many times, so that the content of all metal impurities is less than 100 ppb, reaching the SEMI international standard, and the obtained high-purity electronic-grade product can be used for the preparation of integrated circuit etching solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of crystallization, and particularly relates to a crystallization, purification and preparation method of electronic-grade ammonium cerium nitrate. Background Art

[0002] Cerium ammonium nitrate (NH 4 ) 2 Ce(NO 3 ) 6 ) is a kind of orange-red crystal with strong oxidizing property. Its aqueous solution can oxidize and dissolve many metals, including chromium with high oxidation potential, so it becomes an important component of integrated circuit etching solution. At present, the purity of domestic ammonium cerium nitrate is mostly industrial grade, the content of metal impurities is too high, and the quality is unstable. With the continuous upgrading of electronic industry manufacturing technology, the purity requirements of related raw materials are getting higher and higher. Therefore, it is urgent to develop deep purification technology of ammonium cerium nitrate. Crystallization is an important separation and purification method with the advantages of low energy consumption, low environmental pollution, simple operation and equipment. However, at present, there is a lack of in-depth research on the deep purification technology of electronic grade ammonium cerium nitrate crystallization in China.

[0003] There are very few patents on the preparation of high-purity ammonium cerium nitrate, with only three reports. Chinese Patent 02125765.5 converts trivalent cerium into tetravalent cerium by electrolysis, and then adds ammonium nitrate and concentrated nitric acid for precipitation, thereby preparing ammonium cerium nitrate crystals. This method can save nitric acid compared to the chemical oxidation crystallization method. The Fe, Ni, Pb and other metal contents in the prepared ammonium cerium nitrate crystals are less than 1ppm, which has not yet reached the G1 standard of the International Semiconductor Equipment and Materials Association (SEMI) (metal impurities <100ppb), and cannot be used to prepare etchants for integrated circuits. In addition, the oxidizing and acidic properties of the aqueous solution of ammonium cerium nitrate are extremely strong, which puts forward higher requirements on the membrane materials, electrode materials and concentrator materials involved in the whole process. Therefore, this method is difficult to apply and is not easy to industrialize. Chinese Patent 201510377239.5 first obtains cerium (III) nitrate solution by reacting cerium (III) carbonate with dilute nitric acid, then adds hydrogen peroxide and ammonia water to oxidize and precipitate to prepare tetravalent cerium hydroxide, then dissolves it with nitric acid, and finally adds ammonium nitrate solution to concentrate and crystallize at a slight negative pressure at 130°C to obtain ammonium cerium nitrate. The concentration of metal ions such as Cu, Ni, and Co in the ammonium cerium nitrate crystals prepared by this method is less than 0.5ppm, which does not meet the G1 standard, and the method performs evaporation crystallization at 130°C, which has high energy consumption. Chinese Patent 201910287523.1 adds multiple recrystallization operations of cerium (III) nitrate on the basis of the technical route of Patent 201510377239.5, and obtains ammonium cerium nitrate with higher purity, in which the content of metal impurities such as Cr, Cd, Cu, Ni, and Pb is less than 100ppb, but the content of Ca is less than 200ppb, and the content of Al and Fe is less than 150ppb, which has not yet reached the G1 standard. In summary, the existing preparation technology of ammonium cerium nitrate is still unable to obtain electronic grade ammonium cerium nitrate crystals with a content of all metal impurities less than 100 ppb. In addition, crystallization is the last step in the preparation of ammonium cerium nitrate crystals, but existing research has not conducted in-depth research on the removal of impurities in this process. Summary of the invention

[0004] In view of the shortcomings of the current method for preparing high-purity ammonium cerium nitrate, the present invention proposes a method for preparing high-purity electronic-grade ammonium cerium nitrate using industrial-grade ammonium cerium nitrate as a raw material and adopting multi-stage cooling crystallization, comprising the following steps:

[0005] (1) Preparation of ammonium cerium nitrate solution: adding crude ammonium cerium nitrate into water, heating and dissolving to obtain ammonium cerium nitrate solution;

[0006] (2) Primary crystallization: adding seed crystals to the ammonium cerium nitrate solution, and cooling and crystallizing during stirring. After reaching the final temperature, the crystals are grown at a constant temperature; (3) Washing and drying: after the crystallization is completed, the slurry is filtered, washed, vacuum dried, and screened to obtain ammonium cerium nitrate crystals of a certain particle size;

[0007] (4) Repeat steps (1) to (3) 2-3 times with the ammonium cerium nitrate crystals obtained in step (3) to obtain an electronic grade ammonium cerium nitrate product.

[0008] The water used for dissolving in step (1) is ultrapure water, and the concentration of the ammonium cerium nitrate solution is 1.8-2.2 g / mL.

[0009] In step (2), the seed crystals used have a particle size range of 50-100 μm and the amount of seed crystals added is 0.5%-3%.

[0010] In step (2), the temperature of the cooling crystallization process is reduced from 80°C to 10°C, the cooling rate is 0.1-1.2°C / min, and the stirring speed is 200-450rpm.

[0011] The cooling crystallization process adopts the cooling curve as follows, and the cooling curve equation is T = -5.4 × 10 -4 t 2 +80(t-min; T-℃).

[0012] The stirring speed during the cooling crystallization process is 300-400 rpm.

[0013] In step (2), the crystal growing temperature is 10-20° C., the crystal growing time is 0.5-2 h, and the stirring speed during the crystal growing stage is 100-300 rpm.

[0014] In step (3), ultrapure water is used for washing, the ultrapure water temperature is 5-10° C., and the washing is performed 1-3 times. The amount of water used for washing is 1 / 5-1 / 10 of the volume of the precipitated solid.

[0015] The technical solution of the present invention has the following beneficial effects:

[0016] (1) The present invention uses multi-stage cooling crystallization to purify ammonium cerium nitrate, avoiding the problem in existing patents that the solvent is removed by evaporation and crystallization while metal impurities remain in the crystals. The mother liquor containing metal impurities is separated from the crystals multiple times to achieve a total metal impurity content of less than 100 ppb, meeting the SEMI international standard. The obtained high-purity electronic-grade product can be used for the preparation of integrated circuit etching solution.

[0017] (2) Based on the solubility characteristics of ammonium cerium nitrate, the present invention designs a cooling curve that is slow at first and then fast. The slower cooling rate in the early stage is beneficial to avoiding explosive nucleation, and the faster cooling rate in the later stage is beneficial to the rapid growth of the nucleated crystals. Finally, an ammonium cerium nitrate product with a larger particle size is obtained, which not only improves the purification effect, but also shortens the entire crystallization process time and improves the crystallization efficiency.

[0018] (3) The present invention adds a crystal growing operation after the cooling is completed, and by increasing the crystal growing temperature, the dissolution of small particles is promoted to obtain crystals with a larger average particle size, thereby reducing the adsorption of impurities on the crystal surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of the cooling curve in the present invention.

[0020] Figure 2 The present invention is a process flow chart for purifying and preparing electronic grade ammonium cerium nitrate. DETAILED DESCRIPTION

[0021] In view of the above technical solution, in some actual operation processes, a method for preparing high-purity electronic grade ammonium cerium nitrate by multi-stage cooling crystallization comprises the following steps:

[0022] (1) Preparation of ammonium cerium nitrate solution: Add crude ammonium cerium nitrate into a crystallizer filled with water, accelerate the dissolution of the solid by stirring, and use a constant temperature water bath to control the temperature of the crystallizer. Continue stirring until the solid is completely dissolved and the temperature of the ammonium cerium nitrate solution reaches a constant level;

[0023] (2) Primary crystallization: set a cooling curve, add a certain amount of seed crystals, stir at a constant speed, perform primary crystallization, and after reaching the final temperature, keep the crystals at a constant temperature for a period of time;

[0024] (3) Washing and drying: After the crystallization is completed, the slurry is filtered, the filtered solid is washed in batches, and the solid finally collected is vacuum dried for a period of time;

[0025] (4) Seed crystal screening: The dried ammonium cerium nitrate crystals are sampled for impurity content analysis, and then the particle size is screened to select crystals within a certain particle size range as seed crystals, such as crystals with a particle size range of 50-100 μm, and the remaining solids are used as raw materials for recrystallization;

[0026] (5) Secondary crystallization: using the product of primary crystallization to prepare a secondary crystallization solution according to step (1), setting a secondary crystallization cooling curve, adding a certain amount of seed crystals, stirring at a constant speed, performing secondary crystallization, and after reaching the final temperature, maintaining the crystals at a constant temperature for a period of time. After the crystallization is completed, collecting the secondary crystallized ammonium cerium nitrate product according to steps (3) and (4), screening some crystals and using them as seed crystals, and taking samples for impurity content analysis; (6) Tertiary crystallization: using the product of secondary crystallization to prepare a tertiary crystallization solution according to step (1), setting a tertiary crystallization cooling curve, adding a certain amount of seed crystals, stirring at a constant speed, performing tertiary crystallization, and after reaching the final temperature, maintaining the crystals at a constant temperature for a period of time. After the crystallization is completed, collecting the tertiary crystallized ammonium cerium nitrate product according to steps (3) and (4), and taking samples for impurity content analysis.

[0027] Specifically, in step (1), the water used for dissolving is ultrapure water, and the concentration of the ammonium cerium nitrate solution is 1.8-2.2 g / mL.

[0028] Specifically, in step (2), the seed crystals used have a particle size range of 50-100 μm, and the amount of seed crystals added is 0.5%-3%.

[0029] Specifically, in step (2), the temperature of the cooling crystallization process is reduced from 80°C to 10°C, the cooling rate is 0.1-1.2°C / min, and the cooling curve equation is T=-5.4×10 -4 t 2 +80 (t-min; T-℃), the stirring speed is 200-450rpm, preferably 300-400rpm. Specifically, in the step (2), the crystal growing temperature is 10-20℃, the crystal growing time is 0.5-2h, and the stirring speed in the crystal growing stage is 100-300rpm. Specifically, in the step (3), ultrapure water is used for washing, the ultrapure water temperature is 5-10℃, the water washing is 1-3 times, and the amount of water used for washing is 1 / 5-1 / 10 of the volume of the precipitated solid.

[0030] Specifically, in the step (5), the temperature during the secondary crystallization is reduced from 80°C to 10°C, the cooling rate is 0.1-1.2°C / min, and the cooling curve equation is T=-5.4×10 -4 t 2 +80 (t-min; T-℃), stirring speed is 200-450 rpm, preferably 300-400 rpm.

[0031] Specifically, in step (5), the crystal growing temperature is 10-20° C., the crystal growing time is 0.5-2 h, and the stirring speed during the crystal growing stage is 100-300 rpm.

[0032] Specifically, in step (6), the tertiary crystallization temperature is reduced from 80°C to 10°C, the cooling rate is 0.1-1.2°C / min, and the cooling curve equation is T=-5.4×10 -4 t 2 +80 (t-min; T-℃), stirring speed is 200-450 rpm, preferably 300-400 rpm.

[0033] Specifically, in step (6), the crystal growing temperature is 10-20° C., the crystal growing time is 0.5-2 h, and the stirring speed during the crystal growing stage is 100-300 rpm.

[0034] Example 1

[0035] The crude ammonium cerium nitrate was added to a crystallizer filled with ultrapure water and stirred continuously until the solid was completely dissolved to prepare a 2.2 g / mL ammonium cerium nitrate solution. After the solution was kept constant at 80°C for a period of time, it was linearly cooled to 10°C at a rate of 0.15°C / min (the cooling crystallization process is as follows Figure 1 As shown), stirring at 200 rpm. Add 0.5% seed crystals at 78°C, wherein the seed crystals have a particle size range of 50-100 μm. After the crystallization is completed, filter the slurry, wash the filtered solid twice with 5-10°C ultrapure water, and the amount of water used for washing is 1 / 5 of the volume of the precipitated solid. Finally, vacuum dry the solid for 24 hours. Take the dried primary crystals to prepare ammonium cerium nitrate solution for secondary crystallization. The solution concentration, cooling rate and stirring speed conditions in the secondary crystallization and tertiary crystallization are the same as those in the primary crystallization process, and the post-treatment process including solid-liquid separation, water washing, drying and the like are also consistent. Among them, the tertiary crystallization solution is prepared from the dried secondary crystallization product.

[0036] Example 2

[0037] The crude ammonium cerium nitrate was added to a crystallizer filled with ultrapure water and stirred continuously until the solid was completely dissolved to prepare a 2.2 g / mL ammonium cerium nitrate solution. After the solution was kept constant at 80 °C for a period of time, the solution was stirred at 40 °C for 2 hours at a temperature of -5.4 × 10 -4 t 2 +80 (t-min; T-℃) curve cooling to 10℃ (cooling crystallization process is as follows Figure 1 As shown), stirring at 200rpm. 0.5% seed crystals are added at 78°C, wherein the seed crystals have a particle size range of 50-100μm. After the solution drops to 10°C, crystals are grown at this temperature for 0.5h, and the stirring speed during the crystal growing stage is 150rpm. After the crystal growing is completed, the slurry is filtered, and the filtered solid is washed twice with 5-10°C ultrapure water, and the amount of water used for washing is 1 / 5 of the volume of the precipitated solid. Finally, the solid is vacuum dried for 24h. The dried primary crystals are taken to prepare ammonium cerium nitrate solution for secondary crystallization. The solution concentration, cooling curve and stirring speed conditions in the secondary crystallization and tertiary crystallization are the same as those in the primary crystallization process, and the post-treatment process including solid-liquid separation, water washing, drying and other conditions are also consistent. Among them, the tertiary crystallization solution is prepared from the dried secondary crystallization product.

[0038] Example 3

[0039] The experimental operation was the same as in Example 2, except that the amount of seed added in the primary, secondary and tertiary cooling crystallization was changed to 1.5%.

[0040] Example 4

[0041] The experimental operation was the same as in Example 3, except that the amount of seed added in the primary, secondary and tertiary cooling crystallizations was changed to 3%.

[0042] Example 5

[0043] The experimental operation was the same as in Example 4, except that the stirring speed in the primary, secondary and tertiary cooling crystallization was changed to 300 rpm.

[0044] Example 6

[0045] The experimental operation was the same as in Example 5, except that the stirring speed in the primary, secondary and tertiary cooling crystallization was changed to 400 rpm.

[0046] Example 7

[0047] The experimental operation is the same as in Example 5, except that the temperature of the crystal growing process after the first, second and third stage cooling crystallization is changed to 20°C.

[0048] Example 8

[0049] The experimental operation was the same as in Example 7, except that the stirring speed during the crystal growing process after the first, second and third stage cooling crystallization was changed to 250 rpm.

[0050] Example 9

[0051] The experimental operation was the same as in Example 7, except that the crystal growing process time after the first, second and third stage cooling crystallization was changed to 1.0 h.

[0052] Example 10

[0053] The experimental operation was the same as in Example 7, except that the crystal growing process time after the first, second and third stage cooling crystallization was changed to 2.0 h.

[0054] Table 1

[0055]

[0056]

[0057] From the results in Table 1, it can be seen that the crystal purity obtained by simple linear cooling in Example 1 cannot meet the SEMI G1 standard, while Examples 2-10 adopt a slow-first-fast-later cooling curve to obtain electronic-grade ammonium cerium nitrate with a total impurity metal content of <100ppb, and greatly shorten the time of the entire crystallization process, thereby improving the crystallization efficiency. The present invention adopts a slower cooling rate in the early stage to avoid a large amount of nucleation, and increasing the cooling rate in the later stage is conducive to crystal growth. Therefore, the average particle size of the ammonium cerium nitrate crystals can be increased and the removal of impurities can be facilitated by regulating the crystallization kinetics. In addition, Examples 3-10 optimize the crystallization conditions, and can further improve the purity and particle size of electronic-grade ammonium cerium nitrate on the basis of Example 2:

[0058] (1) By comparing Examples 2-4, it can be seen that when the amount of seed crystals increases, the average particle size of ammonium cerium nitrate increases, and the purity also increases, indicating that increasing the amount of seed crystals is beneficial to controlling the formation of small particles in the cooling crystallization of ammonium cerium nitrate, and can further improve the purity of ammonium cerium nitrate crystals.

[0059] (2) By comparing Examples 4-6, it can be seen that when the stirring speed increases, the average particle size shows a trend of first increasing and then decreasing, and the purity of ammonium cerium nitrate will first increase and then decrease. The present invention provides an optimized stirring speed, which is beneficial to the mass transfer process on the one hand, and on the other hand, can avoid crystal wear and significant secondary nucleation caused by excessive stirring, thereby effectively improving the purity of ammonium cerium nitrate crystals.

[0060] (3) By comparing Examples 5 and 7, it can be seen that increasing the crystal growing temperature in the present invention is conducive to dissolving small particles, allowing large particles to continue to grow, thereby increasing the final average particle size of the crystals and further improving the purity of the ammonium cerium nitrate crystals.

[0061] (4) From the comparison of Examples 7-8, it can be seen that the crystal growing process needs to control the appropriate stirring speed to ensure the purification effect.

[0062] (5) By comparing Examples 7, 9 and 10, it can be seen that the present invention can further increase the crystal size of ammonium cerium nitrate and obtain a crystal product with higher purity by increasing the crystal growing time.

Claims

1. A method for crystallizing and purifying electronic grade ammonium cerium nitrate, characterized in that: The following steps are involved: (1) Preparation of ammonium cerium nitrate solution: adding crude ammonium cerium nitrate into water, heating and dissolving to obtain ammonium cerium nitrate solution; (2) Primary crystallization: Add seed crystals to the ammonium cerium nitrate solution, and perform cooling crystallization during stirring. After reaching the final temperature, the crystals are grown at a constant temperature. During the cooling crystallization process, the following cooling curve is used for cooling crystallization. The cooling curve equation is: , during the cooling crystallization process, the stirring speed is 300-400 rpm, the crystal growing temperature is 10-20℃, the crystal growing time is 0.5-2 h, the stirring speed during the crystal growing stage is 100-300 rpm, the particle size range of the seed crystal used is 50-100 μm, and the seed crystal addition amount is 0.5%-3%; (3) Washing and drying: After the crystallization is completed, the slurry is filtered, washed, vacuum dried, and screened to obtain ammonium cerium nitrate crystals of a certain particle size; (4) Repeat steps (1) to (3) 2-3 times with the ammonium cerium nitrate crystals obtained in step (3) to obtain an electronic grade ammonium cerium nitrate product.

2. The electronic grade ammonium cerium nitrate crystallization and purification method according to claim 1, wherein: The water used for dissolving in step (1) is ultrapure water, and the concentration of the ammonium cerium nitrate solution is 1.8-2.2 g / mL.

3. The electronic grade ammonium cerium nitrate crystallization and purification method according to claim 1, wherein: In step (2), the temperature of the cooling crystallization process is reduced from 80°C to 10°C, the cooling rate is 0.1-1.2°C / min, and the stirring speed is 200-450 rpm.

4. The electronic grade ammonium cerium nitrate crystallization and purification method according to claim 1, wherein: In step (3), ultrapure water is used for washing. The ultrapure water temperature is 5-10° C., and the washing is performed 1-3 times. The amount of water used for washing is 1 / 5-1 / 10 of the volume of the precipitated solid.

Citation Information

Cited By

  • Electronic-grade ceric ammonium nitrate and industrial production method thereof

    CN121342073A