Electrode silver paste and preparation method thereof, chip capacitor
By using an electrode silver paste that combines sheet-like and spherical silver powder, the problems of low adhesion and poor appearance in surface mount capacitors have been solved, resulting in surface mount capacitors with high density and good appearance, suitable for special applications.
Patent Information
- Application Number
- CN202310703072.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-06-13
AI Technical Summary
Existing sinterable electrode silver pastes have problems such as low adhesion, protruding internal electrodes after sintering, and poor appearance in surface mount capacitors, especially in large-size surface mount capacitors, making it difficult to meet the requirements of special fields.
By combining flake and spherical silver powders, along with silver powders of different tap densities and particle sizes, and adding glass powder and binders, a chip capacitor suitable for silver-palladium systems can be prepared by adjusting the density and leveling properties of the silver paste.
The density and leveling properties of the electrode silver paste are improved, ensuring good appearance and reliability of the surface mount capacitors, making them suitable for demanding special applications.
Smart Images

Figure CN116525172B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of conductive pastes, and in particular to an electrode silver paste and a preparation method thereof, and a chip capacitor. Background Art
[0002] In the military, medical, automotive and other industries, the reliability and other requirements for chip capacitors are very high. However, the existing sinterable electrode silver paste has defects such as low adhesion, protruding internal electrodes after sintering, and poor appearance. Especially in large-size chip capacitors, the defects are more prominent and it is difficult to meet the requirements of special fields. Summary of the invention
[0003] The purpose of the present disclosure is to provide an electrode silver paste and a preparation method thereof, and a chip capacitor, which is used to provide an electrode silver paste suitable for silver-palladium system chip capacitors in special fields.
[0004] In order to achieve the above objectives, the present disclosure provides the following technical solutions:
[0005] An electrode silver paste, comprising: flaky silver powder, spherical silver powder, glass powder and adhesive, wherein:
[0006] The flaky silver powder includes flaky silver powder A and flaky silver powder B having different tap densities;
[0007] The spherical silver powder includes spherical silver powder C and spherical silver powder D with different particle sizes.
[0008] Compared with the prior art, the electrode silver paste provided by the present disclosure includes: flaky silver powder, spherical silver powder, glass powder and adhesive. Since only spherical silver powder of different particle sizes is used, although the density of the electrode silver paste can be improved, when there are too many small particles of spherical silver powder in the electrode silver paste, or mutual diffusion is formed between the internal electrode material, the internal electrode protrudes and other undesirable appearance phenomena occur. Therefore, the present disclosure uses flaky silver powder and spherical silver powder at the same time, so that the gaps between the spherical silver powders can be filled with flaky silver powder, thereby reducing the holes between the silver layers of the electrode silver paste, overcoming the above-mentioned diffusion problem, and improving the density of the electrode silver paste. When the electrode silver paste is used to prepare chip capacitors, due to its good density, the dipping process of the silver paste is good, and appearance defects are not easy to occur, so that the reliability of the prepared chip capacitors is high.
[0009] Based on this, the above-mentioned flaky silver powder includes flaky silver powder A and flaky silver powder B with different tap densities. By using flaky silver powders with different tap densities, the leveling property of the electrode slurry is improved, thereby improving the appearance flatness of the chip capacitor prepared using the electrode slurry. The above-mentioned spherical silver powder includes spherical silver powder C and spherical silver powder D with different particle sizes. By using spherical silver powders with different particle sizes, part of the gaps between spherical silver powders and between spherical silver powders and flaky silver powders can be filled with spherical silver powders with different particle sizes, further improving the compactness of the electrode slurry. By using the above-mentioned four types of silver powders, the compactness of the electrode silver paste is improved, and the leveling property is also improved, so that the reliability of the prepared chip capacitor is better, which is suitable for special fields with high requirements for chip capacitors.
[0010] The present disclosure also provides a method for preparing an electrode silver paste based on an exemplary embodiment of the present disclosure, the method comprising:
[0011] preparing glass powder under first reaction conditions; the first reaction conditions include a reaction temperature of 1000° C. to 1500° C. and a reaction time of 1 h to 2 h;
[0012] The flaky silver powder, the spherical silver powder and the glass powder are uniformly mixed with a binder to obtain an electrode silver paste.
[0013] Compared with the prior art, the beneficial effects of the preparation method of the electrode silver paste provided in the present disclosure are the same as the beneficial effects of the electrode silver paste described in the above technical solution, which will not be elaborated here.
[0014] The present disclosure also provides a chip capacitor, including a terminal electrode, wherein the terminal electrode is prepared by applying the electrode silver paste described in the exemplary embodiment of the present disclosure.
[0015] Compared with the prior art, the beneficial effects of the chip capacitor provided by the present invention are the same as the beneficial effects of the electrode silver paste described in the above technical solution, which will not be elaborated here. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings described herein are used to provide a further understanding of the present disclosure and constitute a part of the present disclosure. The illustrative embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute an improper limitation on the present disclosure. In the drawings:
[0017] Figure 1 A flowchart of a method for preparing an electrode silver paste provided by an exemplary embodiment of the present disclosure is shown. DETAILED DESCRIPTION
[0018] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.
[0019] Various structural schematic diagrams according to embodiments of the present disclosure are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may further design regions / layers with different shapes, sizes, and relative positions according to actual needs.
[0020] In the context of the present disclosure, when a layer / element is referred to as being "on" another layer / element, the layer / element may be directly on the other layer / element, or there may be an intermediate layer / element between them. In addition, if a layer / element is "on" another layer / element in one orientation, then when the orientation is reversed, the layer / element may be "under" the other layer / element. In order to make the technical problems, technical solutions and beneficial effects to be solved by the present disclosure clearer, the present disclosure is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not intended to limit the present disclosure.
[0021] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present disclosure, "multiple" means two or more, unless otherwise clearly and specifically defined. "Several" means one or more, unless otherwise clearly and specifically defined.
[0022] In the description of the present disclosure, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.
[0023] Base metals are all metals other than precious metals such as gold, silver, platinum, etc. For example, iron, copper, nickel, aluminum, lead, zinc, tin, tungsten, etc.
[0024] MLCC generally refers to chip capacitors. Chip capacitors are a type of capacitor material. The full name of chip capacitors is: Multilayer (laminated, stacked) chip ceramic capacitors (Multilayer Ceramic Capacitor, MLCC), also known as chip capacitors, chip capacitors.
[0025] MLCC is the most widely used passive component. In recent years, with the rapid development of 5G, smart phones, the Internet of Things, and the automotive medical industry, the market demand for MLCC has continued to increase. Although my country's MLCC industry is developing rapidly, high-end MLCC still needs to rely on imports.
[0026] In the early days, MLCC used the silver-palladium system, that is, the inner electrode used silver-palladium paste or pure palladium paste, and the terminal electrode used silver paste, but the cost was relatively high. In order to reduce costs, MLCC gradually developed into a base metal system, that is, nickel was used as the inner electrode and copper was used as the terminal electrode. Today, BME-MLCC (base metal electrode chip multilayer ceramic capacitor) accounts for more than 90% of all MLCCs. However, in some military, medical, automotive and other industries, the requirements for MLCC reliability and other aspects are very high, and the silver-palladium system is still needed. Therefore, it is necessary to provide an electrode silver paste for the silver-palladium system.
[0027] The existing sinterable electrode silver paste has defects such as low adhesion, protruding internal electrodes after sintering, and poor appearance. Especially in large-size chip capacitors, the defects are more prominent and it is difficult to meet the requirements of special fields.
[0028] In order to overcome the above problems, an exemplary embodiment of the present disclosure provides an electrode silver paste, which has good compactness and can be used to prepare a chip capacitor with good appearance.
[0029] The electrode silver paste comprises: flaky silver powder, spherical silver powder, glass powder and adhesive, wherein the flaky silver powder comprises flaky silver powder A and flaky silver powder B with different tap densities, and the spherical silver powder comprises spherical silver powder C and spherical silver powder D with different particle sizes.
[0030] As can be seen from the above, in the electrode silver paste of the exemplary embodiment of the present disclosure, the electrode silver paste includes: flaky silver powder, spherical silver powder, glass powder and adhesive. Since only spherical silver powder of different particle sizes is used, although the density of the electrode silver paste can be improved, when there are too many small particles of spherical silver powder in the electrode silver paste, or mutual diffusion is formed between the internal electrode material, the internal electrode protrudes and other undesirable appearance phenomena occur. Therefore, the exemplary embodiment of the present disclosure uses flaky silver powder and spherical silver powder at the same time, so that the gaps between the spherical silver powders can be filled with flaky silver powder, thereby reducing the holes between the silver layers of the electrode silver paste, overcoming the above-mentioned diffusion problem, and improving the density of the electrode silver paste. When the electrode silver paste is used to prepare chip capacitors, due to its good density, the dipping process of the silver paste is good, and appearance defects are not easy to occur, so that the reliability of the prepared chip capacitors is high.
[0031] Based on this, the above-mentioned flaky silver powder includes flaky silver powder A and flaky silver powder B with different tap densities. By using flaky silver powders with different tap densities, the leveling property of the electrode slurry is improved, thereby improving the appearance flatness of the chip capacitor prepared using the electrode slurry. The above-mentioned spherical silver powder includes spherical silver powder C and spherical silver powder D with different particle sizes. By using spherical silver powders with different particle sizes, part of the gaps between spherical silver powders and between spherical silver powders and flaky silver powders can be filled with spherical silver powders with different particle sizes, further improving the compactness of the electrode slurry. By using the above-mentioned four types of silver powders, the compactness of the electrode silver paste is improved, and the leveling property is also improved, so that the reliability of the prepared chip capacitor is better, which is suitable for special fields with high requirements for chip capacitors.
[0032] As a possible implementation method, the above-mentioned adhesive includes a polymer resin and an organic solvent. By using an adhesive, the viscosity of the electrode silver paste can be controlled within a reasonable range, so that when the electrode silver paste is used to prepare a chip capacitor, the prepared chip capacitor has a good appearance and good processability. Among them, the mass ratio of the polymer resin, the organic solvent and the flaky silver powder can be (1-5): (10-20): (10-60). For example, the mass ratio of the polymer resin, the organic solvent and the flaky silver powder can be 1:10:10, 2:15:50, 5:20:60, etc., and is not limited to this.
[0033] In some optional ways, the polymer resin may include one or more of ethyl cellulose, polyvinyl butyral resin, acrylic resin, cellulose acetate butyrate, rosin resin, epoxy resin and chloroacetic resin. For example, the polymer resin may include ethyl cellulose, polyvinyl butyral resin, acrylic resin, cellulose acetate butyrate, rosin resin, epoxy resin, chloroacetic resin, cellulose acetate butyrate and rosin resin, epoxy resin and chloroacetic resin, and may also include ethyl cellulose, polyvinyl butyral resin, acrylic resin, cellulose acetate butyrate, rosin resin, epoxy resin and chloroacetic resin, etc., but not limited thereto. By using a polymer resin, all organic matter in the electrode silver paste of the exemplary embodiment of the present disclosure can be uniformly dispersed in the polymer resin, which has a bonding effect.
[0034] In some optional ways, the above-mentioned organic solvent may include one or more of butyl carbitol, butyl carbitol acetate, alcohol ester twelve, pineol, ethylene glycol hexyl ether, diethylene glycol methyl ether, diethylene glycol dimethyl ether and tripropylene glycol methyl ether. For example, the organic solvent may include butyl carbitol, butyl carbitol acetate, alcohol ester twelve, pineol, ethylene glycol hexyl ether, diethylene glycol methyl ether, diethylene glycol dimethyl ether, tripropylene glycol methyl ether, diethylene glycol methyl ether and tripropylene glycol methyl ether, and may also include butyl carbitol, butyl carbitol acetate, alcohol ester twelve, pineol, ethylene glycol hexyl ether, diethylene glycol methyl ether\diethylene glycol dimethyl ether and tripropylene glycol methyl ether, etc., but not limited to this. By adding an organic solvent to the electrode silver paste to adjust the viscosity of the electrode silver paste, it is also used to adjust the surface drying rate of the electrode silver paste during the drying process to ensure that the appearance of the patch capacitor prepared using the electrode silver paste is good.
[0035] In practical applications, the organic solvent may have a boiling point of 180° C. to 250° C. This is to avoid the phenomenon that the electrode silver paste is difficult to dry due to the high temperature of the organic solvent, and the electrode silver paste boils on the surface during vacuuming due to the low temperature, which affects the appearance of the chip capacitor.
[0036] As a possible implementation method, the electrode silver paste may further include an additive. By adding an additive, the leveling property of the electrode silver paste can be further improved to ensure that the chip capacitor prepared using the electrode silver paste has a good appearance and good processing properties. The mass ratio of flaky silver powder, spherical silver powder, glass powder, adhesive and additive can be (10-60): (10-70): (1-10): (11-25): (0-4). For example, the mass ratio of flaky silver powder, spherical silver powder, glass powder, adhesive and additive can be 10:10:1:11:0, 50:55:7:15:2, 60:70:10:25:4, etc., but is not limited thereto.
[0037] The above-mentioned auxiliary agent can be selected according to actual conditions. For example, the auxiliary agent can include one or more of an anti-settling thixotropic agent, a dispersant, a leveling agent and a defoaming agent. For example, the auxiliary agent can include an anti-settling thixotropic agent, a dispersant, a leveling agent, a defoaming agent, an anti-settling thixotropic agent, a dispersant, a leveling agent and a defoaming agent, etc., but is not limited thereto.
[0038] In some optional ways, the anti-settling thixotropic agent may include one or more of polyamide wax, hydrogenated castor oil, carbomer and fumed silica. For example, the anti-settling thixotropic agent may include polyamide wax, hydrogenated castor oil, carbomer, fumed silica, carbomer and fumed silica, polyamide wax, hydrogenated castor oil, carbomer and fumed silica, etc., but not limited thereto. By using the anti-settling thixotropic agent, the various components in the electrode silver paste can be uniformly mixed together to prevent the components from settling.
[0039] In some optional embodiments, the mass ratio of the anti-settling thixotropic agent to the flaky silver powder may be (0-1):(10-60). For example, the mass ratio of the anti-settling thixotropic agent to the flaky silver powder may be 0:10, 5:55, 1:60, etc., but is not limited thereto.
[0040] In some optional ways, the above-mentioned dispersant may include one or more of a phosphate dispersant, a modified polyether phosphate dispersant, and an acrylate dispersant. For example, the dispersant may include a phosphate dispersant, a modified polyether phosphate dispersant, an acrylate dispersant, a phosphate dispersant, a modified polyether phosphate dispersant, and an acrylate dispersant, etc., but is not limited thereto. By using a dispersant, the silver particles and inorganic substances in the electrode silver paste are evenly dispersed, and agglomeration is not likely to occur, thereby improving the leveling property of the electrode silver paste, so that the appearance of the prepared patch electrode is good and the processing technology is good.
[0041] In some optional embodiments, the mass ratio of the dispersant to the spherical silver powder may be (0-1):(10-60). For example, the mass ratio of the dispersant to the spherical silver powder may be 0:10, 5:55, 1:60, etc., but is not limited thereto.
[0042] In some optional ways, the leveling agent may include one or more of polyether-modified silicone, acrylate compounds and fluorocarbon-modified polyacrylate compounds. For example, the leveling agent may include polyether-modified silicone, acrylate compounds, fluorocarbon-modified polyacrylate compounds, polyether-modified silicone, acrylate compounds and fluorocarbon-modified polyacrylate compounds, etc., but is not limited thereto. By adding the leveling agent and the dispersant to produce a synergistic effect, the surface tension of the silver particles in the electrode silver paste is reduced, so that the leveling property of the electrode silver paste is further improved.
[0043] In some optional embodiments, the mass ratio of the leveling agent to the spherical silver powder can be (0-1): (10-60). For example, the mass ratio of the leveling agent to the spherical silver powder can be 0:10, 5:55, 1:60, etc., but is not limited thereto.
[0044] In some optional ways, the above-mentioned defoaming agent may include one or more of modified polysiloxane, acrylate polymer and vinyl polymer. For example, the defoaming agent may include modified polysiloxane, acrylate polymer, vinyl polymer, modified polysiloxane, acrylate polymer and vinyl polymer, etc., but is not limited thereto. By adding a defoaming agent, when the electrode silver paste of the exemplary embodiment of the present disclosure is used in a dipping process, the bubbles in the electrode silver paste can be reduced, thereby ensuring that the performance of the prepared chip capacitor is better.
[0045] In some optional embodiments, the mass ratio of the defoamer to the spherical silver powder may be (0-1):(10-60). For example, the mass ratio of the defoamer to the spherical silver powder may be 0:10, 5:55, 1:60, etc., but is not limited thereto.
[0046] As a possible implementation, the tap density of the above-mentioned flaky silver powder A can be 3.5g / ml to 4.5g / ml. For example, the tap density of the flaky silver powder A can be 3.5g / ml, 4.0g / ml, 4.5g / ml, etc., but not limited thereto. The tap density of the flaky silver powder B is 5g / ml to 6g / ml. For example, the tap density of the flaky silver powder B can be 5g / ml, 5.5g / ml, 6.0g / ml, etc., but not limited thereto. Since the tap density of the flaky silver powder A is relatively low and its specific surface area is high, the viscosity of the electrode slurry will be relatively high, while the tap density of the flaky silver powder B is relatively high, resulting in the viscosity of the electrode slurry being too low, affecting the appearance of the chip capacitor. Therefore, in order to avoid the poor appearance of the chip capacitor due to the high viscosity of the electrode slurry, the flaky silver powder A and the flaky silver powder B can be mixed to adjust the specific surface area of the flaky silver powder and reduce the viscosity of the electrode slurry, so that the electrode slurry has good leveling properties and high density, thereby ensuring the good appearance of the prepared chip capacitor.
[0047] As a possible implementation, the particle size D50 of the spherical silver powder C can be 0.1 μm to 1.5 μm, for example, the particle size D50 of the spherical silver powder C can be 0.1 μm, 0.7 μm, 1.5 μm, etc., but not limited thereto. The tap density of the spherical silver powder C can be 4.0 g / ml to 5.0 g / ml, for example, the tap density of the spherical silver powder C can be 4.0 g / ml, 4.5 g / ml, 5.0 g / ml, etc., but not limited thereto. The particle size D50 of the spherical silver powder D is 2 μm to 6 μm, for example, the particle size D50 of the spherical silver powder D can be 2 μm, 5 μm, 6 μm, etc., but not limited thereto. The tap density of the spherical silver powder D is 5.0 g / ml to 6.0 g / ml. For example, the tap density of the spherical silver powder D can be 5.0 g / ml, 5.5 g / ml, 6.0 g / ml, etc., and is not limited thereto. By using two spherical silver powders with different tap densities and different particle sizes, the electrode silver paste prepared by mixing the spherical silver powder and the flake silver powder has good leveling properties. The spherical silver powder with a small particle size can also be used to fill the gaps between the silver powders to improve the compactness of the electrode silver paste, thereby improving the conductive performance of the chip capacitor.
[0048] As a possible implementation, in order to avoid the poor leveling due to the low tap density of the added silver powder, to ensure the leveling of the electrode silver paste while improving the compactness of the electrode silver paste, the mass ratio of the above-mentioned flaky silver powder A and flaky silver powder B can be (1:5) to (1:1), and the mass ratio of the spherical silver powder C and spherical silver powder D can be (1:4) to (1:1). For example, the mass ratio of the flaky silver powder A and the flaky silver powder B can be 1:5, 1:2, or 1:1, etc., and is not limited thereto. The mass ratio of the spherical silver powder C and the spherical silver powder D can be 1:4, 1:2, or 1:1, etc., and is not limited thereto.
[0049] As a possible implementation, the particle size D50 of the glass powder can be 1 μm to 2 μm, for example, the particle size D50 of the glass powder can be 1 μm, 1.5 μm, or 2 μm, etc., and is not limited thereto. By selecting glass powder with a particle size that meets the requirements of the present disclosure, on the one hand, the effect of too large a particle size on the appearance of the patch capacitor prepared by the electrode silver paste can be avoided, and on the other hand, the effect of too high a viscosity of the electrode silver paste on the appearance of the patch capacitor prepared by the electrode silver paste due to too small a particle size can be avoided.
[0050] In order to provide adhesion between the electrode silver paste and the magnet and prevent the problem of the electrode silver paste falling off during use, the glass powder may include oxides of the following components by weight: 30 to 70 parts of Bi, 5 to 15 parts of Si, 5 to 15 parts of Zn, 0 to 10 parts of B, 2 to 6 parts of Al, 0 to 2 parts of Ti, 0 to 2 parts of Y, 0 to 3 parts of Ca, 0 to 2.5 parts of Nd, and 0.2 to 2 parts of Na2CO3. It should be noted that the oxide of Bi here may include Bi2O3 and Bi2O5, the oxide of Si may include SiO2, the oxide of Zn may include ZnO, the oxide of B may include B2O3, the oxide of Al may include AL2O3, the oxide of Ti may include TiO and TiO2, the oxide of Y may include Y2O3, the oxide of Ca may include CaO, the oxide of Nd may include Nd2O3, etc., but is not limited thereto.
[0051] Exemplarily, the above-mentioned glass powder may include oxides of the following components in parts by mass: 30 parts of Bi, 5 parts of Si, 5 parts of Zn and 2 parts of Al, and 0.2 parts of Na2CO3; it may also include oxides of the following components: 50 parts of Bi, 10 parts of Si and 10 parts of Zn, 5 parts of B, 3 parts of Al, 1 part of Ti, 1 part of Y, 2 parts of Ca and 2 parts of Nd, and 1 part of Na2CO3; it may also be 70 parts of Bi, 15 parts of Si, 15 parts of Zn, 10 parts of B, 6 parts of Al, 2 parts of Ti, 2 parts of Y, 3 parts of Ca and 2.5 parts of Nd, and 2 parts of Na2CO3, etc., but is not limited to this.
[0052] In order to ensure that the chip capacitor prepared by the electrode silver paste has a good appearance, the fineness of the electrode silver paste needs to be limited to avoid excessive fineness, which makes the surface of the chip capacitor uneven. Therefore, the fineness of the above-mentioned electrode silver paste can be less than 7μm.
[0053] The exemplary embodiment of the present disclosure also provides a method for preparing the electrode silver paste based on the exemplary embodiment of the present disclosure. Figure 1 A flowchart of a method for preparing an electrode silver paste according to an exemplary embodiment of the present disclosure is shown. Figure 1 , the preparation method of electrode silver paste comprises:
[0054] Step 101: preparing glass powder under first reaction conditions. The first reaction conditions may include a reaction temperature of 1000° C. to 1500° C. and a reaction time of 1 h to 2 h.
[0055] For example, 30 to 70 parts of Bi oxide, 5 to 15 parts of Si oxide, 5 to 15 parts of Zn oxide, 0 to 10 parts of B oxide, 2 to 6 parts of Al oxide, 0 to 2 parts of Ti oxide, 0 to 2 parts of Y oxide, 0 to 3 parts of Ca oxide, 0 to 2.5 parts of Nd oxide and 0.2 to 2 parts of Na2CO3 can be mixed at a reaction temperature of 1000°C, melted for 1 hour and cooled, and then ground to D50 of 1 μm to 2 μm to obtain glass powder. Of course, the reaction temperature can also be 1200°C, 1500°C, etc., but is not limited thereto. The reaction time can also be 1.5h, 2h, etc., but is not limited thereto.
[0056] Step 102: Evenly mix the flaky silver powder, spherical silver powder and glass powder with a binder to obtain an electrode silver paste. It should be understood that the binder here is prepared by mixing an organic solvent, an additive and a polymer resin together using conventional process means. After evenly mixing the flaky silver powder, spherical silver powder and glass powder with the binder, masking is performed to obtain an electrode silver paste with a fineness that meets the requirements.
[0057] As a possible implementation, when the adhesive includes the above-mentioned polymer resin and organic solvent, the polymer resin and the organic solvent can be evenly mixed at 60°C to 70°C to obtain the adhesive. It should be noted that the reaction temperature here should be controlled within the range of the exemplary embodiment of the present disclosure to avoid excessively high temperature causing the organic solvent to volatilize, thereby increasing the viscosity of the adhesive, thereby increasing the viscosity of the electrode slurry, and the risk of poor appearance of the prepared chip capacitor.
[0058] Compared with the prior art, the beneficial effects of the method for preparing the electrode silver paste provided in the embodiment of the present disclosure are the same as the beneficial effects of the above-mentioned electrode silver paste, which will not be elaborated here.
[0059] The present disclosure is further described below by way of examples, but the present disclosure is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product instructions.
[0060] Example 1
[0061] The tap density of the flaky silver powder A used in this embodiment is 3.5 g / ml, the tap density of the flaky silver powder B is 5 g / ml, the particle size D50 of the spherical silver powder C is 0.1 μm, the tap density of the spherical silver powder C is 4.0 g / ml, the particle size D50 of the spherical silver powder D is 2 μm, and the tap density of the spherical silver powder D is 5 g / ml. The selected polymer resin is ethyl cellulose, the selected organic solvent is a mixed solvent of butyl carbitol and terpineol, the selected anti-settling thixotropic agent is polyamide wax, the selected dispersant is a phosphate dispersant, the selected leveling agent is polyether modified silicone, and the selected defoaming agent is modified polyalkoxy silicon.
[0062] Preparation of adhesive: 20 g of polymer resin is added to 200 g of organic solvent, and the mixture is stirred and dissolved in a water bath at 60° C. After stirring for 2 hours, the mixture is taken out, filtered while hot, and cooled to obtain the adhesive.
[0063] Preparation of glass powder: According to the mass proportions, take 50 parts of Bi2O3, 10 parts of SiO2, 10 parts of ZnO, 10 parts of B2O3, 4 parts of Al2O3, 1.5 parts of TiO2, 1 part of Y2O3, 2 parts of CaO, 1.5 parts of Nd2O3, and 1.5 parts of Na2CO3, mix and stir evenly, melt at 1200°C for 1 hour, cool, and grind using a ball mill until D50 is about 1.5μm.
[0064] Preparation of electrode silver paste: 15g of flaky silver powder A, 20g of flaky silver powder B, 10g of spherical silver powder C, 30g of spherical silver powder D, 5g of glass powder, 15g of adhesive, 3.75g of organic solvent, 0.3g of anti-settling thixotropic agent, 0.35g of dispersant, 0.3g of defoaming agent, and 0.3g of leveling agent are placed in plastic jars respectively, stirred evenly (centrifugal stirring or stirring with a mixer), and then placed on a three-roll grinder for grinding. After 5 to 7 rollings, the fineness is tested. If it is less than 7μm, it is considered that the dispersion is complete. After filtration, the electrode silver paste of the exemplary embodiment of the present disclosure is obtained. Its specific sintering properties are shown in Table 1.
[0065] Example 2
[0066] The tap density of the flaky silver powder A used in this embodiment is 3.7 g / ml, the tap density of the flaky silver powder B is 5.2 g / ml, the particle size D50 of the spherical silver powder C is 0.7 μm, the tap density of the spherical silver powder C is 4.7 g / ml, the particle size D50 of the spherical silver powder D is 2.7 μm, and the tap density of the spherical silver powder D is 5.2 g / ml. The selected polymer resin is polyvinyl butyral resin, the selected organic solvent is butyl carbitol acetate, the selected anti-settling thixotropic agent is hydrogenated castor oil, the selected dispersant is a modified polyether phosphate dispersant, the selected leveling agent is an acrylate compound, and the selected defoaming agent is an acrylate polymer.
[0067] Preparation of adhesive: 20 g of polymer resin was added to 200 g of organic solvent, and the mixture was dissolved by stirring in a water bath at 67° C. After stirring for 1.7 hours, the mixture was taken out, filtered while hot, and cooled to obtain the adhesive.
[0068] Preparation of glass powder: According to the mass proportions, take 30 parts of Bi2O3, 5 parts of SiO2, 5 parts of ZnO, 2 parts of Al2O3, and 0.2 parts of Na2CO3, mix and stir evenly, melt at 1200℃ for 1 hour, cool, and grind with a ball mill until D50 is about 1μm.
[0069] Preparation of electrode silver paste: take 5g of flaky silver powder A, 5g of flaky silver powder B, 35g of spherical silver powder C, 35g of spherical silver powder D, 1g of glass powder, 12g of adhesive, 3g of organic solvent, 1g of anti-settling thixotropic agent, 1g of dispersant, 1g of defoaming agent, and 1g of leveling agent, respectively, put them in plastic jars, stir evenly (centrifugal stirring or stirring with a mixer), and then grind them on a three-roll grinder. After 5 to 7 rollings, test the fineness. If it is less than 7μm, it is considered that the dispersion is complete. After filtration, the electrode silver paste of the exemplary embodiment of the present disclosure is obtained. Its specific sintering properties are shown in Table 1.
[0070] Example 3
[0071] The tap density of the flaky silver powder A used in this embodiment is 4.5 g / ml, the tap density of the flaky silver powder B is 6 g / ml, the particle size D50 of the spherical silver powder C is 1.5 μm, the tap density of the spherical silver powder C is 5 g / ml, the particle size D50 of the spherical silver powder D is 6 μm, and the tap density of the spherical silver powder D is 6 g / ml. The selected polymer resin is a mixture of acrylic resin and cellulose acetate butyrate, and the selected organic solvent is a mixed solvent of diethylene glycol methyl ether, diethylene glycol dimethyl ether and tripropylene glycol methyl ether.
[0072] Preparation of adhesive: 20 g of polymer resin is added to 200 g of organic solvent, and the mixture is stirred and dissolved in a 70° C. water bath. After stirring for 2.2 hours, the mixture is taken out, filtered while hot, and cooled to obtain the adhesive.
[0073] Preparation of glass powder: According to the mass proportions, take 70 parts of Bi2O3, 15 parts of SiO2, 15 parts of ZnO, 5 parts of B2O3, 6 parts of Al2O3, 2 parts of TiO2, 2 parts of Y2O3, 3 parts of CaO, 2.5 parts of Nd2O3, and 2 parts of Na2CO3, mix and stir evenly, melt at 1200°C for 1 hour, cool, and grind using a ball mill until D50 is about 2μm.
[0074] Preparation of electrode silver paste: Take 10g of flaky silver powder A, 50g of flaky silver powder B, 2g of spherical silver powder C, 8g of spherical silver powder D, 5g of glass powder, 21g of adhesive, and 4g of organic solvent, respectively place them in plastic jars, stir evenly (centrifugal stirring or stirring with a mixer), and then grind them on a three-roll grinder. After 5 to 7 rollings, test the fineness. If it is less than 7μm, it is considered that the dispersion is complete. After filtration, the electrode silver paste of the exemplary embodiment of the present disclosure is obtained. Its specific sintering performance is shown in Table 1.
[0075] Example 4
[0076] Different from Example 1, the polymer resin selected in this embodiment is rosin resin, the organic solvent selected is alcohol ester twelve, the anti-settling thixotropic agent selected is hydrogenated castor oil, the dispersant selected is a modified polyether phosphate dispersant, the leveling agent selected is an acrylate compound, and the defoaming agent selected is an acrylate polymer.
[0077] Preparation of glass powder: According to the mass proportions, take 60 parts of Bi2O3, 10 parts of SiO2, 10 parts of ZnO, 10 parts of B2O3, 4 parts of Al2O3, 1.5 parts of TiO2, 1 part of Y2O3, 2 parts of CaO, and 1.5 parts of Na2CO3, mix and stir evenly, melt at 1200°C for 1 hour, cool, and grind using a ball mill until D50 is about 1.5μm.
[0078] Preparation of electrode silver paste: 15g of flaky silver powder A, 20g of flaky silver powder B, 10g of spherical silver powder C, 30g of spherical silver powder D, 5g of glass powder, 15g of adhesive, 3.8g of organic solvent, 0.3g of anti-settling thixotropic agent, 0.3g of dispersant, 0.3g of defoaming agent, and 0.3g of leveling agent are placed in plastic jars respectively, stirred evenly (centrifugal stirring or stirring with a mixer), and then placed on a three-roll grinder for grinding. After 5 to 7 rollings, the fineness is tested. If it is less than 7μm, it is considered that the dispersion is complete. After filtration, the electrode silver paste of the exemplary embodiment of the present disclosure is obtained. Its specific sintering properties are shown in Table 1.
[0079] Example 5
[0080] Different from Example 1, the polymer resin selected in this embodiment is a mixture of ethyl cellulose and chloroacetic acid resin, the organic solvent selected is a mixed solvent of butyl carbitol and ethylene glycol hexyl ether, the anti-settling thixotropic agent selected is fumed silica, the dispersant selected is an acrylic ester dispersant, the leveling agent selected is a fluorocarbon modified polyacrylate compound, and the defoaming agent selected is a vinyl polymer.
[0081] Preparation of electrode silver paste: 15g of flaky silver powder A, 20g of flaky silver powder B, 10g of spherical silver powder C, 30g of spherical silver powder D, 5g of glass powder, 15g of adhesive, 3.8g of organic solvent, 0.3g of anti-settling thixotropic agent, 0.3g of dispersant, 0.3g of defoaming agent, and 0.3g of leveling agent are placed in plastic jars respectively, stirred evenly (centrifugal stirring or stirring with a mixer), and then placed on a three-roll grinder for grinding. After 5 to 7 rollings, the fineness is tested. If it is less than 7μm, it is considered that the dispersion is complete. After filtration, the electrode silver paste of the exemplary embodiment of the present disclosure is obtained. Its specific sintering properties are shown in Table 1.
[0082] Example 6
[0083] Different from Example 1, the ratio of the electrode silver paste prepared in this example is different.
[0084] Preparation of electrode silver paste: 10g of flaky silver powder A, 25g of flaky silver powder B, 15g of spherical silver powder C, 20g of spherical silver powder D, 5g of glass powder, 20g of adhesive, 3.8g of organic solvent, 0.3g of anti-settling thixotropic agent, 0.3g of dispersant, 0.3g of defoaming agent, and 0.3g of leveling agent are placed in plastic jars respectively, stirred evenly (centrifugal stirring or stirring with a mixer), and then placed on a three-roll grinder for grinding. After 5 to 7 rollings, the fineness is tested. If it is less than 7μm, the dispersion is considered to be complete. After filtration, the electrode silver paste of the exemplary embodiment of the present disclosure is obtained. Its specific sintering properties are shown in Table 1.
[0085] Example 7
[0086] Different from the fourth embodiment, the ratio of the glass powder in this embodiment is different.
[0087] Preparation of glass powder: According to the mass percentage, take 60 parts of Bi2O3, 10 parts of SiO2, 10 parts of ZnO, 10 parts of B2O3, 4 parts of Al2O3, 1 part of TiO2, 1.5 parts of Nd2O3, 2 parts of CaO, and 1.5 parts of Na2CO3, mix and stir evenly, melt at 1200°C for 1 hour, cool, and grind with a ball mill until D50 is about 1.5μm. The sintering properties of the electrode silver paste prepared in this embodiment are shown in Table 1.
[0088] Comparative Example
[0089] Different from Example 1, the ratio of glass powder and the ratio of electrode silver paste in this comparative example are different.
[0090] Preparation of glass powder: According to the mass proportions, take 44 parts of BaO, 8 parts of SiO2, 10 parts of ZnO, 3 parts of B2O3, 4 parts of Al2O3, 2 parts of TiO2 and 1 part of Na2CO3, mix and stir evenly, melt at 1200℃ for 1 hour, cool and grind with a ball mill until D50 is about 1.5μm.
[0091] Preparation of electrode silver paste: Take 20g of flaky silver powder B, 55g of spherical silver powder D, 5g of glass powder, 15g of adhesive, 3.75g of organic solvent, 0.3g of anti-settling thixotropic agent, 0.35g of dispersant, 0.3g of defoaming agent, and 0.3g of leveling agent, respectively, put them in plastic jars, stir evenly (centrifugal stirring or stirring with a mixer), and then grind them on a three-roll grinder. After 5 to 7 rollings, test the fineness. If it is less than 7μm, it is considered that the dispersion is complete. After filtration, the electrode silver paste of this comparative example is obtained. Its specific sintering properties are shown in Table 1.
[0092] Table 1 Electrode silver paste sintering performance table
[0093] Test No. Adhesion N Appearance after silver dipping Sintering density Example 1 33 good good Example 2 37 good good Example 3 40 good good Example 4 45 good good Example 5 32 good good Example 6 35 good good Example 7 42 good good Comparative Example 15 Poor, with a bulge in the middle Poor, with many holes in the cross section
[0094] It can be seen from the examples 1 to 7 and the comparative example that, since the exemplary embodiments 1 to 7 of the present disclosure all use the glass powder of the exemplary embodiments of the present disclosure, the adhesion of the electrode silver paste prepared by the method for preparing the exemplary electrode silver paste of the present disclosure is higher than that of the comparative example. Furthermore, since the exemplary embodiments 1 to 7 of the present disclosure all use the mixture of the four kinds of silver powder of the exemplary embodiments of the present disclosure, the appearance and sintering density of the electrode silver paste prepared by the method for preparing the exemplary electrode silver paste of the present disclosure after silver dipping are better than those of the comparative example.
[0095] It can be seen from the above that when the electrode silver paste of the exemplary embodiment of the present disclosure is used to prepare the chip capacitor, because it contains glass powder, the electrode silver paste can be tightly attached to the magnet of the chip capacitor, avoiding the separation of the end electrode layer and the magnet layer over time, which affects the performance of the chip capacitor. By adding 4 different silver powders, the gaps between the silver particles in the electrode silver paste are as small as possible, thereby improving the compactness of the electrode silver paste and the electrical properties of the prepared chip capacitor. Based on this, by using a polymer resin and an organic solvent that meet the exemplary ratio requirements of the present disclosure, the organic matter in the electrode silver paste can be evenly dispersed, ensuring the performance of the prepared chip capacitor, and at the same time adjusting the viscosity of the electrode silver paste, so that the prepared chip capacitor has a good surface appearance and good subsequent processing technology.
[0096] The embodiments of the present disclosure are described above. However, these embodiments are for illustrative purposes only and are not intended to limit the scope of the present disclosure. The scope of the present disclosure is defined by the appended claims and their equivalents. Without departing from the scope of the present disclosure, a person skilled in the art may make a variety of substitutions and modifications, which should all fall within the scope of the present disclosure.
Claims
1. An electrode silver paste, characterized in that: The electrode silver paste comprises: flaky silver powder, spherical silver powder, glass powder and adhesive, wherein: The flaky silver powder comprises flaky silver powder A and flaky silver powder B having different tap densities, and the mass ratio of the flaky silver powder A to the flaky silver powder B is (1:5) to (1:1); The spherical silver powder includes spherical silver powder C and spherical silver powder D with different particle sizes, and the mass ratio of the spherical silver powder C to the spherical silver powder D is (1:4) to (1:1); The mass ratio of the flaky silver powder, the spherical silver powder, the glass powder, the adhesive and the auxiliary agent is (10-60): (10-70): (1-10): (11-25): (0-4), and the auxiliary agent includes one or more of an anti-settling thixotropic agent, a dispersant, a leveling agent and a defoaming agent; The tap density of the flaky silver powder A is 3.5 g / ml~4.5 g / ml, the tap density of the flaky silver powder B is 5 g / ml~6 g / ml, the particle size D50 of the spherical silver powder C is 0.1 μm~1.5 μm, the tap density of the spherical silver powder C is 4.0 g / ml~5.0 g / ml, the particle size D50 of the spherical silver powder D is 2 μm~6 μm, and the tap density of the spherical silver powder D is 5 g / ml~6 g / ml; The particle size D50 of the glass powder is 1 μm~2 μm. The glass powder includes oxides of the following components in parts by mass: 30 parts~70 parts of Bi, 5 parts~15 parts of Si, 5 parts~15 parts of Zn, 0 parts~10 parts of B, 2 parts~6 parts of Al, 0 parts~2 parts of Ti, 0 parts~2 parts of Y, 0 parts~3 parts of Ca and 0 parts~2.5 parts of Nd and 0.2 parts~2 parts of Na2CO3.
2. The electrode silver paste according to claim 1, characterized in that: The adhesive comprises a polymer resin and an organic solvent, and the mass ratio of the polymer resin, the organic solvent and the flaky silver powder is (1-5): (10-20): (10-60).
3. The electrode silver paste according to claim 2, characterized in that: The polymer resin includes one or more of ethyl cellulose, polyvinyl butyral resin, acrylic resin, cellulose acetate butyrate, rosin resin, epoxy resin and chloroacetic acid resin; and / or, The organic solvent includes one or more of butyl carbitol, butyl carbitol acetate, alcohol ester dodecanol, terpineol, ethylene glycol hexyl ether, diethylene glycol methyl ether, diethylene glycol dimethyl ether and tripropylene glycol methyl ether.
4. The electrode silver paste according to claim 1, characterized in that: The anti-settling thixotropic agent includes one or more of polyamide wax, hydrogenated castor oil, carbomer and fumed silica; and / or, The dispersant includes one or more of a phosphate dispersant, a modified polyether phosphate dispersant and an acrylate dispersant; and / or, The leveling agent includes one or more of polyether-modified silicone, acrylate compound and fluorocarbon-modified polyacrylate compound; and / or, The defoaming agent includes one or more of modified polysiloxane, acrylic polymer and vinyl polymer.
5. The electrode silver paste according to claim 1, characterized in that: The mass ratio of the anti-settling thixotropic agent to the flaky silver powder is (0-1): (10-60); and / or, The mass ratio of the dispersant to the spherical silver powder is (0-1): (10-60); and / or, The mass ratio of the leveling agent to the spherical silver powder is (0-1): (10-60); and / or, The mass ratio of the defoaming agent to the spherical silver powder is (0-1): (10-60).
6. The electrode silver paste according to claim 1, characterized in that: The fineness of the electrode silver paste is less than 7 μm.
7. A method for preparing the electrode silver paste according to any one of claims 1 to 6, characterized in that: The method comprises: preparing glass powder under first reaction conditions; the first reaction conditions include a reaction temperature of 1000° C. to 1500° C. and a reaction time of 1 h to 2 h; The flaky silver powder, the spherical silver powder and the glass powder are uniformly mixed with a binder to obtain an electrode silver paste.
8. The method for preparing electrode silver paste according to claim 7, characterized in that: When the adhesive is the adhesive according to claim 2, the method comprises: The polymer resin and the organic solvent are uniformly mixed at 60°C to 70°C to obtain an adhesive.
9. A chip capacitor, characterized in that: It comprises a terminal electrode, and the terminal electrode is prepared by using the electrode silver paste described in any one of claims 1 to 6.