Lubricating oil with high cold resistance and good low-temperature fluidity and preparation method thereof
By using coal-derived oil and various additives to form a smaller crystal structure in lubricating oil, the problem of poor low-temperature fluidity of lubricating oil is solved, improving cold resistance and low-temperature fluidity, and extending the service life of the engine.
Patent Information
- Application Number
- CN202310404154.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Existing lubricating oils have poor fluidity at low temperatures, leading to a decline in performance. How can we improve the cold resistance and low-temperature fluidity of lubricating oils?
Coal-derived oil is used as the base oil, and detergents, dispersants, antioxidants, friction reducers, extreme pressure agents, viscosity index depressants, pour point depressants, and antifoaming agents are added. Through mixing and stirring, smaller crystal structures are formed, which improves the cold resistance and low-temperature fluidity of the lubricating oil.
This allows lubricating oil to flow more easily at low temperatures, reducing engine wear and extending engine life.
Smart Images

Figure BDA0004180690110000011 
Figure BDA0004180690110000021 
Figure BDA0004180690110000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lubricating oils, and in particular relates to a lubricating oil with high cold resistance and good low-temperature fluidity. Background Art
[0002] As the technology of the automotive industry continues to develop by leaps and bounds, automobile engines are also becoming more refined, and the viscosity and temperature requirements of the oil products are constantly decreasing. If the fluidity of the oil product deteriorates or even completely loses its fluidity, the performance of the oil product at low temperatures will drop sharply. In order to ensure good oil supply at low temperatures and make the lubrication system work normally, the lubricating oil should have good low-temperature fluidity.
[0003] In order to make the lubricating oil have the performance of low temperature resistance, a pour point depressant can be added to the ordinary lubricating oil base. The mechanism of action of the pour point depressant to make the lubricating oil have the performance of low temperature resistance is to form a eutectic with the base oil, change the size and shape of the paraffin crystal, and make it difficult to form a network structure, thereby playing a role in reducing the pour point of the oil. Although the addition of the pour point depressant can effectively reduce the pour point of the base oil, when the addition amount of the pour point depressant reaches a certain content, the pour point reduction effect is not obvious, and when the alkyl naphthalene and polymethacrylate type pour point depressants accumulate to a certain extent, it will cause the low temperature resistance of the lubricating oil to become worse. Therefore, how to improve the low temperature resistance of lubricating oil is a problem to be solved in this field. Summary of the invention
[0004] An object of the present invention is to provide a lubricating oil having high cold resistance and good low temperature fluidity, which comprises the following components in parts by weight:
[0005]
[0006]
[0007] In another preferred embodiment, the base oil is selected from coal-to-liquid, for example, Lu'an "coal-to-liquid" CTL4 and CTL6 base oils.
[0008] In another preferred embodiment, the detergent dispersant is selected from petroleum sulfonates, alkylphenol salts, salicylates, succinimides, succinates, or combinations thereof.
[0009] In another preferred embodiment, the antioxidant is selected from dialkyl dithiophosphates, antioxidant HBT, octyl zinc thiophosphate, or a combination thereof.
[0010] In another preferred embodiment, the friction reducing agent is selected from sulfided isobutylene, chlorinated paraffin, or a combination thereof.
[0011] In another preferred embodiment, the extreme pressure agent is selected from graphite, molybdenum disulfide, cubic boron nitride, tungsten disulfide, or a combination thereof.
[0012] In another preferred embodiment, the viscosity index agent is selected from polyisobutylene (e.g., Daelim PIB2400 of South Korea), ethylene propylene copolymer (e.g., Afton HITEC5748), polymethacrylate (e.g., Evonik 8-310), hydrogenated styrene diene copolymer (e.g., Infineum SV603), or a combination thereof.
[0013] In another preferred embodiment, the pour point depressant is selected from polyalkyl methacrylates, for example, Evonik VISCOPLEX 1-300 and / or Infineum V382.
[0014] In another preferred embodiment, the antifoaming agent is selected from dimethyl silicone oil, non-silicone antifoaming agent and composite antifoaming agent.
[0015] In another preferred embodiment, the non-silicon anti-foaming agent is selected from acrylic non-silicon anti-foaming agent or polyolefin anti-foaming agent.
[0016] In another preferred embodiment, the composite antifoaming agent is selected from a compound of an acrylic non-silicon antifoaming agent and a silicon-containing antifoaming agent, and more preferably, the ratio of the two is 1:0.1-9.
[0017] Another aspect of the present invention provides a method for preparing the lubricating oil having high cold resistance and good low-temperature fluidity, which comprises the following steps:
[0018] S1: Add base oil, detergent dispersant, antioxidant, friction reducer, extreme pressure agent and viscosity modifier into a container and slowly raise the temperature to 45-55°C;
[0019] S2: stirring the liquid in the container for 2 to 3 hours, and simultaneously adding a pour point depressant and an antifoaming agent;
[0020] S3: Cooling to room temperature and continuing to stir the liquid in the container for 2 to 3 hours to obtain lubricating oil.
[0021] Compared with the prior art, the beneficial effect of the present invention is that the lubricating oil of the present invention is mixed with a detergent dispersant, an antioxidant, a wear reducer, an extreme pressure agent, a viscosity index agent, a pour point depressant and an anti-foaming agent through the "coal-to-oil" product of the industrialization of the independent technology of indirect liquefaction of coal as a base oil to obtain a lubricating oil with high cold resistance and good low-temperature fluidity. DETAILED DESCRIPTION
[0022] In view of the shortcomings of the existing lubricating oils, which have insufficient cold resistance and low-temperature fluidity, the inventors of the present application have found through in-depth research that the lubricating oil obtained by mixing the base oil with a detergent dispersant, an antioxidant, a friction reducer, an extreme pressure agent, a viscosity modifier, a pour point depressant, and an antifoaming agent has good cold resistance and low-temperature fluidity. The reason may be that these added components can be adsorbed onto the surface of the metal film and promote different crystal forms, which will bring more and smaller three-dimensional needle-shaped or cubic crystals. These smaller crystals can keep the protective film suspended for a longer time, and the distribution of particles is more uniform, which can make the engine easier to start, reduce engine wear, and extend the engine life.
[0023] In the description of the present invention, "room temperature" refers to 4-40°C, more preferably, 25±5°C.
[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with specific embodiments.
[0025] In the following examples, all components used are commercially available unless otherwise specified.
[0026] Example 1
[0027] 1.1 The lubricating oil with high cold resistance and good low temperature fluidity is composed of the following components in parts by weight:
[0028]
[0029]
[0030] 1.2 The preparation steps of lubricating oil are as follows:
[0031] S1: Add the mixed liquid of Lu'an coal-to-liquid CTL4 and CTL6, petroleum sulfonate, dialkyl dithiophosphate, sulfided isobutylene, graphite, and Dalin PIB2400 of South Korea in a volume ratio of 1:1 into a container, and slowly raise the temperature to 45-55°C;
[0032] S2: Stir the liquid in the container for 2 to 3 hours using a stirring device, and simultaneously add Evonik VISCOPLEX 1-300 and dimethyl silicone oil;
[0033] S3: Cooling to room temperature, and continuing to stir the liquid in the container for 2 to 3 hours using a stirring device to obtain lubricating oil.
[0034] Embodiment 2:
[0035] 2.1 Lubricating oil with high cold resistance and good low temperature fluidity is composed of the following components by weight:
[0036]
[0037] 2.2 The preparation steps of the above lubricating oil are as follows:
[0038] S1: Add the mixed solution of Lu'an coal-to-liquid CTL4 and CTL6, petroleum sulfonate, dialkyl dithiophosphate, sulfided isobutylene, graphite and polyisobutylene in a volume ratio of 1:1 into a container according to the above weight parts, and slowly raise the temperature to 45-55°C;
[0039] S2: stirring the liquid in the container for 2 to 3 hours by a stirring device, and simultaneously adding the pour point depressant T801 of alkyl naphthalene compounds and dimethyl silicone oil;
[0040] S3: Cooling to room temperature, and continuing to stir the liquid in the container for 2 to 3 hours using a stirring device to obtain lubricating oil.
[0041] Example 3
[0042] 3.1 The lubricating oil with high cold resistance and good low temperature fluidity is composed of the following components in parts by weight:
[0043]
[0044] 3.2 The preparation steps of the above lubricating oil are as follows:
[0045] S1: Add 88 parts of a mixture of Lu'an coal-to-liquid CTL4 and CTL6 in a volume ratio of 1:2, 1 part of alkylphenol, 0.85 parts of dialkyl dithiophosphate, 1.05 parts of chlorinated paraffin, 0.96 parts of molybdenum disulfide, and 5.8 parts of ethylene propylene copolymer into a container, and slowly raise the temperature to 45-55°C;
[0046] S2: stirring the liquid in the container for 2 to 3 hours by a stirring device, and simultaneously adding 1.2 parts of a pour point depressant of polymethacrylate (PMA) 1-248 and a non-silicon antifoaming agent;
[0047] S3: Cooling to room temperature, and continuing to stir the liquid in the container for 2 to 3 hours using a stirring device to obtain lubricating oil.
[0048] Example 4
[0049] 4.1 The lubricating oil with high cold resistance and good low temperature fluidity is composed of the following components in parts by weight:
[0050]
[0051]
[0052] 4.2 The specific steps for preparing lubricating oil are as follows:
[0053] S1: 89 parts of a mixture of Lu'an coal-to-liquid CTL4 and CTL6 in a volume ratio of 2:1, 0.86 parts of salicylate, 0.85 parts of dialkyl dithiophosphate, 1.2 parts of chlorinated paraffin, 0.68 parts of cubic boron nitride, and 5.6 parts of ethylene propylene copolymer are added into a container, and the temperature is slowly raised to 45-55°C;
[0054] S2: stirring the liquid in the container for 2 to 3 hours by means of a stirring device, and simultaneously adding a polyolefin compound pour point depressant T803A and a polyolefin antifoaming agent;
[0055] S3: Cooling to room temperature, and continuing to stir the liquid in the container for 2 to 3 hours using a stirring device to obtain lubricating oil.
[0056] Example 5
[0057] 5.1 Cold resistance performance High and low temperature fluidity lubricating oil is composed of the following components in parts by weight:
[0058]
[0059] 5.2 The specific steps for preparing lubricating oil are as follows:
[0060] S1: Add a mixed solution of Lu'an coal-to-liquid CTL4 and CTL6 in a volume ratio of 2:1, salicylate, dialkyl dithiophosphate, chlorinated paraffin, cubic boron nitride, and ethylene propylene copolymer into a container, and slowly raise the temperature to 45-55°C;
[0061] S2: stirring the liquid in the container for 2 to 3 hours by means of a stirring device, and simultaneously adding a pour point depressant of a polyolefin compound and a non-silicon antifoaming agent;
[0062] S3: Cooling to room temperature, and continuing to stir the liquid in the container for 2 to 3 hours using a stirring device to obtain lubricating oil.
[0063] Embodiment 6:
[0064] 6.1 Lubricating oil with high cold resistance and good low temperature fluidity is composed of the following components in parts by weight:
[0065]
[0066] 6.2 The specific steps for preparing lubricating oil are as follows:
[0067] S1: Add 5.5 parts of a mixture of Lu'an coal-to-liquid CTL4 and CTL6 in a volume ratio of 1:1, succinate and polymer, dialkyl dithiophosphate, chlorinated paraffin, tungsten disulfide, and hydrogenated styrene diene copolymer into a container, and slowly raise the temperature to 45-55°C;
[0068] S2: stirring the liquid in the container for 2 to 3 hours by means of a stirring device, and simultaneously adding a pour point depressant T803A of a poly-alpha-olefin compound and a composite antifoaming agent;
[0069] S3: Cooling to room temperature, and continuing to stir the liquid in the container for 2 to 3 hours using a stirring device to obtain lubricating oil.
[0070] Comparative Examples 1, 2 and 3
[0071] The coal-based base oils used in Examples 1, 2 and 3 were replaced with commercially available paraffin-based base oils (e.g., 150N and 100N from Formosa Plastics), respectively, while other components and amounts remained unchanged, to prepare lubricating oils.
[0072] Comparative Examples 4, 5 and 6
[0073] The coal-based base oils used in Examples 4, 5 and 6 were replaced with commercially available hydrogenated base oils (eg, South Korea's Ssangyong Aramco ULTRA 4 and Aramco ULTRA 6), respectively, while other components and amounts remained unchanged, to prepare lubricating oils.
[0074] The CCS@-35 low temperature apparent viscosity and pour point / °C of the lubricating oils of Examples 1 to 6 were tested using the ASTM D5293 test method and the ASTM D97 test method, respectively. The results are shown in Table 1.
[0075] The CCS@-35 low temperature apparent viscosity and pour point / °C of the lubricating oils of Comparative Examples 1 to 6 were tested using the ASTM D5293 test method and the ASTM D97 test method, respectively. The results are shown in Table 2.
[0076] The CCS@-35 low temperature apparent viscosity and pour point / °C of commercially available lubricating oils were tested using the ASTM D5293 test method and the ASTM D97 test method, respectively. The results are shown in Table 3.
[0077] Table 1
[0078]
[0079] Table 2
[0080]
[0081] Table 3
[0082]
[0083] Comparison of the data in Table 1 and Table 2 shows that the use of coal-based base oil has better low temperature performance than normal mineral paraffin base oil or hydrotreated base oil.
[0084] Comparison of the data in Table 1 and Table 3 shows that the lubricating oil of the present invention has better cold resistance than commercially available lubricating oils and has better lubrication effect at low temperatures.
[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a lubricating oil having high cold resistance and good low-temperature fluidity, It is characterized in that The lubricating oil comprises the following components in parts by weight: 85-90 parts of base oil, 0.5 to 1 part of detergent and dispersant, 0.7-2 parts of antioxidant, 0.4-1.2 parts of antifriction agent, 0.3 to 1 part of extreme pressure agent, 2 to 6 parts of adhesive finger agent, Pour point depressant 0.8-1.6 parts, 0.8-1.6 parts of antifoaming agent; The preparation method comprises the following steps: S1: Add base oil, detergent dispersant, antioxidant, antifriction agent, extreme pressure agent and viscosity modifier into a container and slowly raise the temperature to 45~55℃; S2: Stir the liquid in the container for 2-3 hours, and simultaneously add the pour point depressant and antifoaming agent; S3: cooling to room temperature and continuing to stir the liquid in the container for 2 to 3 hours to obtain the lubricating oil with high cold resistance and good low-temperature fluidity; The base oil is selected from coal-to-liquids; The detergent dispersant is selected from petroleum sulfonates, alkylphenols, salicylates, succinimides, succinates, or combinations thereof; The antioxidant is selected from dialkyl dithiophosphates; The friction reducing agent is selected from sulfided isobutylene, chlorinated paraffin, or a combination thereof; The extreme pressure agent is selected from graphite, molybdenum disulfide, cubic boron nitride, tungsten disulfide, or a combination thereof; The viscosity modifier is selected from polyisobutylene, ethylene propylene copolymer, polymethacrylate, hydrogenated styrene diene copolymer, or a combination thereof; The pour point depressant is selected from polyalkyl methacrylate; The antifoaming agent is selected from dimethyl silicone oil, non-silicone antifoaming agent and composite antifoaming agent, The non-silicon antifoaming agent is selected from acrylic non-silicon antifoaming agent, polyolefin antifoaming agent, and / or The composite antifoaming agent is selected from a compound of an acrylic non-silicon antifoaming agent and a silicon-containing antifoaming agent.