Polylactic acid-based composite material and preparation method and application thereof
Through the design of polylactic acid-based composite materials, combined with polyadipate/butylene terephthalate and filler, the problem of difficult degradation and insufficient resilience of existing nose bridge strip materials is solved, and an environmentally friendly and aging-resistant nose bridge is achieved Strip material, suitable for disposable masks.
Patent Information
- Application Number
- CN202310465813.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-26
AI Technical Summary
The existing mask nose bridge materials are mainly polyolefin resins, which are difficult to degrade, resulting in environmental pollution, lack of resilience and aging resistance.
The polylactic acid-based composite materials, including polylactic acid, polyadipic acid/butylene terephthalate and fillers, are prepared through esterification reaction to control the content and intrinsic viscosity of the polybutylene terephthalate segment. Combined with lubricants, a biodegradable nose bridge strip material is formed.
It achieves excellent resilience, degradability and aging resistance of the material, meets the use standards of disposable mask nose bridge strips, and is suitable for large-scale production through simple and environmentally friendly processes.
Smart Images

Figure CN116554660B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer composite materials, and in particular to a polylactic acid-based composite material and a preparation method and application thereof. Background Art
[0002] The nose bridge strip, also known as the nose bridge muscle or nose bridge line, is a thin rubber strip inside the mask. It fixes the mask on the bridge of the nose and makes the mask fit well with the bridge of the nose and the skin on both sides, thereby reducing the leakage of pollutants from the gaps on both sides of the nose bridge when wearing the mask.
[0003] At present, the nose bridge of masks is mainly made of polyolefin resin. Like metal wire, it has the excellent performance of bending and deforming with external force, not rebounding when the external force is removed, and maintaining the existing shape unchanged, playing the role of fixing the mask on the nose bridge. Although polyolefin resin is cheap, it is difficult to degrade and is very easy to cause environmental pollution, which is not in line with the concept of green environmental protection development. It is of great significance to develop a nose bridge with good resilience and good degradation performance. Summary of the invention
[0004] Based on this, the present invention provides a polylactic acid-based composite material with good resilience, aging resistance and biodegradability, which can be used to prepare a nose bridge strip.
[0005] The technical solution is as follows:
[0006] A biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0007] 15-55 parts of polylactic acid;
[0008] 30-70 parts of polybutylene adipate / terephthalate; and
[0009] 15-40 parts of filler;
[0010] In the polylactic acid, the mass content of residual monomers is ≤0.3%;
[0011] The polybutylene adipate / terephthalate has a structure shown in formula (I):
[0012]
[0013] p is 0.44 to 0.54, p+q=1;
[0014] At 25° C., the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g.
[0015] In one embodiment, the biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0016] 15-45 parts of polylactic acid;
[0017] 40-60 parts of polybutylene adipate / terephthalate; and
[0018] 15 to 35 parts of filler.
[0019] In one of the embodiments, the mass content of the poly(butylene adipate / terephthalate) in the biodegradable poly(lactic acid)-based composite material is ≥ 20%.
[0020] In one embodiment, the D50 particle size of the filler is ≤10 μm.
[0021] In one embodiment, the filler is talc and calcium carbonate or a mixture of both.
[0022] In one of the embodiments, the biodegradable polylactic acid-based composite material further comprises 0.1 to 2 parts of lubricant by weight.
[0023] The present invention also provides a method for preparing the biodegradable polylactic acid-based composite material as described above, comprising the following steps:
[0024] The polylactic acid, polybutylene adipate / terephthalate and filler are blended and extruded.
[0025] In one embodiment, the extrusion temperature is 130°C to 220°C.
[0026] In one embodiment, the preparation method of polybutylene adipate / terephthalate comprises the following steps:
[0027] Terephthalic acid, 1,4-butanediol and a catalyst are mixed to prepare an esterified product A1 through an esterification reaction, wherein the molar ratio of terephthalic acid to 1,4-butanediol is (1.1-2.5):1;
[0028] Adipic acid and 1,4-butanediol are mixed in a molar ratio of (1 to 1.8):1, and an esterification reaction is performed to prepare an esterified product A2;
[0029] The esterified product A1 and the esterified product A2 are mixed and reacted at a temperature of 200° C. to 245° C. and a pressure of 1 KPa to 10 KPa for 0.5 h to 5 h to prepare a prepolymer;
[0030] The prepolymer is reacted for 1 h to 5 h at a temperature of 230° C. to 255° C. and a pressure of ≤150 Pa to prepare the polybutylene adipate / terephthalate.
[0031] In one embodiment, the process parameters for preparing the esterification product A1 include:
[0032] The temperature is 200℃~250℃, the pressure is 30KPa~110KPa, and the time is 1.5h~3.5h.
[0033] In one embodiment, the process parameters for preparing the esterification product A2 include:
[0034] The temperature is 100℃~250℃, the pressure is 30KPa~110KPa, and the time is 2h~4h.
[0035] The present invention also provides a nose bridge strip, comprising the biodegradable polylactic acid-based composite material as described above, or the biodegradable polylactic acid-based composite material prepared according to the preparation method as described above.
[0036] The present invention also provides a mask comprising the nose bridge strip as described above.
[0037] The present invention has the following beneficial effects:
[0038] The biodegradable polylactic acid-based composite material of the present invention comprises specific polylactic acid, filler and specific poly(butylene adipate / terephthalate). The inventor has found through research that the content of poly(butylene terephthalate) segments in poly(butylene adipate / terephthalate) will affect the degradation performance and resilience of the composite material. The higher the content of poly(butylene terephthalate), the better the resilience and shaping effect; and the characteristic viscosity of poly(butylene adipate / terephthalate) will also affect the degradation performance of the composite material. The higher the characteristic viscosity, the worse the degradation performance of the composite material, the better the resilience and shaping effect, especially the aging shaping effect; and the higher the residual monomer content in the polylactic acid, the worse the aging shaping effect of the composite material. The present invention controls the molar fraction of the polybutylene terephthalate segment in the polybutylene adipate / terephthalate to be 0.44-0.54, and the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g-1.9 dL / g, the mass content of the residual monomer in the polylactic acid is ≤0.3%, and a filler is used in combination to prepare a biodegradable polylactic acid-based composite material with excellent resilience, degradability and aging resistance, and the biodegradable polylactic acid-based composite material can be applied to nose bridge strips and masks.
[0039] After testing, the melt flow rate (melt index) of the biodegradable polylactic acid-based composite material is 2g / 10min-15g / 10min, and the bending modulus is greater than 1000MPa. The above biodegradable polylactic acid-based composite material is used to prepare a nose bridge strip, and the prepared nose bridge strip has a rebound angle of less than 10° when folded at 180°, and rebound of less than 15° when folded at 90°. After aging, the rebound angle of less than 15° when folded at 180°, and rebound of less than 20° when folded at 90°, meeting the standard of "Plastic Nose Bridge Strip for Disposable Masks".
[0040] In addition, the preparation method of the biodegradable polylactic acid-based composite material of the present invention has simple process, is environmentally friendly and safe, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a hydrogen nuclear magnetic resonance spectrum of PBAT prepared in a synthesis example of the present invention. DETAILED DESCRIPTION
[0042] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0044] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0045] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.
[0046] In the present invention, when it comes to the unit of the data range, if there is a unit only after the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 150-160°C means that the units of the left endpoint "150" and the right endpoint "160" are both ℃ (Celsius).
[0047] In the present invention, in the description of the invention, the meaning of "several" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0048] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.
[0049] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0050] It should be noted that, in the description of the present invention, directional words such as the terms "center", "lateral", "longitudinal", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc., indicating directions and positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of narrating the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and cannot be understood as limiting the specific protection scope of the present invention.
[0051] Where “including,” “having,” and “comprising” are used herein, it is intended to cover a non-exclusive inclusion, and another component may also be added unless explicit limiting terms such as “only,” “consisting of,” etc. are used.
[0052] Unless mentioned to the contrary, terms in the singular may include plural forms and should not be construed as being one in number.
[0053] In the present invention, the ratio of polybutylene terephthalate in polybutylene adipate / terephthalate can be obtained by measuring the hydrogen nuclear magnetic resonance spectrum of polybutylene adipate / terephthalate and calculating the peak area of the corresponding peak.
[0054] In the present invention, the intrinsic viscosity is determined according to DIN 53728, Part 3, January 3, 1985, and the solvent used includes a mixture of phenol and dichlorobenzene in a weight ratio of 50:50; the test temperature is 25°C.
[0055] The residual monomer content of polylactic acid in the present invention is tested as follows:
[0056] 1. Prepare standard solution
[0057] (1) Weigh 100±10 mg of pentamethylbenzene and mix it with 100 mL of dichloromethane solution. Shake well. This is called the internal standard solution.
[0058] (2) Weigh 100 ± 10 mg of L-lactide standard, prepare 100 mL of dichloromethane solution, shake well, and record it as the standard solution;
[0059] (3) Take 1.0, 2.0, 5.0, 10.0, and 20.0 mL of the standard solution and place them in 25 mL volumetric flasks. Add 4.0 mL of the internal standard solution to each flask, fill it up with n-hexane, and shake at a constant temperature. This is called the calibration standard solution.
[0060] 2. Sample testing
[0061] (1) Weigh 200±20 mg of polylactic acid sample (W) in a 20 ml glass vial, add 4.0 ml of internal standard solution, and dissolve the sample at room temperature. Stirring can be used to assist dissolution. After the sample is completely dissolved, slowly add 10 ml of n-hexane to the inner wall of the flask, stopper the vial, and then shake it vigorously for 5 to 10 seconds. Let the sample stand for 10 minutes;
[0062] (2) After filtering with a membrane filter, transfer to a dedicated injection vial for gas chromatography and perform the test according to the above-mentioned gas chromatography analysis conditions. Each sample solution should be injected at least 3 times.
[0063] 3. Calculation of residual monomer content of polylactic acid
[0064] Calculate the area ratio AR of lactide and pentamethylbenzene in the injected sample S and read the corresponding content ratio CR from the calibration curve S .
[0065] The lactide content of the sample during each GC run was calculated as follows:
[0066]
[0067] CR S : The content ratio read in the calibration curve;
[0068] IS S : The mass of pentamethylbenzene in 100mL of internal standard solution for sample determination [mg / 100mL];
[0069] W: weight of PLA sample weighed [mg].
[0070] In the present invention, the median particle size D50 test method is determined by referring to the GB / T 19077-2016 "Particle size distribution laser diffraction method".
[0071] The invention adopts a specific resin polymer formula to provide a polylactic acid-based composite material with good resilience, aging resistance and biodegradability, which can be used for nose bridge strips.
[0072] The technical solution is as follows:
[0073] A biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0074] 15-55 parts of polylactic acid;
[0075] 30-70 parts of polybutylene adipate / terephthalate; and
[0076] 15-40 parts of filler;
[0077] The polybutylene adipate / terephthalate has a structure shown in formula (I):
[0078]
[0079] p is 0.44 to 0.54, p+q=1;
[0080] The intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g.
[0081] The inventors have found through research that the content of polybutylene terephthalate segments in polybutylene adipate / terephthalate will affect the degradation performance and strength of the composite material. The higher the polybutylene terephthalate content, the better the resilience and shaping effects; and the intrinsic viscosity of polybutylene adipate / terephthalate will also affect the degradation performance of the composite material. The higher the intrinsic viscosity, the worse the degradation performance of the composite material, the better the resilience and shaping effects, especially the aging shaping effect; and the higher the residual monomer content in polylactic acid, the worse the aging shaping effect of the composite material. The present invention controls the molar fraction of the polybutylene terephthalate segment in the polybutylene adipate / terephthalate to be 0.44-0.54, and the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9dL / g-1.9dL / g, the mass content of the residual monomer in the polylactic acid is ≤0.3%, and a filler is used in combination to prepare a biodegradable polylactic acid-based composite material with excellent resilience, degradability and aging resistance.
[0082] It can be understood that in the present invention, in the polybutylene adipate / terephthalate, the mole fraction of the polybutylene terephthalate segment is 0.44 to 0.54, including but not limited to 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53 and 0.54.
[0083] It can be understood that in the present invention, the intrinsic viscosity of the polyadipate / butylene terephthalate is 0.9dL / g to 1.9dL / g, including but not limited to 0.9dL / g, 1.0dL / g, 1.1dL / g, 1.2dL / g, 1.3dL / g, 1.4dL / g, 1.5dL / g, 1.6dL / g, 1.7dL / g, 1.8dL / g and 1.9dL / g. Preferably, the intrinsic viscosity of the polyadipate / butylene terephthalate is 1dL / g to 1.9dL / g. Further, the intrinsic viscosity of the polyadipate / butylene terephthalate is 1.1dL / g to 1.6dL / g.
[0084] It can be understood that in the present invention, the biodegradable polylactic acid-based composite material contains 30 to 70 parts of poly(butylene adipate) / terephthalate in parts by weight, including but not limited to 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts and 70 parts, preferably 40 to 60 parts.
[0085] In one embodiment, the mass content of the poly(butylene adipate / terephthalate) in the biodegradable poly(lactic acid)-based composite material is ≥ 20%, including but not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70% and 75%. Further, the mass content of the poly(butylene adipate / terephthalate) in the biodegradable poly(lactic acid)-based composite material is 25% to 65%.
[0086] It is understood that the mass content of residual monomers in the polylactic acid is ≤0.3%, so that the composite material can have excellent degradability, resilience and aging setting effects. It is understood that the mass content of residual monomers in the polylactic acid includes but is not limited to 0, 0.1%, 0.2% and 0.3%.
[0087] It can be understood that in the present invention, the biodegradable polylactic acid-based composite material contains 15 to 55 parts of polylactic acid (PLA) by weight, including but not limited to 15, 20, 25, 30, 35, 40, 45, 50 and 55 parts, preferably 15 to 55 parts.
[0088] It can be understood that in the present invention, the biodegradable polylactic acid-based composite material contains 15 to 40 parts of filler by weight, including but not limited to 15, 20, 25, 30, 35 and 40 parts, preferably 15 to 35 parts.
[0089] The inventors have found that the larger the D50 particle size of the filler, the worse the aging setting effect of the composite material. In one embodiment, the D50 particle size of the filler is ≤10μm, so that the composite material can have excellent degradability, resilience and aging setting effects. It can be understood that the D50 particle size of the filler includes but is not limited to 0.1μm, 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm and 10μm. Preferably, the D50 particle size of the filler is ≤5μm.
[0090] In one embodiment, the filler is talcum powder and / or calcium carbonate. Preferably, the filler is talcum powder.
[0091] In one embodiment, the biodegradable polylactic acid-based composite material further comprises a lubricant.
[0092] In one embodiment, the lubricant is selected from one or a mixture of stearamide, oleamide, erucamide, zinc stearate, high molecular weight complex ester of metal soap, ethylene bisstearamide, polyethylene wax and silicone lubricants.
[0093] In one embodiment, the biodegradable polylactic acid-based composite material also includes 0.1 to 2 parts of lubricant, by weight, including but not limited to 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 and 2 parts, preferably 0.1 to 1 part.
[0094] In one embodiment, the biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0095]
[0096] In one embodiment, the biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0097]
[0098] The present invention also provides a method for preparing the biodegradable polylactic acid-based composite material as described above, comprising the following steps:
[0099] The polylactic acid, polybutylene adipate / terephthalate and filler are blended and extruded.
[0100] In one embodiment, the extrusion temperature is 130° C. to 220° C. In one embodiment, after extrusion, the extruded product is cooled, shaped and granulated.
[0101] In one embodiment, the preparation method of polybutylene adipate / terephthalate comprises the following steps:
[0102] Terephthalic acid, 1,4-butanediol and a catalyst are mixed to prepare an esterified product A1 through an esterification reaction; wherein, preferably, the molar ratio of terephthalic acid to 1,4-butanediol is (1.1-2.5):1; the catalyst is 0.3%-2.65% of the total mass of the raw materials, and the catalyst is one or a mixture of zinc-based, tin-based and titanium-based catalysts;
[0103] Adipic acid and 1,4-butanediol are mixed in a molar ratio of (1 to 1.8):1, and an esterification reaction is performed to prepare an esterified product A2;
[0104] The esterified product A1 and the esterified product A2 are mixed and reacted at a temperature of 200° C. to 245° C. and a pressure of 1 KPa to 10 KPa for 0.5 h to 5 h (prepolymerization stage) to prepare a prepolymer;
[0105] The prepolymer is allowed to continue to react (post-polymerization stage) for 1.0 h to 5 h at a temperature of 230° C. to 255° C. and a pressure of ≤150 Pa to prepare the polybutylene adipate / terephthalate.
[0106] The content of the polybutylene terephthalate segment in the PBAT and the intrinsic viscosity of the PBAT are controlled by adjusting the ratio of the raw materials and the reaction time of the polymerization process, so that in the PBAT having the structure represented by formula (I), the molar fraction of the polybutylene terephthalate segment is 0.44 to 0.54, and at 25° C., the intrinsic viscosity of the PBAT is 0.9 dL / g to 1.9 dL / g.
[0107] In one embodiment, the process parameters for preparing the esterification product A1 include:
[0108] The temperature is 200℃~250℃, the pressure is 30KPa~110KPa, and the time is 1.5h~3.5h.
[0109] In one embodiment, the process parameters for preparing the esterification product A2 include:
[0110] The temperature is 100℃~250℃, the pressure is 30KPa~110KPa, and the time is 2h~4h.
[0111] The present invention also provides a nose bridge strip, comprising the biodegradable polylactic acid-based composite material as described above, or the biodegradable polylactic acid-based composite material prepared according to the preparation method as described above.
[0112] The present invention also provides a mask comprising the nose bridge strip as described above.
[0113] The following is a specific embodiment:
[0114] (1) Raw materials description:
[0115] ① Polylactic acid:
[0116] PLA-1, purchased from Nature Works, residual monomer content 0.1%;
[0117] PLA-2, purchased from Nature Works, residual monomer content 0.3%;
[0118] PLA-3, purchased from Nature Works, with a residual monomer content of 0.5% by mass.
[0119] ②Packing:
[0120] Talc-1, commercially available, D50 particle size 5 μm;
[0121] Talc-2, commercially available, D50 particle size 10 μm;
[0122] Calcium carbonate, commercially available, D50 particle size is 8 μm.
[0123] ③Lubricant: ethylene bisstearamide.
[0124] (2) Synthesis example:
[0125] Synthesis example 1:
[0126] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0127] 1) adding terephthalic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.1:1, and adding a catalyst of n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0128] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.6:1, and reacting for 2.5 hours at a temperature of 200° C. and a pressure of 40 KPa to obtain an esterified product A2;
[0129] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, and then polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable polybutylene adipate / terephthalate PBAT-1.
[0130] Synthesis example 2:
[0131] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0132] 1) adding terephthalic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.1:1, and adding a catalyst of n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0133] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.5:1, and reacting for 2.5 hours at a temperature of 200° C. and a pressure of 40 KPa to obtain an esterified product A2;
[0134] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 200° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, and then polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable polybutylene adipate / terephthalate PBAT-2.
[0135] Synthesis example 3:
[0136] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0137] 1) adding terephthalic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.1:1, and adding a catalyst of n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0138] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.3:1, and reacting for 2.5 hours at a temperature of 200° C. and a pressure of 40 KPa to obtain an esterified product A2;
[0139] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, and then polymerized at a temperature of 200° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable polybutylene adipate / terephthalate PBAT-3.
[0140] Synthesis example 4:
[0141] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0142] 1) adding terephthalic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.1:1, and adding a catalyst of n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0143] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.0:1, and reacting for 2.5 hours at a temperature of 200° C. and a pressure of 40 KPa to obtain an esterified product A2;
[0144] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, and then polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain a biodegradable polybutylene adipate / terephthalate PBAT-4.
[0145] Synthesis example 5:
[0146] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0147] 1) adding terephthalic acid and 1,4-butanediol in a molar ratio of 1.5:1 into an esterification reaction kettle, and adding a catalyst n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0148] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.67:1, and reacting at a temperature of 200° C. and a pressure of 40 KPa for 2.5 h to obtain an esterified product A2;
[0149] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, and then polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable polybutylene adipate / terephthalate PBAT-5.
[0150] Synthesis example 6:
[0151] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0152] 1) adding terephthalic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.1:1, and adding a catalyst of n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0153] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.3:1, and reacting for 2.5 hours at a temperature of 200° C. and a pressure of 40 KPa to obtain an esterified product A2;
[0154] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 h to obtain a prepolymer, and then polymerized at a temperature of 240° C. and a pressure of 120 Pa for 0.5 h to obtain biodegradable polybutylene adipate / terephthalate PBAT-6.
[0155] Synthesis example 7:
[0156] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0157] 1) adding terephthalic acid and 1,4-butanediol in a molar ratio of 1:1 into an esterification reaction kettle, and adding a catalyst of n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0158] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.3:1, and reacting for 2.5 hours at a temperature of 200° C. and a pressure of 40 KPa to obtain an esterified product A2;
[0159] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, and then polymerized at a temperature of 240° C. and a pressure of 120 Pa for 5 hours to obtain biodegradable polybutylene adipate / terephthalate PBAT-7.
[0160] Synthesis example 8:
[0161] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0162] 1) adding terephthalic acid and 1,4-butanediol in a molar ratio of 1:1 into an esterification reaction kettle, and adding a catalyst of n-butyl titanate accounting for 1% of the total mass of the raw materials, and reacting for 2.5 hours at a temperature of 240° C. and a pressure of 40 KPa to obtain an esterified product A1;
[0163] 2) adding adipic acid and 1,4-butanediol into an esterification reaction kettle at a molar ratio of 1.3:1, and reacting for 2.5 hours at a temperature of 200° C. and a pressure of 40 KPa to obtain an esterified product A2;
[0164] 3) The two esters A1 and A2 are continuously fed into a mixer for mixing, reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, and then polymerized at a temperature of 240° C. and a pressure of 120 Pa for 6 hours to obtain biodegradable polybutylene adipate / terephthalate PBAT-8.
[0165] 1. By testing the hydrogen nuclear magnetic resonance spectrum of the above polybutylene adipate / terephthalate PBAT and calculating the peak area of the corresponding peak, the mole fraction of the polybutylene terephthalate segment in each PBAT is measured, and the calculation method is as follows:
[0166] T%=A 8.09 / (A 8.09 +A 2.33 )
[0167] Wherein, T% represents the molar fraction of polybutylene terephthalate in PBAT;
[0168] A 8.09 represents the peak area at 8.09 in the NMR spectrum;
[0169] A 2.33 It represents the peak area at 2.33 in the NMR spectrum.
[0170] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of PBAT prepared in Synthesis Example 3.
[0171] (1) The results of the mole fraction of the polybutylene terephthalate segment in the PBAT prepared in each synthesis example are shown in Table 1 below.
[0172] (2) A mixed solvent was prepared by compounding phenol and dichlorobenzene in a weight ratio of 50:50. The intrinsic viscosity of each PBAT at 25° C. was measured according to DIN 53728, Part 3 of January 3, 1985. The results are shown in Table 1 below.
[0173] Table 1
[0174]
[0175]
[0176] 3. The above PBATs are used to prepare biodegradable polylactic acid-based composite materials and nose bridge strips:
[0177] Embodiment 1:
[0178] This embodiment provides a biodegradable polylactic acid-based composite material, a preparation method thereof, and a nose bridge strip, as follows:
[0179] (1) 45 parts of PLA-1, 40 parts of PBAT-3, 15 parts of talc-1 and 0.4 parts of lubricant were mixed uniformly according to the above-mentioned feeding ratio, and then put into a twin-screw extruder, extruded at 200° C., granulated and dried to obtain a biodegradable polylactic acid-based composite material-1.
[0180] (2) The biodegradable polylactic acid-based composite material-1 is fed into an extruder, and the temperature of different body sections is adjusted to 150-180° C. for processing and molding, thereby obtaining a degradable nose bridge strip.
[0181] Referring to the operating steps shown in Example 1 and according to the formulation shown in Table 2, the biodegradable polylactic acid-based composite materials of Examples 2 to 12 and Comparative Examples 1 to 7 were prepared.
[0182] Table 2
[0183]
[0184]
[0185]
[0186] Note: Blanks in the table indicate that the substance was not added;
[0187] 4. The biodegradable polylactic acid-based composite materials and nose strips with a width of 3.0 mm and a thickness of 0.8 mm prepared in Examples 1 to 12 and Comparative Examples 1 to 7 were subjected to performance tests. The test method is as follows:
[0188] (1) Melt flow rate was measured according to GB / T 3682.1-2018, under the conditions of 190°C and 2.16 kg.
[0189] (2) Bending performance test: Use a specified mold to fold a finished nose bridge strip with a length of 8 cm, hold it for 10 seconds and then release it. After the finished nose bridge strip is left to stand for 1 minute, use a protractor to test its forming angle. The experimental conditions are temperature (23±2)°C and relative humidity (50±10)%.
[0190] (3) Aging conditions are 60°C, 60% humidity, and aging time is 72h.
[0191] The test results are shown in Table 3 below:
[0192] Table 3
[0193]
[0194]
[0195] Note: * indicates that the nose bridge sample has brittle fracture.
[0196] It can be seen from Table 3 that the all-plastic nose bridge strip products of Examples 1 to 12 have a folded rebound angle of less than 10°, and a 90° rebound angle of less than 15°; the biodegradable nose bridge strip product has a folded rebound angle of less than 15° after aging, and a 90° rebound angle of less than 20°; it shows better bending performance than Comparative Examples 1 to 7, and is more suitable for use as a plastic nose bridge strip for disposable masks.
[0197] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0198] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A biodegradable polylactic acid-based composite material, characterized in that: The composition comprises the following components in parts by weight: 15-55 parts of polylactic acid; 30-70 parts of polybutylene adipate / terephthalate; and 15-40 parts of filler; In the polylactic acid, the mass content of residual monomers is ≤0.3%; The polybutylene adipate / terephthalate has a structure shown in formula (I): p is 0.44 to 0.54, p+q=1; At 25° C., the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g.
2. The biodegradable polylactic acid-based composite material according to claim 1, characterized in that: The composition comprises the following components in parts by weight: 15-45 parts of polylactic acid; 40-60 parts of polybutylene adipate / terephthalate; and 15 to 35 parts of filler.
3. The biodegradable polylactic acid-based composite material according to claim 1 or 2, characterized in that: The D50 particle size of the filler is ≤10 μm.
4. The biodegradable polylactic acid-based composite material according to claim 3, characterized in that: The filler is one of talc and calcium carbonate or a mixture of both.
5. The biodegradable polylactic acid-based composite material according to claim 4, characterized in that: The biodegradable polylactic acid-based composite material further comprises 0.1 to 2 parts of lubricant in parts by weight.
6. A method for preparing the biodegradable polylactic acid-based composite material according to any one of claims 1 to 5, characterized in that: The steps include: The polylactic acid, polybutylene adipate / terephthalate and filler are blended and extruded.
7. The method for preparing the biodegradable polylactic acid-based composite material according to claim 6, characterized in that: The preparation method of polybutylene adipate / terephthalate comprises the following steps: Terephthalic acid, 1,4-butanediol and a catalyst are mixed to prepare an esterified product A1 through an esterification reaction, wherein the molar ratio of terephthalic acid to 1,4-butanediol is (1.1-2.5):1; Adipic acid and 1,4-butanediol are mixed in a molar ratio of (1 to 1.8):1, and an esterification reaction is performed to prepare an esterified product A2; The esterified product A1 and the esterified product A2 are mixed and reacted at a temperature of 200° C. to 245° C. and a pressure of 1 KPa to 10 KPa for 0.5 h to 5 h to prepare a prepolymer; The prepolymer is reacted for 1 h to 5 h at a temperature of 230° C. to 255° C. and a pressure of ≤150 Pa to obtain the polybutylene adipate / terephthalate.
8. The method for preparing the biodegradable polylactic acid-based composite material according to claim 7, characterized in that: The process parameters for preparing the esterification product A1 include: The temperature is 200℃~250℃, the pressure is 30KPa~110KPa, and the time is 1.5h~3.5h; and / or The process parameters for preparing the esterification product A2 include: The temperature is 100℃~250℃, the pressure is 30KPa~110KPa, and the time is 2h~4h.
9. A nose bridge strip, characterized in that: The invention relates to a biodegradable polylactic acid-based composite material comprising the biodegradable polylactic acid-based composite material according to any one of claims 1 to 5, or a biodegradable polylactic acid-based composite material prepared by the preparation method according to any one of claims 6 to 8.
10. A mask, characterized in that: The nose bridge strip comprising claim 9.