A kind of water-based white ink for flexible packaging and its preparation method and application

By using a combination of modified polyurethane and aqueous acrylic resin emulsion in aqueous inks, the problems of slow drying speed and poor adhesion of water-based inks are solved, and efficient printing and environmental protection performance are improved, and it is suitable for plastic film printing.

CN116554728BActive Publication Date: 2024-11-26ZHENGZHOU UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310657122.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-11-26
Estimated Expiration
2043-06-05

AI Technical Summary

Technical Problem

The existing water-based inks have problems such as slow drying speed, poor transferability, poor adhesion and high cost, which affect printing efficiency and environmental protection performance.

Method used

Modified polyurethane emulsion and aqueous acrylic resin emulsion are used as connecting materials, combined with molecular weight optimization and wetting leveling agents to improve the viscosity, adhesion and peel strength of aqueous inks to prepare a water-based white ink for flexible packaging.

Benefits of technology

The rapid drying, good adhesion and high peel strength of water-based ink are achieved, the printing speed reaches 350-380 m/min, the adhesion is ≥90, the peel strength is 2.5-3.2 N/m, and it is environmentally friendly and free of benzene, ketone, and esters. Organic hazardous substances, suitable for plastic film printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004267436780000011
    Figure HDA0004267436780000011
  • Figure HDA0004267436780000012
    Figure HDA0004267436780000012
  • Figure HDA0004267436780000021
    Figure HDA0004267436780000021
Patent Text Reader

Abstract

The present invention belongs to the field of new environmentally friendly water-based white ink, and specifically discloses a water-based white ink for flexible packaging, a preparation method thereof and an application thereof. The water-based white ink for flexible packaging comprises the following components by weight: 5-15 parts of modified polyurethane emulsion, 25-40 parts of water-based acrylic resin emulsion, 18-22 parts of dispersion medium, 30-40 parts of titanium dioxide, 0.02-0.10 parts of wetting and leveling agent, and 1-4 parts of other auxiliary agents; the dispersion medium is ethanol and water. The present invention selects a modified polyurethane emulsion with a weight-average molecular weight of 901 and a water-based acrylic resin emulsion with a trimodal molecular weight distribution (3064, 738, 289) as a connecting material. The two materials cooperate with each other, and the prepared water-based white ink for flexible packaging has good printing suitability, safety and environmental protection, and is not easy to fade. The printing speed on the PE substrate is 350-380 m / min, the adhesion is ≥90, and the peel strength is 2.5-3.2 N / m, which can be widely used in plastic film printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of novel environmentally friendly water-based inks, and in particular relates to a water-based white ink for flexible packaging, a preparation method and an application thereof. Background Art

[0002] At present, 90% of enterprises in my country's film and soft-cover industry adopt gravure printing technology, and most of them use solvent-based inks. This type of ink is easy to volatilize harmful gases during use, causing harm to the environment and human body. In recent years, with the increase of people's environmental protection, the environmental protection department has introduced a series of policies and regulations to reduce VOCs in response to environmental pollution problems in printing. In order to cope with this policy, most companies currently use terminal treatment technology to install organic waste gas treatment devices at the end of production, but this method cannot really solve the problem from the source. In 2020, after China proposed to achieve the "dual carbon" goal, the state's governance and control of the high-pollution printing industry has become increasingly strict, and enterprises have suffered huge losses due to production restrictions and shutdowns. At the same time, the cost of RTO equipment and maintenance costs of enterprises are too high. In this case, the demand for water-based inks by enterprises is increasing.

[0003] Water-based ink is environmentally friendly and safe, which is mainly reflected in the following three aspects. First, it does not pollute the environment. Since water-based ink uses water as a solvent, it will hardly emit volatile organic gases (VOC) into the atmosphere during the production process or the use process. Second, it reduces residual toxic substances and ensures food hygiene and safety. Since it does not contain organic solvents, the toxic substances remaining on the surface of printed products are greatly reduced. This feature makes it more popular in packaging and printing products with strict hygiene requirements such as tobacco, alcohol, food, beverages, medicines, and children's toys. Third, it reduces consumption and costs. Since water-based ink has a high solid content and can be deposited in a thin film, the coating amount of water-based ink is less than that of solvent-based ink, which can reduce the coating amount by about 20%.

[0004] The main technical difficulties in the water-based ink industry at present are: (1) Slow printing drying speed: After printing, water-based ink can only rely on volatilization to dry and solidify, which will affect the printing speed. The printing speed of solvent-based ink on domestic printing machines is 300-350 m / min, while the printing speed of water-based ink is only 150-200 m / min, which greatly affects the benefits of enterprises. (2) Poor transferability: The surface tension of water-based ink is large and the wettability is poor. It cannot be well wetted and spread on substrates with low surface energy such as PP. (3) Poor adhesion: When water-based ink uses acrylic acid as a binder, the adhesion is poor. (4) Cost problem: The price of polyurethane binder is high. Although the price of acrylic acid binder is low, its printing performance is poor. In response to the above technical difficulties, Chinese patent CN107286732A discloses a water-based plastic backing composite gravure printing ink and its preparation method. The water-based ink particles prepared by using a self-made emulsion with a special functional structure and a micro-lipid slurry process slurry are dispersed to the nanometer level, which improves the color saturation concentration and adhesion fastness. Patent CN111363403A discloses a water-based film gravure composite ink and its preparation method and application, using water-based polyurethane resin and water-based acrylic resin as connecting materials to improve the adhesion, peel strength and other properties of water-based ink. Although the printing speed, wetting performance (blocking and knife line problems) and adhesion of this patent have been improved to a certain extent, the ethanol content in the formula is relatively high (28%), which is not conducive to environmental protection and affects the printing quality. While the cost is increased, the printing speed is still far lower than that of solvent-based ink. Summary of the invention

[0005] In view of the problems and shortcomings in the prior art, the purpose of the present invention is to provide an aqueous white ink for flexible packaging and a preparation method and application thereof.

[0006] To achieve the purpose of the invention, the technical solution adopted by the present invention is as follows:

[0007] The first aspect of the present invention provides a water-based white ink for flexible packaging, which comprises the following components by weight: 5-15 parts of modified polyurethane emulsion, 25-40 parts of water-based acrylic resin emulsion, 18-22 parts of dispersion medium, 30-40 parts of titanium dioxide, 0.02-0.10 parts of wetting and leveling agent, and 1-4 parts of auxiliary agent.

[0008] According to the water-based white ink for soft packaging, preferably, the solid content of the modified polyurethane emulsion is 31.5%-33.5%, and the weight average molecular weight of the modified polyurethane is 901. The molecular weight of polyurethane determines the viscosity of water-based ink, the drying speed of printed water-based ink, and the printability. If the printing speed is too fast, the printability deteriorates, and phenomena such as unclear scraping, plate blocking, and knife lines occur. Therefore, the present invention selects a modified polyurethane with a weight average molecular weight of 901 after multiple experiments, so that the viscosity of the water-based ink can take into account both the drying speed and the printability.

[0009] According to the water-based white ink for flexible packaging, preferably, the solid content of the water-based acrylic resin emulsion is 32%-35%; the molecular weight distribution of the water-based acrylic resin is 3064, 738, 289.

[0010] The acrylic resin emulsion selected in the present invention is a water-soluble resin, and contains a large number of amide bonds in the structure, which can effectively enhance the adhesion and compatibility with water-based polyurethane. In addition, the larger the polymer molecular weight, the better the adhesion of the material, and the smaller the molecular weight, the better the printability of the material. Therefore, the present invention selects an acrylic resin with a molecular weight showing a trimodal distribution (3064, 738, 289), which can provide excellent mechanical properties for water-based ink and ensure the printing performance of water-based ink.

[0011] According to the water-based ink for flexible packaging, preferably, the wetting and leveling agent has an anionic polyether silicone with a molecular weight of 20,000-30,000.

[0012] According to the water-based ink for flexible packaging, preferably, the dispersion medium is ethanol and water, and the mass ratio of ethanol to water in the dispersion medium is (5-10): (9-15).

[0013] According to the water-based ink for flexible packaging, preferably, the auxiliary agent includes ED30 matte powder and a defoamer, and the defoamer is polyether-modified silicone oil.

[0014] According to the water-based ink for flexible packaging, preferably, the fineness of the water-based ink for flexible packaging is less than or equal to 20 μm.

[0015] The second aspect of the present invention provides a method for preparing the above-mentioned aqueous white ink for flexible packaging, comprising the following steps:

[0016] 1) Mix the modified polyurethane emulsion, ethanol and water, then add the defoamer, stir for 20-30 min, then add titanium dioxide, water and wetting and leveling agent, and continue stirring for 50-60 min to obtain a mixed dispersion;

[0017] 2) grinding the mixed dispersion to obtain a grinding product;

[0018] 3) Add the aqueous acrylic resin emulsion to the obtained ground product, stir and mix for 30-40 min to obtain aqueous white ink for flexible packaging.

[0019] The third aspect of the present invention provides a use of the aqueous white ink for flexible packaging described in the first aspect in plastic film printing.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention selects a modified polyurethane emulsion with a weight average molecular weight of 901 and an aqueous acrylic resin emulsion with a molecular weight trimodal distribution (3064, 738, 289) as a connecting material. The two materials cooperate with each other to improve the water resistance, adhesion and peel strength of the water-based ink. The prepared water-based ink has good printability, is safe and environmentally friendly, has a fast printing speed, is resistant to friction, has a high peel strength, is not easy to fade, and can be widely used in plastic film printing.

[0022] 2. The printing speed of the water-based ink for flexible packaging prepared by the present invention on the PE substrate is 350-380 m / min, the adhesion is ≥90, and the peel strength is 2.5-3.2 N / m. The PE film prepared by the water-based ink for flexible packaging is tested with a weight of 30g / rubber and rubbed back and forth 10,000 times. The fonts and patterns have no obvious color difference changes, are clearly recognizable, and have no shedding or broken lines.

[0023] 3. In the raw materials for preparing the water-based ink of the present invention, ethanol accounts for 4.5-9.5% of the water-based ink for flexible packaging, and the raw materials do not contain benzene, ketone, ester and other organic harmful substances, and are environmentally friendly, thus being an environmentally friendly water-based ink. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the infrared absorption spectrum of the modified polyurethane of the present invention;

[0025] Figure 2 is a molecular weight distribution curve diagram of the modified polyurethane of the present invention;

[0026] Figure 3 is the infrared absorption spectrum of the waterborne acrylic resin of the present invention;

[0027] Figure 4 is a molecular weight distribution curve diagram of the waterborne acrylic resin of the present invention;

[0028] Figure 5 is the infrared absorption spectrum of the wetting and leveling agent of the present invention;

[0029] Figure 6 The contact angle results of the samples obtained in Example 1 of the present invention and Comparative Example 3 on the substrate are shown in FIG. DETAILED DESCRIPTION

[0030] The following examples are only for further explanation of the present invention. It should be noted that all technical and scientific terms used in the present invention have the same meanings as in the technical field to which the present invention belongs unless otherwise specified. The experimental methods in the following examples without specifying specific conditions are all based on conventional techniques in the technical field, or according to the conditions recommended by the manufacturer; the reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0031] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0032] Example 1

[0033] A water-based white ink for flexible packaging, the raw material composition of which is calculated by weight fraction, including:

[0034] 13 parts of modified polyurethane emulsion, 32 parts of water-based acrylic resin emulsion, 5 parts of ethanol, 15 parts of water, 36 parts of titanium dioxide, 0.05 parts of wetting and leveling agent, 3.93 parts of ED30 matte powder (selenium dioxide), and 0.02 parts of defoaming agent (polyether modified silicone oil).

[0035] The solid content of the modified polyurethane emulsion (purchased from Wuhan Zhongmo Tianhong New Material Technology Co., Ltd., product model: 218 resin) is 32.5±1.0%, and the weight average molecular weight of the modified polyurethane is 901. Its structural characterization can be found in Figure 1 and Figure 2 The solid content of water-based acrylic resin emulsion (purchased from Foshan Xuanli Pigment Co., Ltd., product model: XL-1130 resin) is 32%-35%, and the molecular weight distribution of acrylic resin is 3064, 738, and 289. Its structural characterization can be found in Figure 3 and Figure 4 The wetting and leveling agent is an anionic polyether silicone with a molecular weight of 20,000-30,000 and a pigment affinity group, and a solid content of 40%. The infrared absorption spectrum of the polyether silicone is as follows: Figure 5 shown.

[0036] The preparation method of the above-mentioned aqueous white ink for flexible packaging is as follows:

[0037] 1) Add the modified polyurethane emulsion, ethanol and water into the reaction container according to the above ratio, then add the defoamer, and stir with a high-speed disperser for 20 minutes to fully dissolve; then add titanium dioxide, wetting and leveling agent, ED30 matte powder (selenium dioxide), and continue stirring for 50 minutes;

[0038] 2) The reaction product obtained in step 1) was taken out and added into a ball mill, and ground for 60 minutes to obtain a ground product with a particle size of 10-15 μm.

[0039] 3) Adding the water-soluble acrylic resin emulsion to the ground product obtained in step 2), stirring and mixing for 30 minutes, to obtain a water-based white ink for flexible packaging.

[0040] Example 2

[0041] A water-based white ink for flexible packaging, the raw material composition of which is calculated by weight fraction, including:

[0042] 10 parts of modified polyurethane emulsion, 34 parts of water-based acrylic resin emulsion, 7 parts of ethanol, 14 parts of water, 32 parts of titanium dioxide, 0.08 parts of wetting and leveling agent, 2.90 parts of ED30 matte powder (selenium dioxide), and 0.02 parts of defoaming agent (polyether modified silicone oil).

[0043] The solid content of the modified polyurethane emulsion (purchased from Wuhan Zhongmo Tianhong New Material Technology Co., Ltd., product model: 218 resin) is 32.5±1.0%, and the weight average molecular weight of the modified polyurethane is 901. The solid content of the water-based acrylic resin emulsion (purchased from Foshan Xuanli Pigment Co., Ltd., product model: XL-1130 resin) is 32%-35%, and the molecular weight distribution of the acrylic resin is 3064, 738, and 289. The wetting and leveling agent uses an anionic polyether silicone with a molecular weight of 20,000-30,000 containing pigment affinity groups, and the solid content is 40%.

[0044] The preparation method of the above-mentioned aqueous white ink for flexible packaging is the same as that in Example 1.

[0045] Example 3

[0046] A water-based white ink for flexible packaging, the raw material composition of which is calculated by weight fraction, including:

[0047] 5 parts of modified polyurethane emulsion, 40 parts of water-based acrylic resin emulsion, 10 parts of ethanol, 12 parts of water, 30 parts of titanium dioxide, 0.02 parts of wetting and leveling agent, 2.94 parts of ED30 matte powder (selenium dioxide), and 0.04 parts of defoaming agent (polyether modified silicone oil).

[0048] The solid content of the modified polyurethane emulsion (purchased from Wuhan Zhongmo Tianhong New Material Technology Co., Ltd., product model: 218 resin) is 32.5±1.0%, and the weight average molecular weight of the modified polyurethane is 901. The solid content of the water-based acrylic resin emulsion (purchased from Foshan Xuanli Pigment Co., Ltd., product model: XL-1130 resin) is 34%, and the molecular weight distribution of the acrylic resin is 3064, 738, and 289. The wetting and leveling agent uses an anionic polyether silicone with a molecular weight of 20,000-30,000 containing pigment affinity groups, and the solid content is 40%.

[0049] The preparation method of the above-mentioned aqueous white ink for flexible packaging is the same as that in Example 1.

[0050] Example 4

[0051] A water-based white ink for flexible packaging, the raw material composition of which is calculated by weight fraction, including:

[0052] 15 parts of modified polyurethane emulsion, 25 parts of water-based acrylic resin emulsion, 9 parts of ethanol, 9 parts of water, 40 parts of titanium dioxide, 0.06 parts of wetting and leveling agent, 1.91 parts of ED30 matte powder (selenium dioxide), and 0.03 parts of defoaming agent (polyether modified silicone oil).

[0053] The solid content of the modified polyurethane emulsion (purchased from Wuhan Zhongmo Tianhong New Material Technology Co., Ltd., product model: 218 resin) is 32.5±1.0%, and the weight average molecular weight of the modified polyurethane is 901. The solid content of the water-based acrylic resin emulsion (purchased from Foshan Xuanli Pigment Co., Ltd., product model: XL-1130 resin) is 32%-35%, and the molecular weight distribution of the acrylic resin is 3064, 738, and 289. The wetting and leveling agent uses an anionic polyether silicone with a molecular weight of 20,000-30,000 containing pigment affinity groups, and the solid content is 40%.

[0054] The preparation method of the above-mentioned aqueous white ink for flexible packaging is the same as that in Example 1.

[0055] Comparative Example 1

[0056] A water-based white ink, the raw material composition of which is calculated by weight fraction, including:

[0057] 40 parts of water-based acrylic resin emulsion, 6 parts of ethanol, 15 parts of water, 35 parts of titanium dioxide, 0.07 parts of wetting and leveling agent, 3.90 parts of ED30 matte powder (selenium dioxide), and 0.03 parts of defoaming agent (polyether modified silicone oil).

[0058] The solid content of the water-based acrylic resin emulsion is 32%-35%, and the molecular weight distribution of the acrylic resin is 3064, 738, and 289. The wetting and leveling agent is an anionic polyether silicone with a molecular weight of 20,000-30,000 and a pigment-affinity group, and the solid content is 40%.

[0059] The preparation method of the above-mentioned water-based white ink is the same as that of Example 1.

[0060] Comparative Example 2

[0061] A water-based white ink, the raw material composition of which is calculated by weight fraction, including:

[0062] 40 parts of modified polyurethane emulsion, 6 parts of ethanol, 15 parts of water, 35 parts of titanium dioxide, 0.07 parts of wetting and leveling agent, 3.90 parts of ED30 matte powder (selenium dioxide), and 0.03 parts of defoaming agent (polyether modified silicone oil).

[0063] The solid content of the modified polyurethane emulsion is 32.5±1.0%, and the weight average molecular weight of the modified polyurethane is 901. The wetting and leveling agent is an anionic polyether silicone with a molecular weight of 20000-30000 and a pigment affinity group, and the solid content is 40%.

[0064] The preparation method of the above-mentioned water-based white ink is the same as that of Example 1.

[0065] Comparative Example 3

[0066] A water-based white ink, the raw material composition of which is calculated by weight fraction, including:

[0067] 10 parts of modified polyurethane emulsion, 30 parts of water-based acrylic resin emulsion, 6 parts of ethanol, 15 parts of water, 35 parts of titanium dioxide, 3.90 parts of ED30 matte powder (selenium dioxide), 0.03 parts of defoaming agent (polyether modified silicone oil).

[0068] The solid content of the modified polyurethane emulsion is 32.5±1.0%, and the weight average molecular weight of the modified polyurethane is 901. The solid content of the waterborne acrylic resin emulsion is 32%-35%, and the molecular weight distribution of the acrylic resin is 3064, 738, and 289.

[0069] The preparation method of the above-mentioned aqueous white ink for flexible packaging is the same as that in Example 1.

[0070] Structural Characterization Performance Test

[0071] 1. Structural Characterization

[0072] Figure 1 The infrared absorption spectrum of the modified polyurethane selected for use in the present invention is shown in FIG. Figure 1 Middle 1690 cm -1 (amide I band), 1535 cm -1 (amide II band), 1245 cm -1 (amide III band), 1173 cm -1 The peaks near the ester bond correspond to the stretching vibration of the carbon-oxygen single bond COC, 1728 cm -1 Corresponding to the C=O stretching vibration of the carbon-oxygen double bond of the ester carbonyl group in polyurethane, all of the above are characteristic peaks of polyurethane. 3361 cm -1 Corresponding to the stretching vibration of OH and NH, 1645 cm -1 is the stretching vibration of the urea group, 600 cm -1 is the bending vibration of the isocyanate group.

[0073] Figure 2 This is the molecular weight distribution curve of the modified polyurethane selected for use in the present invention.

[0074] Figure 3The infrared absorption spectrum of the water-based acrylic resin selected for use in the present invention is: Figure 3 Medium 1632 cm -1 The amide I band vibration mode corresponding to the amide bond in waterborne acrylic resin is 1545 cm -1 The amide II band vibration mode corresponding to the amide bond, 1071 cm -1 Corresponding to the COC stretching vibration of the ester group, all of the above are characteristic peaks of water-based acrylic resin. 3328 cm -1 Corresponding to OH and NH stretching vibration, 1405 cm -1 、697 cm -1 Corresponding to CH bending vibration.

[0075] Figure 4 This is a molecular weight distribution curve of the water-based acrylic resin selected for use in the present invention.

[0076] Figure 5 This is the infrared absorption spectrum of the wetting and leveling agent (polyether silicone) selected in the present invention. -1 Corresponding to silicon-carbon bond Si-CH 3 Bending vibration mode, 753cm -1 and 839cm -1 Corresponding to the Si-C antisymmetric stretching vibration mode and stretching vibration mode of the silicon-carbon bond. 1077 cm -1 、1043cm -1 Corresponding to the antisymmetric stretching vibration of Si-O-Si of silane ether bond, 2864 cm -1 Corresponding to the stretching vibration of carbon and hydrogen CH.

[0077] Performance Testing

[0078] In order to facilitate the comparison of the raw material ratios of Examples 1-4 and Comparative Examples 1-3, they are now organized into Table 1:

[0079] The specific raw material ratios are listed in Table 1.

[0080] .

[0081] The performance tests were performed on the products prepared in Examples 1-4 and Comparative Examples 1-3. The test results are shown in Table 2. The specific test methods are as follows:

[0082] Drying speed: The printing speed was tested using a Beiren printing press.

[0083] Adhesion: The adhesion of the aqueous white ink for the flexible packaging of the present invention coated on the PE substrate was tested according to the national standard GB / T 13217.7-2009 “Test method for adhesion fastness of liquid ink”.

[0084] Friction resistance: The samples of the embodiments and comparative examples were coated on a PE substrate to test their friction resistance. The PE film was tested with a rubber load of 30 g / rubber and rubbed back and forth 10,000 times.

[0085] Peel strength: The peel strength of the OPP / VMCPP composite film prepared with aqueous white ink for flexible packaging of the present invention at 180° C. was tested according to the method of national standard GB / T 26394-2011 “Aqueous Film Gravure Composite Ink”.

[0086] Contact angle: Contact angle test results refer to Figure 6 .

[0087] The above performance test results are shown in Table 2:

[0088] .

[0089] Result analysis:

[0090] As can be seen from Table 2, compared with Comparative Example 1 (printing speed of 250 m / min, adhesion ≥50, peel strength of 1.5 N / m) without using modified polyurethane emulsion, the printing speed, adhesion and peel strength of Examples 1-4 (printing speed of 350-380 m / min, adhesion ≥90, peel strength of 2.5-3.2 N / m) are significantly improved. This is because the modified polyurethane structure selected by the present invention contains a large number of urea bonds, which can better form an action force with the corona-exposed substrate, thereby increasing the adhesion of the water-based ink. The peel strength of the obtained water-based ink is also significantly higher than the industry standard of 0.6-1N / m. In addition, hydrogen bonds can be formed in the modified polyurethane molecules, weakening the action force between polyurethane and water molecules and the action force between polyurethane molecules. In the process of water volatilization and film formation, the action force required for water volatilization is reduced, the molecular steric hindrance is reduced, and a water molecule release channel is created. It is no longer necessary to pass through the dense resin film structure layer, and the printing drying speed can be effectively improved at a lower temperature.

[0091] Compared with Comparative Example 2 in which no aqueous acrylic resin emulsion is used, the printing speed and peel strength of Examples 1-4 (printing speed of 350-380 m / min, adhesion ≥90, peel strength of 2.5-3.2 N / m) are significantly improved. This is because the aqueous acrylic resin emulsion selected in the present invention contains a large number of amide bonds in its structure, which effectively enhances the adhesion to the substrate and enhances the compatibility with aqueous polyurethane, better reduces the contact between polyurethane and water molecules, reduces the force required for water volatilization during the water volatilization film formation process, and effectively improves the printing drying speed at a lower temperature.

[0092] Compared with the comparative example 3 (contact angle of 75 o), Example 1-4 (contact angle is 40 o -46 o ) has a significantly reduced contact angle. The solvent of water-based ink is mainly water, which has a large surface tension and poor wettability. Therefore, it cannot be well wetted and spread on substrates such as PP with low surface energy, which is manifested as a large contact angle. Examples 1-4 of the present invention use anionic polyether silicone with a molecular weight of 20,000-30,000 containing pigment affinity groups as a surfactant (i.e., a wetting and leveling agent). The wetting and leveling agent has an amphiphilic structure (Si-O-Si hydrophilic, alkyl chain hydrophobic). When the water-based ink is coated on the surface of the substrate, the wetting and leveling agent is at the bottom of the coating, the lipophilic group adheres to the solid surface for directional adsorption, and the hydrophilic group extends into the liquid, so that the liquid forms a continuous phase on the solid surface, and the contact between water and the substrate is converted into the contact between water and the hydrophilic group of the wetting and leveling agent, forming a sandwich structure with the wetting and leveling agent as the intermediate layer, making the water phase easier to spread, thereby reducing the contact angle of the water-based ink on the substrate and effectively improving the wetting and leveling property of the water-based ink.

[0093] In addition, in the raw materials for preparing the water-based ink of the present invention, ethanol accounts for 4.5-9.5% of the water-based white ink for soft packaging, and the raw materials do not contain benzene, ketone, ester and other organic harmful substances, which is environmentally friendly and is an environmentally friendly water-based ink.

[0094] In summary, the present invention uses modified polyurethane emulsion and water-based acrylic resin emulsion as connecting materials. The two materials cooperate with each other to improve the water resistance, adhesion and peeling strength of water-based ink. The prepared water-based white ink has good printing suitability, safety and environmental protection, fast printing speed, friction resistance, high peeling strength, and is not easy to fade. It can be suitable for packaging surface printing and back printing. The water-based ink prepared by the present invention is applied to PE, PA, OPP / VMCPP, etc., and the printing speed can reach more than 300 m / min while ensuring low cost. It is an environmentally friendly water-based ink and can be widely used in plastic film printing.

[0095] The above embodiments are specific implementation methods of the present invention, but the implementation methods of the present invention are not limited to the above embodiments. Any other combination, change, modification, substitution and simplification that does not exceed the design concept of the present invention shall fall within the protection scope of the present invention.

Claims

1. A water-based white ink for flexible packaging, characterized in that: By weight, it includes the following components: 15 parts of modified polyurethane emulsion, 25 parts of water-based acrylic resin emulsion, 9 parts of ethanol, 9 parts of water, 40 parts of titanium dioxide, 0.06 parts of wetting and leveling agent, 1.91 parts of ED30 matte powder, and 0.03 parts of polyether modified silicone oil; the modified polyurethane is 218 resin containing urea group, with a solid content of 32.5±1.0%, and the weight average molecular weight of the modified polyurethane is 901, which is purchased from Wuhan Zhongmo Tianhong New Material Technology Co., Ltd.; the solid content of the water-based acrylic resin emulsion is 32%-35%, the molecular weight distribution of the acrylic resin is 3064, 738, and 289, and the water-based acrylic resin emulsion is XL-1130 resin, which is purchased from Foshan Xuanli Pigment Co., Ltd.; the wetting and leveling agent is an anionic polyether silicone containing pigment affinity groups with a molecular weight of 20000-30000, and the solid content is 40%.

2. The aqueous white ink for flexible packaging according to claim 1, characterized in that: The fineness of the aqueous white ink for flexible packaging is less than or equal to 20 μm.

3. The method for preparing aqueous white ink for flexible packaging according to any one of claims 1-2, characterized in that: The following steps are involved: 1) Add the modified polyurethane emulsion, ethanol and water into a reaction vessel, then add the polyether modified silicone oil, and stir and disperse with a high-speed disperser for 20 minutes to fully dissolve; then add titanium dioxide, wetting and leveling agent, and ED30 matte powder, and continue stirring for 50 minutes; 2) taking out the reaction product obtained in step 1) and adding it into a ball mill, grinding for 60 minutes to obtain a grinding product with a particle size of 10-15 μm; 3) Adding the aqueous acrylic resin emulsion to the ground product obtained in step 2), stirring and mixing for 30 minutes, to obtain aqueous white ink for flexible packaging.

4. Use of the aqueous white ink for flexible packaging according to any one of claims 1-2 in plastic film printing.