Photovoltaic silver paste and preparation method and application thereof

By adding metal oxides, hydroxides and low-melting-point metal dopants into the conductive silver paste of photovoltaic cells, and using their reaction and fusion with the TCO layer, the problem of poor ohmic contact performance of traditional silver paste is solved and better Current collection and photoelectric conversion efficiency.

CN116580870BActive Publication Date: 2024-10-01安徽思尔维新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310764980.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-27
Publication Date
2024-10-01
Estimated Expiration
2043-06-27

AI Technical Summary

Technical Problem

Existing conductive silver pastes used in photovoltaic cells have poor ohmic contact properties. Especially low-temperature silver pastes cannot meet the sintering conditions of silver powder, aluminum powder and glass powder due to their low curing temperature, resulting in poor conductivity.

Method used

Metal oxides, metal hydroxides and low-melting point metals are added as dopants in the conductive silver paste. Through reaction and fusion with the TCO layer of the heterojunction photovoltaic cell, a doping or rearrangement structure is formed to improve the interaction between the silver paste and the TCO. layer contact effect.

Benefits of technology

At a temperature of about 200°C, the dopant reacts with the TCO layer material, slightly destroying its structure, increasing the contact area between the silver powder and the TCO layer, significantly improving the ohmic contact performance, while maintaining the stability of the resistivity, and enhancing the photoelectric conversion efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a photovoltaic silver paste and a preparation method and application thereof. The photovoltaic silver paste of the present invention comprises a conductive silver paste and a dopant; the dopant comprises at least one of a metal oxide, a metal hydroxide, and a low melting point metal; by adding a dopant to a conventional conductive silver paste formula, a substance added to the dopant that can react and fuse with the TCO layer of a heterojunction photovoltaic cell sheet, reacts, dopes or rearranges to a certain extent with the traditional TCO layer material indium tin oxide at a temperature of about 200°C, thereby slightly destroying the surface structure of the indium tin oxide, and the added dopant, due to its small particle property, can have a larger specific area to overlap with the silver powder, thereby greatly improving the contact between the silver paste and the TCO layer. The photovoltaic silver paste of the present invention reduces the influence of ohmic contact while less affecting the resistivity, thereby better collecting the current of the heterojunction photovoltaic cell sheet and providing better photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of conductive silver paste, and in particular to a photovoltaic silver paste and a preparation method and application thereof. Background Art

[0002] Photovoltaic cells are the core raw materials for photovoltaic power generation and play a core role in photoelectric conversion. In addition to silicon, the most important conductive material in the cell is silver paste. The quality of silver paste directly affects the current collection efficiency. The resistivity and ohmic contact quality are the most critical factors in evaluating whether a silver paste is compatible with photovoltaic cells.

[0003] Traditional high-temperature silver paste can puncture silicon wafers at high temperatures through the combined effects of silver powder, aluminum powder and glass powder, thereby forming a very direct conductive line and a better ohmic contact. However, low-temperature photovoltaic silver paste, due to its low final curing temperature, is far from meeting the sintering conditions of silver powder, aluminum powder and glass powder. The current mainstream relies on the shrinkage of the resin to form very weak ohmic contact performance. This is also the reason why traditional low-temperature silver paste has poor ohmic contact.

[0004] Based on the defects of the current conductive silver paste used in photovoltaic cells, it is necessary to improve it. Summary of the invention

[0005] In view of this, the present invention proposes a photovoltaic silver paste and a preparation method and application thereof to solve the technical problems existing in the prior art.

[0006] In a first aspect, the present invention provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0007] Wherein, the dopant includes at least one of metal oxide, metal hydroxide and low melting point metal.

[0008] Preferably, in the photovoltaic silver paste, the metal oxide includes at least one of aluminum oxide, silicon oxide, phosphorus oxide, nickel oxide, copper oxide, cuprous oxide, iron oxide, tellurium oxide, cadmium oxide, tin oxide, indium oxide, antimony oxide, silver oxide, lead oxide, and bismuth oxide.

[0009] Preferably, in the photovoltaic silver paste, the metal hydroxide includes at least one of aluminum hydroxide, iron hydroxide, copper hydroxide, tellurium hydroxide, cadmium hydroxide, tin hydroxide, indium hydroxide, antimony hydroxide, silver hydroxide, lead hydroxide and bismuth hydroxide.

[0010] Preferably, in the photovoltaic silver paste, the low melting point metal includes at least one of mercury, gallium, indium, tin, bismuth, lead, cadmium, dysprosium, amalgam, gallium alloy, indium alloy, tin alloy, bismuth alloy, lead alloy, cadmium alloy and dysprosium alloy.

[0011] Preferably, in the photovoltaic silver paste, the mass of the dopant is 0.05-5% of the mass of the conductive silver paste.

[0012] Preferably, in the photovoltaic silver paste, the particle size of the dopant is 10 to 1000 nm.

[0013] Preferably, the photovoltaic silver paste, the conductive silver paste comprises: silver powder, resin, solvent, curing agent;

[0014] The resin includes at least one of epoxy resin, polyester resin and acrylic resin;

[0015] And / or, the solvent includes at least one of DBE, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether, and terpineol;

[0016] And / or, the curing agent includes at least one of a self-blocking isocyanate curing agent, a phthalate, a silane coupling agent, dicyandiamide, modified dicyandiamide, imidazole, modified imidazole, anhydride, boron trifluoride monoethylamine and an amino resin.

[0017] Preferably, in the photovoltaic silver paste, the mass ratio of the silver powder, the resin, the solvent and the curing agent is (80-100):(5-10):(8-15):(1-5).

[0018] In a second aspect, the present invention also provides a method for preparing the photovoltaic silver paste, comprising the following steps: mixing silver powder, resin, solvent, curing agent and dopant, and stirring to obtain photovoltaic silver paste.

[0019] In a third aspect, the present invention further provides an application of the photovoltaic silver paste or the photovoltaic silver paste prepared by the preparation method in photovoltaic cells.

[0020] The photovoltaic silver paste and its preparation method and application of the present invention have the following beneficial effects compared with the prior art:

[0021] The photovoltaic silver paste of the present invention comprises a conductive silver paste and a dopant; the dopant comprises at least one of a metal oxide, a metal hydroxide, and a low melting point metal; by adding a dopant to a conventional conductive silver paste formula, a substance added to the dopant that can react and fuse with the TCO layer of a heterojunction photovoltaic cell sheet, reacts, dopes, or rearranges to a certain extent with the traditional TCO layer material indium tin oxide at a temperature of about 200°C, thereby slightly destroying the surface structure of the indium tin oxide, and the added dopant, due to its small particle property, can have a larger specific area to overlap with the silver powder, thereby greatly improving the contact between the silver paste and the TCO layer. The photovoltaic silver paste of the present invention reduces the influence of ohmic contact while having less influence on resistivity, thereby better collecting the current of the heterojunction photovoltaic cell sheet and providing better photoelectric conversion efficiency. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0024] The present invention provides a photovoltaic silver paste, comprising the following components: conductive silver paste and a dopant;

[0025] Wherein, the dopant includes at least one of metal oxide, metal hydroxide and low melting point metal.

[0026] It should be noted that the photovoltaic silver paste of the present invention is prepared by adding a dopant to the conventional conductive silver paste formula, wherein the dopant includes at least one of a metal oxide, a metal hydroxide, and a low melting point metal, and the dopant is a substance that can react and fuse with the TCO layer of the heterojunction photovoltaic cell sheet, and by forming a doping or rearrangement of the TCO layer at a temperature of about 200°C, the overlapping effect with the silver powder in the silver paste is improved, thereby improving the ohmic contact of the silver paste. The photovoltaic silver paste of the present invention, in the overall formula, has the most core key point of the additionally added dopant, which reacts, dopes, or rearranges with the traditional TCO layer material indium tin oxide to a certain extent at 200°C, thereby slightly destroying the surface structure of the indium tin oxide, and the added dopant, due to its small particle property, can have a larger specific area to overlap with the silver powder, thereby greatly improving the contact between the silver paste and the TCO layer.

[0027] The conductive silver paste of the present invention is a conventional low-temperature photovoltaic silver paste, which includes conventional formula combinations and proportions of silver powder, epoxy resin, curing agent, rheological agent, solvent, etc. The specific ingredients of the conductive silver paste are not described here.

[0028] In some embodiments, the core principle of the dopant is to select a substance that can react or be doped with indium tin oxide, generally including at least one of metal oxides, metal hydroxides, and low-melting-point metals; wherein the metal oxide includes at least one of aluminum oxide, silicon oxide, phosphorus oxide, nickel oxide, copper oxide, cuprous oxide, iron oxide, tellurium oxide, cadmium oxide, tin oxide, indium oxide, antimony oxide, silver oxide, lead oxide, and bismuth oxide; these metal oxides can all undergo a doping reaction with indium tin oxide at a certain temperature.

[0029] In some embodiments, the metal hydroxide includes at least one of aluminum hydroxide, iron hydroxide, copper hydroxide, tellurium hydroxide, cadmium hydroxide, tin hydroxide, indium hydroxide, antimony hydroxide, silver hydroxide, lead hydroxide, and bismuth hydroxide.

[0030] In some embodiments, the low melting point metal includes at least one of mercury, gallium, indium, tin, bismuth, lead, cadmium, dysprosium, amalgam, gallium alloy, indium alloy, tin alloy, bismuth alloy, lead alloy, cadmium alloy, and dysprosium alloy; that is, in addition to metals such as mercury, gallium, indium, tin, bismuth, lead, cadmium, and dysprosium, the low melting point metal also includes alloys formed by the above metals.

[0031] Specifically, the tin-bismuth alloy may be Sn 99 Bi1 alloy, Sn 99.5 Bi 0.5 Alloy, bismuth-lead-tin alloy can be Bi 50 Pb 30 Sn 20 Alloy, Bi-Pb-Sn-GGa-In can be Bi 50 Pb25 Sn 10 Ga 10 In5 alloy.

[0032] In some embodiments, the mass of the dopant is 0.05-5% of the mass of the conductive silver paste. If the amount of dopant added is too little, it will be difficult to dope the TCO layer, and if too much is added, it will affect the resistivity of the entire silver paste, especially when the original resistivity is relatively large. The added amount should not be too much, otherwise, even if the ohmic contact becomes better, the excessive resistivity will also affect the final photoelectric conversion efficiency.

[0033] In some embodiments, the particle size of the dopant is 10 to 1000 nm. If the particle size is too small, it will lead to serious agglomeration and fail to play the role of doping. If the particle size is too large, the specific surface area is too small and it is difficult to play the role of doping. In addition, large particles are difficult to sink to the pyramids on the surface of the silicon wafer and fail to play the role of doping.

[0034] In some embodiments, the conductive silver paste includes: silver powder, resin, solvent, and curing agent.

[0035] In some embodiments, the resin includes at least one of epoxy resin, polyester resin, and acrylic resin; preferably, the resin is epoxy resin, and more preferably bisphenol A epoxy resin.

[0036] In some embodiments, the solvent includes at least one of DBE, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether, and pineneol, preferably DBE. DBE solvent (named DBE by DuPont) is a mixture of three divalent acid esters, commonly known as nylon acid methyl ester, which is a combination of three good environmental solvents: dimethyl succinate (butanedioic acid) CH3OOC(CH2)2COOCH3, dimethyl glutarate CH3OOC(CH2)3COOCH3 and dimethyl adipate CH3OOC(CH2)4COOCH3.

[0037] In some embodiments, the curing agent includes at least one of a self-blocking isocyanate curing agent, a phthalate, a silane coupling agent, dicyandiamide, a modified dicyandiamide, an imidazole, a modified imidazole, an acid anhydride, boron trifluoride monoethylamine and an amino resin, preferably imidazole.

[0038] In some embodiments, the mass ratio of silver powder, resin, solvent, and curing agent is (80-100):(5-10):(8-15):(1-5).

[0039] In some embodiments, the average particle size of the silver powder is 1-5 μm.

[0040] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned photovoltaic silver paste, comprising the following steps: mixing the conductive silver paste and the dopant, and stirring to obtain the photovoltaic silver paste.

[0041] In some embodiments, after the conductive silver paste and the dopant are mixed, they are stirred and mixed by a disperser until the fineness is less than 15 μm, thereby obtaining a photovoltaic silver paste.

[0042] Based on the same inventive concept, the present invention also provides an application of the above-mentioned photovoltaic silver paste or the photovoltaic silver paste prepared by the above-mentioned preparation method in photovoltaic cells.

[0043] The photovoltaic silver paste of the present application and its preparation method and application are further described below with specific examples. This section further illustrates the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0044] Example 1

[0045] The embodiment of the present application provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0046] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0047] The dopant includes: phosphorus oxide with an average particle size of 100 nm and metal indium particles with an average particle size of 100 nm;

[0048] The mass of phosphorus oxide is 0.5% of the mass of the conductive silver paste, and the mass of the metal indium particles is 0.5% of the mass of the conductive silver paste.

[0049] Example 2

[0050] The embodiment of the present application provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0051] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0052] The dopants include: copper hydroxide with an average particle size of 25 nm and tin oxide with an average particle size of 50 nm;

[0053] The mass of copper hydroxide is 0.1% of the mass of the conductive silver paste, and the mass of tin oxide is 1.2% of the mass of the conductive silver paste.

[0054] Example 3

[0055] The embodiment of the present application provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0056] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0057] The dopants include: indium oxide with an average particle size of 10 nm, lead hydroxide with an average particle size of 50 nm, and tin-bismuth alloy (specifically Sn 99 Bi1 alloy, the molar ratio of Sn to Bi is 99:1);

[0058] The mass of indium oxide is 0.3% of the mass of the conductive silver paste, the mass of lead hydroxide is 0.3% of the mass of the conductive silver paste, and the mass of tin-bismuth alloy is 0.3% of the mass of the conductive silver paste.

[0059] Example 4

[0060] The embodiment of the present application provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0061] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0062] The dopant includes: bismuth-lead-tin alloy (specifically Bi 50 Pb 30 Sn 20 alloy, the molar ratio of Bi, Pb and Sn is 50:30:20) and the bismuth-lead-tin-gallium-indium alloy (specifically Bi 50 Pb 25 Sn 10 Ga 10 In5 alloy, the molar ratio of Bi, Pb, Sn, Ga and In is 50:25:10:10:5);

[0063] The mass of the bismuth-lead-tin alloy is 0.5% of the mass of the conductive silver paste, and the mass of the bismuth-lead-tin-gallium-indium alloy is 1% of the mass of the conductive silver paste.

[0064] Example 5

[0065] The embodiment of the present application provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0066] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0067] The dopant includes: indium oxide with an average particle size of 10 nm and tin-bismuth alloy (specifically Sn 99.5 Bi 0.5 alloy, the molar ratio of Sn to Bi is 99.5:0.5);

[0068] The mass of indium oxide is 0.05% of the mass of the conductive silver paste, and the mass of the tin-bismuth alloy is 0.15% of the mass of the conductive silver paste.

[0069] Comparative Example 1

[0070] This comparative example provides a photovoltaic silver paste, comprising the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent.

[0071] Comparative Example 2

[0072] This comparative example provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0073] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0074] The dopant is indium oxide with an average particle size of 10 nm;

[0075] The mass of indium oxide is 15% of the mass of the conductive silver paste.

[0076] Comparative Example 3

[0077] This comparative example provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0078] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0079] The dopant is lead oxide with an average particle size of 15 μm;

[0080] The mass of lead oxide is 1.5% of the mass of the conductive silver paste.

[0081] Comparative Example 4

[0082] This comparative example provides a photovoltaic silver paste, comprising the following components: a conductive silver paste and a dopant;

[0083] The conductive silver paste includes the following raw materials in parts by weight: 45 parts by weight of silver powder with an average particle size of 5 μm, 45 parts by weight of silver powder with an average particle size of 1 μm, 8 parts by weight of bisphenol A epoxy resin, 2 parts by weight of imidazole curing agent, and 10 parts by weight of DBE solvent;

[0084] The dopant is metal tin powder with an average particle size of 5 μm;

[0085] The mass of the tin powder is 1% of the mass of the conductive silver paste.

[0086] Performance Testing

[0087] After mixing the raw material components of the photovoltaic silver paste in Examples 1 to 5 and Comparative Examples 1 to 4, the mixture was stirred and mixed evenly by a disperser, and then printed on the surface of the heterojunction solar cell, and then dried and cured at 200° C. for 30 minutes, and the ohmic contact and resistivity values ​​were tested. The results are shown in Table 1 below.

[0088] Table 1 - Ohmic contact and resistivity data of photovoltaic pastes in different embodiments

[0089] Example Resistivity (μΩ·cm) <![CDATA[Ohmic contact (mΩ·cm 2 )]]> Example 1 8.8 3.7 Example 2 9.0 3.1 Example 3 8.3 1.8 Example 4 7.6 2.0 Example 5 8.0 3.4 Comparative Example 1 8.5 5.2 Comparative Example 2 150 4.8 Comparative Example 3 15.4 5.5 Comparative Example 4 8.8 5.0

[0090] As can be seen from Table 1, in Example 1, by adding a certain amount of oxide and low-melting-point metal, the ohmic contact can be reduced to a certain extent. At the same time, due to the large resistivity of the oxide, the resistivity will be slightly affected. In Example 2, by adding a certain amount of hydroxide and oxide, the ohmic contact can be improved, but the resistivity will also be increased. In Example 3, by adding oxides, hydroxides and low-melting-point alloys, while paying attention to balancing the size of the added particles, a better effect is achieved, and the ohmic contact is greatly reduced without almost affecting the resistivity. In Example 4, by adding two low-melting-point metal alloys, the resistivity can be reduced to a certain extent, while the ohmic contact is greatly reduced. In Example 5, by adding a small amount of small-particle metal oxides and low-melting-point metal alloys, it is also possible to achieve a good resistivity effect while maintaining a good low-ohmic contact. Conventional low-temperature photovoltaic silver paste is used in Comparative Example 1, which has a good resistivity, but the ohmic contact level is poor. Too much oxide is added in Comparative Example 2, resulting in a sudden change in the resistivity of the silver paste, which cannot be used in the end. In Comparative Example 3, too much oxide was added, which resulted in the additive not being able to reach the gaps inside the silicon wafer pyramids. At the same time, the overlap surface with the silver powder was too small, which ultimately affected the resistivity. In Comparative Example 4, a certain amount of low-melting-point metal powder was added alone. Compared with Comparative Example 1 without adding low-melting-point metal powder, the resistivity and ohmic contact were very close, and there was no significant improvement.

[0091] The present invention adds a dopant to the conductive paste to cause a certain reaction and doping on the surface of indium tin oxide, thereby making it easier for silver powder to contact with it, thereby reducing ohmic contact. At the same time, the amount and size of the added dopant are standardized to make the addition more effective and to minimize the impact on the resistivity level. Compared with the prior art, the photovoltaic silver paste of the present invention reduces the impact of ohmic contact while having less impact on resistivity, thereby better collecting the current of the heterojunction photovoltaic cell and providing better photoelectric conversion efficiency.

[0092] The above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. Application of photovoltaic silver paste in photovoltaic cells; The photovoltaic silver paste comprises the following components: conductive silver paste and dopant; The dopant is a substance that reacts and fuses with the TCO layer of the heterojunction photovoltaic cell; in, The dopant is composed of metal oxide, metal hydroxide and low melting point metal; The metal oxide includes at least one of tin oxide and indium oxide; The metal hydroxide includes at least one of copper hydroxide and lead hydroxide; The low melting point metal includes at least one of indium, tin-bismuth alloy, bismuth-lead-tin alloy, and bismuth-lead-tin-gallium-indium alloy; The mass of the dopant is 0.05-5% of the mass of the conductive silver paste; The particle size of the dopant is 10-1000 nm; The conductive silver paste also includes: silver powder, resin, solvent, and curing agent; The mass ratio of the silver powder, resin, solvent and curing agent is (80-100):(5-10):(8-15):(1-5).

2. The use according to claim 1, characterized in that The resin includes at least one of epoxy resin, polyester resin and acrylic resin; And / or, the solvent includes at least one of DBE, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether, and terpineol; And / or, the curing agent includes at least one of a self-blocking isocyanate curing agent, a phthalate, a silane coupling agent, dicyandiamide, modified dicyandiamide, imidazole, modified imidazole, anhydride, boron trifluoride monoethylamine and an amino resin.

3. The use according to claim 1, characterized in that The preparation method of the photovoltaic silver paste comprises the following steps: mixing the conductive silver paste and the dopant, and stirring to obtain the photovoltaic silver paste.