Mildew-proof double-core corrugated paperboard and preparation method thereof
By applying a waterproof and antibacterial layer on the surface of the double-core corrugated cardboard, the problems of poor waterproof and mildew resistance are solved, and higher waterproof and antibacterial properties are achieved, and the service life is extended.
Patent Information
- Application Number
- CN202310670099.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-07
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-06-07
AI Technical Summary
During storage and use, double-core corrugated cardboard has poor waterproofness and moisture resistance due to pores and water absorption, which is prone to mildew and deterioration of performance.
Using a waterproof and antibacterial layer, including bisphenol A type epoxy resin, guanidine salt compound, propylene glycol diglycidyl ether, hydrophobically modified nanometal oxide and isoacetone, a crosslinked structure is formed to enhance the attachment by coating the surface of corrugated cardboard. Focus and stability.
It improves the waterproofness and antibacterial properties of double-core corrugated cardboard, prevents mildew, extends service life, and maintains waterproof and antibacterial properties during processing and use.
Smart Images

Figure BDA0004272596820000051 
Figure BDA0004272596820000061 
Figure BDA0004272596820000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of corrugated paperboard, and in particular to a mildew-proof double-core corrugated paperboard and a preparation method thereof. Background Art
[0002] Corrugated cardboard is a multi-layer bonded body, which is composed of at least one layer of corrugated core paper and one layer of cardboard. Double-core corrugated cardboard is made of face paper, lining paper, sandwich paper and two layers of corrugated core paper bonded together. The corrugated core paper is sandwiched between the face paper and the lining paper, and there is another layer of sandwich paper separating the two layers of corrugated core paper. Compared with single-layer corrugated cardboard, double-core corrugated cardboard has higher mechanical strength and can be used to package fragile items and withstand collision and impact during transportation.
[0003] However, during the storage and use of double-core corrugated cardboard, due to the pores between the corrugated core paper and the surface paper and lining paper, and the paper material is easy to absorb water, the waterproof and moisture-proof properties of the corrugated cardboard are poor, which in turn reduces the performance of the corrugated cardboard. On the other hand, when the corrugated cardboard is damp, it provides a suitable growth environment and nutrients for mold, and the corrugated cardboard is prone to mildew. Summary of the invention
[0004] In order to solve the problem of mildew and performance degradation caused by poor moisture-proof performance of double-core corrugated paperboard, the present application provides a mildew-proof double-core corrugated paperboard and a preparation method thereof.
[0005] In a first aspect, a mildew-proof double-core corrugated paperboard comprises face paper, lining paper, sandwich paper and two layers of corrugated core paper, characterized in that the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper are coated with a waterproof and antibacterial layer; the waterproof and antibacterial layer comprises the following raw materials in parts by weight:
[0006] 8-11 parts of bisphenol A epoxy resin;
[0007] 2 to 4 parts of a guanidine salt compound;
[0008] 8-12 parts of propylene glycol diglycidyl ether;
[0009] 1-2 parts of curing agent;
[0010] 4 to 7 parts of hydrophobically modified nano metal oxide;
[0011] 60-80 parts of isopropyl ketone.
[0012] By adopting the above technical solution, nano metal oxides are treated with hydrophobic surface and coated on the hydrophilic surface of paperboard, which can isolate the water molecules in the environment from the corrugated paperboard, making the double-core corrugated paperboard waterproof; nano metal oxides also have stable antibacterial properties, and through catalytic oxidation, they act on intracellular substances, destroy bacterial reproduction and kill bacteria, achieving the effect of mildew prevention. At the same time, nano metal oxides have special structural properties of small size effect, which can increase the strength and toughness of the waterproof and antibacterial film layer, and the waterproof and antibacterial film layer of corrugated base paper will not be damaged during the rolling process.
[0013] Guanidine salt compounds have broad-spectrum and highly effective bactericidal properties. The guanidine group they contain has high chemical activity. The compounds are positively charged, while the surfaces of various bacteria and viruses are usually negatively charged. The compounds are easily adsorbed by bacteria and viruses, thereby inhibiting the division of bacteria and viruses and making them lose their ability to reproduce.
[0014] The waterproof and antibacterial film layer is formed by a waterproof and antibacterial agent. The raw materials of the waterproof and antibacterial film layer, i.e., the raw materials of the waterproof and antibacterial agent, include hydrophobically modified nano-metal oxides and guanidine salt compounds. The guanidine salt compounds and the hydrophobically modified nano-metal oxides are cross-linked together by bisphenol A type epoxy resin. On the one hand, the hydrophobically modified nano-metal oxides are coated on the surface of the cardboard, which is easily fallen off due to friction during processing and use, resulting in the loss of hydrophobicity on the surface of the corrugated cardboard and a decrease in antibacterial properties. Through mutual cross-linking, the adhesion of hydrophobic modified nano-metal oxides to corrugated cardboard is enhanced and will not fall off easily. At the same time, the cross-linking structure also enhances the stability and strength of the waterproof and antibacterial agent after film formation. The heat resistance of guanidine salt compounds and hydrophobic modified nano-metal oxides also prevents the waterproof and antibacterial film layer on the corrugated base paper from being damaged under the pressure and temperature of the corrugator rolling machine. On the other hand, the guanidine salt compounds and the hydrophobic modified nano-metal oxides are cross-linked with each other, and the targeting effect of the guanidine salt compounds can be used to adsorb the mold on the corrugated cardboard, so that the hydrophobic nano-metal oxides can quickly exert a sterilization effect, thereby increasing the waterproof and antibacterial properties of the double-core corrugated cardboard.
[0015] Preferably, the guanidine salt compound includes one or a combination of polyhexamethylene biguanidine hydrochloride, polyhexamethylene guanidine hydrochloride, polyhexamethylene guanidine stearate, polyhexamethylene guanidine propionate, and polyhexamethylene guanidine phosphate.
[0016] By adopting the above technical solution, the guanidine salt compound can adsorb molds and prevent them from dividing and multiplying; on the other hand, the guanidine salt compound can act on the phospholipid bilayer in the cytoplasm of microorganisms such as molds through transmembrane transport, and combine with the negatively charged phospholipid group, thereby destroying the selective permeability of the cell membrane and cell metabolism, thereby killing bacteria and other microorganisms and achieving an antibacterial effect. At the same time, the guanidine group in the guanidine salt compound can react with the hydroxyl group on the cellulose in the cardboard, thereby increasing the adhesion of the waterproof antibacterial agent on the corrugated cardboard, and it is not easy to fall off during the processing process.
[0017] Preferably, the hydrophobically modified nano metal oxide is prepared by vapor precipitation of nano metal oxide and cured polydimethylsiloxane in a mass ratio of 1:(1.5-2).
[0018] Preferably, the preparation method of the hydrophobically modified nano metal oxide comprises the following steps: uniformly mixing polydimethylsiloxane and an organosilicon curing agent in a mass ratio of (11-13):1, and curing at 75-85°C for 2-4 hours; placing the cured polydimethylsiloxane and the nano metal oxide in a sealed container, performing constant temperature vapor precipitation in a muffle furnace at a temperature of 220-240°C for 1-2 hours, and then grinding and sieving to obtain the hydrophobically modified nano metal oxide.
[0019] Preferably, the nano metal oxide includes one or more of nano zinc oxide, nano titanium dioxide, and nano aluminum oxide; the organosilicon curing agent includes one or more of methyltriethoxysilane, methyltripropoxysilane, and benzyltrimethoxysilane.
[0020] By adopting the above technical scheme, the small molecular broken segments of polydimethylsiloxane pyrolysis and other small molecular substances are vapor-precipitated on the surface of nano-metal oxide, and the surface of the nano-metal oxide is modified by the rough structure of the surface to reduce the surface energy of the nano-metal oxide, so that the nano-metal oxide has hydrophobicity, and finally a hydrophobically modified nano-metal oxide with uniform powder, small particle size and less agglomeration can be obtained, while the nano-oxide obtained by the general chemical modification method has a low grafting rate and poor hydrophobic modification effect of the nano-metal oxide. Zn-O-Si bonds and Si-O-Si bonds exist on the surface of the hydrophobically modified nano-metal oxide after vapor precipitation. The silicon-oxygen bonds can form dynamic crosslinks with bisphenol A epoxy resin in the preparation process of waterproof antibacterial agents.
[0021] The hydrophobically modified nano-metal oxide is coated on the surface of the double-core corrugated board to isolate the water molecules in the environment, which can effectively increase the waterproof performance of the double-core corrugated board; at the same time, the hydrophobic modification does not destroy the structure and performance of the original nano-metal oxide. The metal ions in the hydrophobically modified nano-metal oxide will act on the bacterial cell membrane and cell wall after contacting the bacteria, destroying the structure of the cell membrane and cell wall, causing the internal substances to dissolve and the bacteria to inactivate; at the same time, the high chemical activity of the nano-scale oxide acts on the intracellular substances, destroying the bacterial reproduction, thereby achieving an antibacterial effect.
[0022] Preferably, the preparation process of the waterproof and antibacterial agent is as follows:
[0023] S1: adding bisphenol A epoxy resin to isopropanol, stirring and mixing, then adding guanidine salt compound aqueous solution, stirring evenly, adding curing agent and propylene glycol diglycidyl ether, stirring and reacting in a water bath at 40-50° C. for 3-4 hours to obtain a mixed solution; S2: adding hydrophobically modified nano-metal oxide to the mixed solution obtained in S1, and adding a catalyst and a curing agent, stirring and reacting in a water bath at 30-40° C. for 5-6 hours to obtain a waterproof antibacterial agent;
[0024] S3: coating the waterproof antibacterial agent obtained in S2 on the surface of the face paper, the lining paper, the sandwich paper and the two layers of corrugated core paper by one or a combination of brushing, spraying, dipping and rolling.
[0025] Preferably, in step S2, a catalyst is added together with the curing agent, and the mass ratio of the catalyst to the bisphenol A epoxy resin is (0.02-0.05):1; the catalyst includes one or more of potassium hydroxide and potassium carbonate.
[0026] Preferably, the coating amount of the waterproof and antibacterial agent on the surface of the face paper, the back paper, the sandwich paper and the two layers of corrugated core paper is 0.2-0.4wt%.
[0027] Preferably, the curing agent includes one or more of ethylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine.
[0028] By adopting the above technical scheme, the epoxy group in the bisphenol A epoxy resin reacts with the guanidine group in the guanidine salt compound under the catalytic action of the curing agent, and the hydrophobically modified nano metal oxide surface contains silicon oxygen bonds, and the silicon ether bond structure is reversibly disconnected and formed under the electrophilic action of the catalyst, and a dynamic cross-linking network is constructed between the bisphenol A epoxy resin; the guanidine compound and the hydrophobically modified nano metal oxide are interconnected through the bisphenol A epoxy resin, which enhances the mildew and antibacterial effect of the system. At the same time, the bisphenol A epoxy resin also ensures the strength of the waterproof and antibacterial film layer, and the addition of propylene glycol diglycidyl ether improves the toughness of the waterproof and antibacterial film layer, so that the formed waterproof and antibacterial film layer will not be easily brittle during processing and use, ensuring the long-term effectiveness of the waterproof and antibacterial performance.
[0029] In a second aspect, the present application provides a method for preparing a mildew-proof double-core corrugated paperboard, comprising the following steps:
[0030] S1: Coating waterproof antibacterial agent on the surface of corrugated base paper, face paper, lining paper and sandwich paper;
[0031] S2: rolling the corrugated base paper obtained in S1 through corrugated rollers to obtain corrugated core paper;
[0032] S3: The corrugated core paper is bonded with the face paper, the lining paper and the sandwich paper by a double-sided corrugating machine with starch adhesive, and then cut to obtain a mildew-proof double-core corrugated paperboard.
[0033] By adopting the above technical solution, the waterproof antibacterial agent is evenly coated on the contact surface between the corrugated board and the air, preventing the corrugated board from getting damp while effectively inhibiting the growth of mold. The corrugated base paper is subjected to the high pressure and high temperature of the corrugated roller, which promotes the chemical linking of the guanidine group contained in the waterproof antibacterial film layer with the hydroxyl group on the fiber in the board, thereby increasing the adhesion of the waterproof antibacterial film layer on the corrugated board, so that the obtained mildew-proof double-core corrugated board can have long-term waterproof and antibacterial properties.
[0034] In summary, this application has the following beneficial effects:
[0035] 1. The mildew-proof double-core corrugated cardboard of the present application contains a waterproof antibacterial film layer, and the waterproof antibacterial film layer contains a hydrophobic modified nano metal oxide and a guanidine salt compound, which are interconnected by a bisphenol A epoxy resin. On the one hand, through the mutual cross-linking effect, the adhesion of the hydrophobic modified nano metal oxide to the corrugated cardboard is enhanced, and it is not easy to fall off and lose its function during processing and use. At the same time, the cross-linking structure also enhances the stability and strength of the waterproof antibacterial agent after film formation; on the other hand, the guanidine salt compound and the hydrophobic modified nano metal oxide are cross-linked together, and the targeting effect of the guanidine salt compound can be utilized to adsorb the mold on the corrugated cardboard, so that the hydrophobic nano metal oxide can quickly exert a sterilization effect, thereby increasing the waterproof and antibacterial properties of the double-core corrugated cardboard.
[0036] 2. The waterproof and antibacterial film layer in the mildew-proof double-core corrugated cardboard of the present application contains guanidine groups, which have high reactivity and can react with the hydroxyl groups on the cellulose contained in the corrugated cardboard to increase the adhesion ability of the waterproof and antibacterial agent. The waterproof and antibacterial film layer is not easy to be damaged or fall off during the processing and use of the double-core corrugated cardboard, thereby losing the waterproof and antibacterial effect, thereby achieving a long-term mildew-proof effect. DETAILED DESCRIPTION
[0037] Preparation example of hydrophobically modified nano metal oxides
[0038] Preparation Example 1-1, a hydrophobically modified nano metal oxide, is prepared by the following steps:
[0039] Take 120g of polydimethylsiloxane (viscosity 4×10 5 mm 2 / s 25℃) and 10g methyltriethoxysilane are mixed evenly, allowed to stand for 6h to remove bubbles, and cured at 80℃ for 3h; 70g nano zinc oxide (particle size is 20-30nm) is placed together with the cured polydimethylsiloxane in a sealed weighing bottle, and is subjected to constant temperature vapor precipitation in a muffle furnace at a temperature of 230℃ for 1h, and the obtained solid particles are ground and sieved to obtain hydrophobically modified nano zinc oxide.
[0040] Preparation Example 1-2, a hydrophobically modified nano metal oxide, is different from Preparation Example 1-1 only in that the added amount of nano zinc oxide is 80 g.
[0041] Preparation Example 1-3, a hydrophobically modified nano metal oxide, is different from Preparation Example 1-1 only in that the added amount of nano zinc oxide is 60 g.
[0042] Preparation Example 1-4, a hydrophobically modified nano-metal oxide, is different from Preparation Example 1-1 only in that an equal amount of nano-titanium dioxide is used to replace nano-zinc oxide. Preparation Example 1-5, a hydrophobically modified nano-metal oxide, is prepared as follows: 120 g of polydimethylsiloxane (viscosity 4×10 5 mm 2 / s 25°C) was dissolved in 500ml20wt% ethanol aqueous solution, 70g nano zinc oxide was added, and the mixture was stirred and dispersed at 80°C for 4h. After filtering, it was washed with anhydrous ethanol and dried to obtain hydrophobically modified nano zinc oxide.
[0043] Preparation example of waterproof antibacterial agent
[0044] Preparation Example 2-1, a waterproof antibacterial agent, is prepared by the following steps:
[0045] Take 100g of bisphenol A epoxy resin (model E-44) and add it to 700g of isopropyl tone and stir to mix; take 30g of polyhexamethylene biguanide hydrochloride (model P304025), and prepare it with 120g of deionized water into a 20% polyhexamethylene biguanide hydrochloride aqueous solution, add the obtained polyhexamethylene biguanide hydrochloride aqueous solution to the uniformly mixed bisphenol A epoxy resin solution, stir for 30min, then add 6g of ethylenediamine and 100g of propylene glycol diglycidyl ether, stir and react in a 45°C water bath for 4h to obtain a mixed solution.
[0046] Add 50g of the hydrophobically modified nano zinc oxide prepared in Preparation Example 1-1 to the mixed solution, and add 3g of potassium hydroxide and 12g of ethylenediamine. Stir and react in a water bath at 35°C for 6h to obtain a waterproof antibacterial agent.
[0047] The difference between Preparation Example 2-2, Preparation Example 2-3 and Preparation Example 2-4 and Preparation Example 2-1 is that the ratio of the raw materials used is different, as shown in Table 1:
[0048] Table 1 Formulations of Preparation Examples 2-1 to 2-4
[0049]
[0050]
[0051] Preparation Example 2-2 uses the hydrophobically modified nano zinc oxide prepared in Preparation Example 1-3; Preparation Example 2-3 uses the hydrophobically modified nano zinc oxide prepared in Preparation Example 1-2.
[0052] Preparation Example 2-5, a waterproof antibacterial agent, is different from Preparation Example 2-1 only in that the hydrophobically modified nano-titanium dioxide prepared in Preparation Example 1-4 is used to replace the hydrophobically modified nano-zinc oxide prepared in Preparation Example 1-1.
[0053] Preparation Example 2-6, a waterproof antibacterial agent, is different from Preparation Example 2-1 only in that the added amount of polyhexamethylene biguanide hydrochloride is 60 g.
[0054] Preparation Example 2-7, a waterproof antibacterial agent, is different from Preparation Example 2-1 only in that the added amount of polyhexamethylene biguanide hydrochloride is 10 g.
[0055] Preparation Example 2-8, a waterproof and antibacterial agent, is different from Preparation Example 2-1 only in that the added amount of the hydrophobically modified nano zinc oxide prepared in Preparation Example 1-1 is 80 g.
[0056] Preparation Example 2-9, a waterproof and antibacterial agent, is different from Preparation Example 2-1 only in that the added amount of the hydrophobically modified nano zinc oxide prepared in Preparation Example 1-1 is 30 g.
[0057] Preparation Example 2-10, a waterproof antibacterial agent, is different from Preparation Example 2-1 only in that polyhexamethylene biguanide hydrochloride is not added.
[0058] Preparation Example 2-11, a waterproof antibacterial agent, is different from Preparation Example 2-1 only in that the hydrophobic modified nano zinc oxide prepared in Preparation Example 1-1 is not added.
[0059] Preparation Example 2-12, a waterproof antibacterial agent, is different from Preparation Example 2-1 only in that the hydrophobic modified nano-zinc oxide prepared in Preparation Example 1-1 is replaced by an equal amount of hydrophobic modified nano-titanium dioxide prepared in Preparation Example 1-5.
[0060] Preparation Example 2-13, a waterproof antibacterial agent, differs from Preparation Example 2-1 only in that potassium hydroxide is not added.
[0061] Preparation Example 2-14, a waterproof and antibacterial agent, is different from Preparation Example 2-1 only in that propylene glycol diglycidyl ether is not added.
[0062] Example
[0063] Example 1, a mildew-proof double-core corrugated paperboard is prepared by the following method:
[0064] A layer of waterproof and antibacterial agent prepared in Preparation Example 2-1 is applied on the surface of face paper, lining paper, sandwich paper and two layers of corrugated core paper by spraying, and the coating amount is 0.3wt%; then the corrugated base paper with a layer of waterproof and antibacterial film on the surface is rolled by corrugating rollers to obtain corrugated core paper, and the corrugated core paper is then passed through a double-sided corrugator, and the face paper, lining paper, sandwich paper and corrugated core paper are bonded together by the bonding action of starch adhesive (model MJL-520), and then cut to obtain mildew-proof double-core corrugated board.
[0065] According to the provisions of GB / T 6544-2008 "Corrugated Cardboard" for double-layer corrugated cardboard, the structure of mildew-proof double-core corrugated cardboard is 300g kraft card for face paper / 180g corrugated base paper (A / B flute) / 280g kraft card for lining paper.
[0066] Example 2, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Example 2-2 is coated on the surface of the face paper, the lining paper, the sandwich paper and the two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0067] Example 3, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Example 2-3 is coated on the surface of the face paper, the lining paper, the sandwich paper and the two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0068] Example 4, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-4 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0069] Example 5, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-5 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0070] Example 6, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-6 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0071] Example 7, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-7 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0072] Example 8, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-8 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0073] Example 9, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-9 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0074] Example 10, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Example 2-2 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.1wt%.
[0075] Example 11, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Example 2-2 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.6wt%.
[0076] Example 12, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-13 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0077] Comparative Example
[0078] Comparative Example 1, a mildew-proof double-core corrugated paperboard, is different from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-10 is coated on the surface of the face paper, the lining paper, the sandwich paper and the two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0079] Comparative Example 2, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Example 2-11 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0080] Comparative Example 3, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-14 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0081] Comparative Example 4, a mildew-proof double-core corrugated paperboard, differs from Example 1 only in that the waterproof antibacterial agent prepared in Preparation Examples 2-12 is coated on the surface of the face paper, lining paper, sandwich paper and two layers of corrugated core paper, and the coating amount is 0.3wt%.
[0082] Comparative Example 5 is a mildew-proof double-core corrugated paperboard, which is different from Example 1 in that the surface paper, the lining paper, the sandwich paper and the surfaces of the two layers of corrugated base paper are not coated with a waterproof and antibacterial agent.
[0083] Performance testing
[0084] 1. Mildew resistance test of mildew-proof double-core corrugated paperboard: Mildew resistance test was performed on the mildew-proof double-core corrugated paperboards prepared in Examples 1 to 12 and Comparative Examples 1 to 5 according to GB / T 4768-2008 “Mold-proof packaging”.
[0085] Preparation of test samples: The mildew-proof double-core corrugated paperboards prepared in Examples 1 to 12 and Comparative Examples 1 to 5 were cut into blocks of 10 cm × 10 cm and tested according to the standard requirements. The test period was 28 days, and the mildew-proof properties of the samples were compared by the mildew-proof grades of the samples after the test. Grade I means that no mildew growth was found after 28 days of mildew testing; Grade II means that the mildew growth area does not exceed 10% of the inner and outer surfaces; Grade III means that the mildew growth area does not exceed 25% of the inner and outer surfaces; Grade IV means that the mildew growth area accounts for more than 25% of the inner and outer surfaces.
[0086] 2. Waterproof test of mildew-proof double-core corrugated paperboard: According to GB / T 1540-2002 "Determination of water absorption of paper and paperboard - water absorption method", the surface water absorption capacity of the mildew-proof double-core corrugated paperboards prepared in Examples 1 to 12 and Comparative Examples 1 to 5 was measured. The relative humidity of the high and low temperature humidity test box (model PRO T / C 4-600) was set to 85%. The mildew-proof double-core corrugated paperboards prepared in Examples 1 to 12 and Comparative Examples 1 to 5 were placed in the test box for 48 hours. The water absorption values of the mildew-proof double-core corrugated paperboards before and after placement were compared. The water absorption capacity and long-term waterproof effect of the samples were compared by calculating the water absorption values of the samples, where the water absorption values are:
[0087] C=(m2-m1)×100
[0088] Where C represents the Ke Bo value, m1 represents the mass of the sample before water absorption, and m2 represents the mass of the sample after water absorption.
[0089] 3. Strength test of mildew-proof double-core corrugated cardboard: set the relative humidity of the high and low temperature humidity test box (model PRO T / C 4-600) to 85%, and place the mildew-proof double-core corrugated cardboards prepared in Examples 1 to 12 and Comparative Examples 1 to 5 in the test box for 48 hours, and compare the edge compression strength of the mildew-proof double-core corrugated cardboard before and after placement. The edge compression strength test is carried out according to GB / B6546-2021 "Determination of edge compression strength of corrugated cardboard".
[0090] The test results are shown in Table 2:
[0091] Table 2 Test results of mildew resistance, water absorption and strength of corrugated cardboard
[0092]
[0093]
[0094] According to Table 2, in combination with Example 1 and Comparative Example 5, it can be seen that the mildew resistance level of Comparative Example 5 is Level IV, which is much lower than the mildew resistance level of Example 1. The KE value of Comparative Example 5 after being treated in an environment with a relative humidity of 85% is significantly increased compared with that of Example 1, and the edge compression strength after treatment is significantly reduced, indicating that the mildew resistance and water resistance of Comparative Example 5 are significantly lower than those of Example 1. The reason may be that Comparative Example 5 has not been surface treated with a waterproof antibacterial agent. On the one hand, there is no hydrophobic effect of hydrophobically modified nano zinc oxide to isolate water molecules in the environment, and on the other hand, there is no sterilization effect of polyhexamethylene biguanide hydrochloride and hydrophobically modified nano zinc oxide. After absorbing water, the corrugated board provides a suitable growth environment for mold, which is conducive to the growth and reproduction of mold. At the same time, affected by moisture and mold, the edge compression strength of the double-core corrugated board is also significantly reduced.
[0095] Combining Example 1 and Comparative Example 2, it can be seen that the mildew resistance level of Comparative Example 2 is level III, which is lower than the mildew resistance level of Example 1. The KE value of Comparative Example 2 before and after being treated in an environment with a relative humidity of 85% is significantly increased compared with that of Example 1, and the edge compression strength decreases significantly after treatment, indicating that the mildew resistance and water resistance of Comparative Example 2 are significantly lower than those of Example 1. The reason may be that the waterproof antibacterial agent used in Comparative Example 2 does not contain hydrophobically modified nano zinc oxide, the surface of the corrugated board has not been treated with hydrophobicity, has strong hydrophilicity, and is easy to combine with water molecules in the environment, the waterproofness of the double-core corrugated board is significantly reduced, and when the water content of the corrugated board is large, the edge compression strength of the board is also significantly reduced; at the same time, the lack of hydrophobically modified nano zinc oxide makes it impossible to form a dynamic cross-linked structure in the system, the strength of the waterproof antibacterial film layer is reduced, and the dual sterilization effect with polyhexamethylene biguanide hydrochloride is lost. After the board absorbs water, the reproduction of mold is promoted, so that the mildew resistance of the double-core corrugated board is significantly reduced.
[0096] Combining Example 1 and Comparative Example 1, it can be seen that the mildew resistance level of Comparative Example 1 is Level IV, which is significantly lower than the mildew resistance level of Example 1. The KE value of Comparative Example 1 before and after being treated in an environment with a relative humidity of 85% is increased compared with that of Example 1, and the edge compressive strength decreases significantly after treatment, indicating that the mildew resistance of Comparative Example 1 is significantly reduced compared with Example 1, and the waterproofness is reduced. The reason may be that the waterproof antibacterial agent used in Comparative Example 1 does not contain polyhexamethylene biguanide hydrochloride, which has a significant antibacterial effect, and the mildew resistance of Comparative Example 1 is significantly reduced. At the same time, although hydrophobic nano zinc oxide is added in Comparative Example 1, the connection between the guanidine group and the hydroxyl group in the corrugated board is lost, and the adhesion between the waterproof antibacterial film layer and the corrugated board decreases, resulting in a decrease in the waterproofness of Comparative Example 1.
[0097] Combining Example 1 and Comparative Example 3, it can be seen that the mildew resistance level of Comparative Example 3 is level III, which is significantly lower than the mildew resistance level of Example 1. The value of Comparative Example 3 before and after being treated in an 85% relative humidity environment is significantly increased compared with Example 1, and the change before and after the treatment is very obvious. The edge compression strength decreases significantly after the treatment, indicating that the mildew resistance and water resistance of Comparative Example 3 are significantly reduced compared with Example 1. The reason may be that the waterproof antibacterial agent in Comparative Example 3 does not add propylene glycol diglycidyl ether. In the process of preparing the waterproof antibacterial agent, the addition of propylene glycol diglycidyl ether can effectively improve the toughness of the waterproof antibacterial film layer, so that the waterproof antibacterial film layer on the surface of the double-layer corrugated core paper is not easy to crack easily during production and use, thereby significantly reducing the strength of the waterproof antibacterial film layer and the long-term hydrophobic effect, and the mildew resistance, water resistance and edge compression strength of the double-core corrugated paperboard are also significantly reduced.
[0098] Combining Example 1 and Comparative Example 4, it can be seen that the mildew resistance level of Comparative Example 4 is level III, which is significantly lower than the mildew resistance level of Example 1. The value of Comparative Example 4 before and after being treated in an 85% relative humidity environment is increased compared with Example 1, and the edge compression strength after treatment is significantly reduced, indicating that the mildew resistance and water resistance of Comparative Example 4 are significantly reduced compared with Example 1. The reason may be that the hydrophobically modified nano zinc oxide used in the waterproof antibacterial agent in Comparative Example 4 is not prepared by vapor precipitation method but by general chemical grafting method, and the obtained nano oxide grafting rate is low, and the hydrophobic modification effect of nano metal oxide is poor, so that the strength of the waterproof antibacterial film layer and the long-term hydrophobic effect are significantly reduced, and the mildew resistance, water resistance and edge compression strength of the double-core corrugated board are also significantly reduced.
[0099] Combining Example 1 with Examples 2 to 4, it can be seen that the mildew resistance level, the KE value, and the edge compression strength before and after high humidity treatment of Examples 2 to 4 have no significant changes compared with Example 1, indicating that the mildew resistance and water resistance of Examples 2 to 4 are similar to those of Example 1. The reason may be that the waterproof antibacterial agent used in Examples 2 to 4 only changes the amount of raw materials added, and the amount of raw materials added is within the required range, indicating that changing the amount of raw materials added within the required range has no significant effect on the mildew resistance and water resistance of the double-core corrugated paperboard.
[0100] Combining Example 1 and Example 5, it can be seen that the mildew resistance level, the KE value, and the edge compression strength before and after high humidity treatment of Example 5 have no significant changes compared with Example 1, indicating that the mildew resistance and water resistance of Example 5 are similar to those of Example 1. The reason may be that the waterproof antibacterial agent used in Example 5 replaces the hydrophobically modified nano zinc oxide with hydrophobically modified nano titanium dioxide, indicating that the selection of different hydrophobic nano oxides has no significant effect on the mildew resistance and water resistance of the double-core corrugated paperboard.
[0101] Combining Example 6, Example 7 and Example 1, it can be seen that the mildew resistance level of Example 6 and Example 7 is Level II, which is lower than the mildew resistance level of Example 1. The K values of Example 6 and Example 7 before and after being treated in an 85% relative humidity environment are increased compared with Example 1, and the edge compressive strength is slightly decreased after treatment, indicating that the mildew resistance and water resistance of Example 6 and Example 7 are reduced compared with Example 1. The reason may be that the amount of polyhexamethylene biguanide hydrochloride added in the waterproof antibacterial agent used in Example 7 is reduced, and the amount of polyhexamethylene biguanide hydrochloride added in the waterproof antibacterial agent used in Example 6 is increased. When the addition amount of polyhexamethylene biguanide hydrochloride decreases, the antibacterial active substances in the waterproof and antibacterial agent decrease, thereby affecting the waterproof and antibacterial effect of the waterproof and antibacterial agent; when the addition amount of polyhexamethylene biguanide hydrochloride increases, during the reaction with bisphenol A type epoxy resin, the number of connections increases, and the steric hindrance of the epoxy resin becomes larger during the cross-linking process with hydrophobically modified nano zinc oxide, the cross-linking density decreases, and the waterproofness and antibacterial properties of the corrugated cardboard decrease.
[0102] Combining Example 1, Example 8 and Example 9, it can be seen that the mildew resistance level of Example 8 and Example 9 is Level II, which is lower than the mildew resistance level of Example 1. At the same time, the KE values of Example 8 and Example 9 before and after being treated in an 85% relative humidity environment are increased compared with Example 1, and the edge compressive strength after treatment is reduced, indicating that the mildew resistance and water resistance of Example 8 and Example 9 are reduced compared with Example 1. The reason may be that the amount of hydrophobically modified nano zinc oxide added in Example 8 is increased, the nano zinc oxide is easy to agglomerate, the crosslinking density between the nano zinc oxide and the epoxy resin is reduced, and the waterproof and mildew resistance effect of the waterproof antibacterial agent is reduced; the amount of hydrophobically modified nano zinc oxide added in Example 9 is reduced, so the waterproofness of the corrugated board is significantly reduced, and the water absorption of Example 9 is significantly increased.
[0103] Combining Example 1, Example 10 and Example 11, it can be seen that the mildew resistance level of Example 10 is Level II, which is lower than the mildew resistance level of Example 1. At the same time, the KE values of Example 10 and Example 11 before and after being treated in an 85% relative humidity environment are increased compared with Example 1, and the edge compressive strength after treatment is reduced, indicating that the mildew resistance and water resistance of Example 10 and Example 11 are reduced compared with Example 1. The reason may be that the coating amount of the waterproof antibacterial agent in Example 11 is increased, and the coating amount of the waterproof antibacterial agent in Example 10 is reduced. When the coating amount is reduced, the density of the active substance for waterproofing and antibacterial on the surface of the double-core corrugated cardboard is reduced, and the waterproofness and mildew resistance are reduced; when the coating amount is increased, the thickness of the waterproof antibacterial layer formed on the surface of the double-core corrugated cardboard increases, the film layer is easily lost during processing, and the content of the active substance for waterproofing and antibacterial on the surface of the double-core corrugated cardboard is also reduced, and the waterproofness and mildew resistance are reduced accordingly.
[0104] Combining Example 1 and Example 12, it can be seen that the mildew resistance level of Example 12 is Level II, which is lower than the mildew resistance level of Example 1. The value of Example 12 before and after being treated in an 85% relative humidity environment is increased compared with Example 1, and the edge compression strength after treatment is significantly reduced, indicating that the mildew resistance and water resistance of Example 12 are reduced compared with Example 1. The reason may be that the waterproof antibacterial agent in Example 12 does not add a catalyst. In the process of preparing the waterproof antibacterial agent, the silyl ether bond contained in the hydrophobically modified nano metal oxide is difficult to reversibly break and connect without the action of a catalyst, and the dynamic network structure formed between the hydrophobic modified nano metal oxide and the bisphenol A epoxy resin is reduced, thereby reducing the strength of the waterproof antibacterial film layer and the long-term hydrophobic effect, and the edge compression strength of the double-core corrugated board is also reduced.
[0105] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A mildew-proof double-core corrugated paperboard, comprising face paper, lining paper, sandwich paper and two layers of corrugated core paper, characterized in that: The surface of the face paper, the inner paper, the sandwich paper and the two layers of corrugated core paper are coated with a waterproof and antibacterial layer; the waterproof and antibacterial layer comprises the following raw materials in parts by weight: 8 to 11 parts of bisphenol A epoxy resin; 2 to 4 parts of guanidine salt compound; 8 to 12 parts of propylene glycol diglycidyl ether; 1 to 2 parts of curing agent; 4 to 7 parts of hydrophobically modified nano metal oxide; 60 to 80 parts of isopropyl ketone; the hydrophobically modified nano metal oxide is prepared by mixing nano metal oxide with cured polydimethylsiloxane in a mass ratio of 1: (1.5 to 2) The hydrophobically modified nano metal oxide is prepared by vapor precipitation method; the preparation method of the hydrophobically modified nano metal oxide comprises the following steps: uniformly mixing polydimethylaminosiloxane and an organosilicon curing agent at a mass ratio of (11-13):1, and curing at 75-85°C for 2-4h; placing the cured polydimethylsiloxane and the nano metal oxide in a sealed container, and performing constant temperature vapor precipitation at a temperature of 220-240°C in a muffle furnace for 1-2h, and then grinding and sieving to obtain the hydrophobically modified nano metal oxide; In the step S2, a catalyst is added together with the curing agent, and the mass ratio of the catalyst to the bisphenol A epoxy resin is (0.02-0.05):1; the catalyst includes one or more of potassium hydroxide and potassium carbonate; The coating amount of the waterproof and antibacterial layer on the surface of the face paper, the lining paper, the sandwich paper and the two layers of corrugated core paper is 0.2-0.4wt%.
2. The mildew-proof double-core corrugated paperboard according to claim 1, characterized in that: The guanidine salt compound includes one or a combination of polyhexamethylene biguanidine hydrochloride, polyhexamethylene guanidine hydrochloride, polyhexamethylene guanidine stearate, polyhexamethylene guanidine propionate, and polyhexamethylene guanidine phosphate.
3. The mildew-proof double-core corrugated paperboard according to claim 1, characterized in that: The nano metal oxide includes one or more of nano zinc oxide, nano titanium dioxide, and nano aluminum oxide; the organosilicon curing agent includes one or more of methyl triethoxy silane, methyl tripropoxy silane, and benzyl trimethoxy silane.
4. The mildew-proof double-core corrugated paperboard according to claim 1, characterized in that: The preparation method of the waterproof and antibacterial layer is as follows: S1: adding bisphenol A epoxy resin to isopropanol, stirring and mixing, then adding guanidine salt compound aqueous solution, stirring evenly, adding curing agent and propylene glycol diglycidyl ether, stirring and reacting for 3 to 4 hours in a water bath at 40 to 50° C., to obtain a mixed solution; S2: adding hydrophobically modified nano metal oxide, catalyst and curing agent to the mixed solution obtained in S1, and stirring and reacting for 5 to 6 hours in a water bath at 30 to 40° C., to obtain a waterproof and antibacterial agent; S3: coating the waterproof and antibacterial agent obtained in S2 on the surface of the face paper, the lining paper, the sandwich paper and the two layers of corrugated core paper by one or a combination of brushing, spraying, dipping and roller coating.
5. The mildew-proof double-core corrugated paperboard according to claim 1, characterized in that: The curing agent includes one or more of ethylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine.
6. A method for preparing a mildew-proof double-core corrugated paperboard according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1: coating a waterproof antibacterial agent on the surface of corrugated base paper, face paper, lining paper and sandwich paper; S2: rolling the corrugated base paper obtained in S1 through a corrugating roller to obtain corrugated core paper; S3: bonding the corrugated core paper with the face paper, lining paper and sandwich paper by a double-sided corrugator using a starch adhesive, and then cutting the paper to obtain a mildew-proof double-core corrugated paperboard.
Citation Information
Patent Citations
Water-in-oil emulsion sunscreen cosmetic
CN103945824A
Nano-coated waterproof and anti-fouling corrugated carton
CN106882468A
Hydrophobic Y molecular sieve for VOCs adsorption and preparation method thereof
CN110586050A