A method for preparing a magnesium-aluminum composite plate and a magnesium-aluminum composite plate
By pretreating the surface of the magnesium plate and cold spraying metal powder, fixing it on the magnesium plate and forming discontinuous compounds during the hot rolling composite process, the problem of continuous growth of the intermediate phase at the interface of the magnesium-aluminum composite material is solved, and the interface is significantly improved Binding strength.
Patent Information
- Application Number
- CN202310595463.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-24
AI Technical Summary
The continuous growth of the hard and brittle mesophase of the existing magnesium-aluminum composite materials at the interface leads to connection failure and fracture, and it is difficult to fix the metal powder after spraying, resulting in limited interface bonding strength.
After pretreating the surface of the magnesium plate, the metal powder is cold sprayed, fixed on the surface of the magnesium plate, and the powder and the magnesium plate and the aluminum plate form discontinuous intermetallic compounds during the hot rolling composite process to improve the interface bonding strength.
The uniform distribution and metallurgical combination of metal powder were achieved, and the interface bonding strength of the magnesium-aluminum composite plate was significantly improved. The interface bonding strength was measured to reach more than 8.1N/mm, overcoming the problems of powder agglomeration and discontinuous distribution.
Smart Images

Figure CN116623165B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of magnesium-aluminum composite materials, and in particular relates to a preparation method of a magnesium-aluminum composite plate and the magnesium-aluminum composite plate. Background Art
[0002] In the face of the global environmental crisis and energy crisis, the development of lightweight and new energy has received more and more attention. Magnesium and aluminum have become the most effective materials for lightweighting due to their light weight, high specific strength and rich mineral resources. They are widely used in the fields of aerospace, large-scale transportation equipment such as cars, ships and trains, and electronics. At the same time, magnesium alloys have strong electromagnetic shielding effects, good die-casting performance, and high damping, while aluminum alloys have the advantages of corrosion resistance and easy processing. Therefore, by combining the advantages of magnesium and aluminum alloys, magnesium-aluminum composite materials that meet various performance requirements are prepared, thereby achieving comprehensive performance that a single alloy does not have, which has extremely high engineering application value.
[0003] There are many methods for preparing magnesium-aluminum composite materials, such as welding, rolling, extrusion and casting, but they all have a common problem, that is, the Mg at the interface 2 Al 3 and Mg 17 Al 12 The continuous growth of hard and brittle intermediate phases is one of the main reasons for the failure and fracture of magnesium-aluminum composites. Therefore, reducing or eliminating the continuous growth of intermediate phases is of great significance for improving the interfacial bonding performance of magnesium-aluminum composites. There are two main research directions at present: one is to improve the composite process to avoid the generation of continuous intermediate phases; the other is to prevent the mutual diffusion of magnesium and aluminum elements by adding an intermediate layer to avoid the formation of intermediate phases.
[0004] In previous research work, the applicant disclosed a method for improving the interface bonding strength of aluminum-magnesium composite plates in the patent document with application number 201910396674.0. By spraying metal powder on the interface of the aluminum-magnesium composite plate, the growth of intermetallic compounds was effectively prevented, and the bonding strength of the aluminum plate and the magnesium plate was improved. However, in the related art, the metal powder is only sprayed on the surface of the magnesium plate and the aluminum plate, and is not fixed. During the subsequent rolling, the powder is easily agglomerated due to shaking and other reasons, resulting in uneven distribution of powder at the interface of the magnesium-aluminum composite plate, which ultimately limits the improvement of the interface bonding strength of the plate. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a magnesium-aluminum composite plate and a magnesium-aluminum composite plate, by cold spraying metal powder to fix it on the surface of the magnesium plate, the interface bonding strength of the magnesium-aluminum composite plate can be further improved.
[0006] In a first aspect, the present invention provides a method for preparing a magnesium-aluminum composite plate, comprising the following preparation steps:
[0007] S1. Providing a magnesium plate and an aluminum plate, and pre-treating the surfaces of the magnesium plate and the aluminum plate, respectively, wherein the pre-treatment includes at least one of a surface cutting treatment, a surface grinding treatment or a surface cleaning treatment;
[0008] S2. The pretreated surface of the magnesium plate is cold-sprayed with metal powder;
[0009] S3. After stacking the cold-sprayed surface of the magnesium plate and the pre-treated surface of the aluminum plate, hot-rolling and cladding the magnesium plate and the aluminum plate to obtain a magnesium-aluminum composite plate.
[0010] Optionally, in step S2, the metal powder includes at least one of a single metal powder, an alloy powder or a metal composite powder, and the composition of the metal powder includes at least one of copper, nickel, titanium, aluminum, iron, cobalt, chromium, zinc, magnesium, tungsten, molybdenum, manganese or rare earth.
[0011] Optionally, in step S2, the temperature of the cold spraying is 400-900° C., and the pressure is 2-5 MPa.
[0012] Optionally, in step S2, the average particle size of the metal powder is 10-120 μm, and the spraying amount of the metal powder is 30-400 g / m 2 The cold spraying gun moves at a uniform speed along the rolling direction or the casting crystallization direction of the magnesium plate for spraying, and the vertical spacing between adjacent parallel moving paths of the spraying gun is 5 to 15 mm.
[0013] Optionally, in step S3, the stacking is carried out in the form of magnesium plate + aluminum plate or aluminum plate + magnesium plate + aluminum plate, the temperature of the hot rolling composite is 200-500° C., and the total deformation of the hot rolling composite is more than 30%.
[0014] Optionally, in step S2, the metal powder is copper powder or nickel powder, the temperature of the cold spraying is 600-800° C., and the pressure is 3-5 MPa.
[0015] Optionally, in step S2, the average particle size of the copper powder or nickel powder is 10-120 μm, and the spraying amount of the copper powder or nickel powder is 50-360 g / m 2 The cold spraying gun moves at a uniform speed along the rolling direction or the casting crystallization direction of the magnesium plate for spraying, and the vertical spacing between adjacent parallel moving paths of the spraying gun is 5 to 15 mm.
[0016] Optionally, in step S2, the spraying amount of the copper powder or nickel powder is 330-360 g / m 2 The vertical spacing between adjacent parallel moving paths of the spray gun is 8 to 12 mm.
[0017] Optionally, in step S3, the temperature of the hot rolling composite is 400-480°C, and the total rolling deformation is more than 50%; when the metal powder in step S2 is copper powder, the phase structure on the composite surface of the magnesium-aluminum composite plate includes Cu phase, MgCu 2 Phase and AlCu 3 Mutually.
[0018] In a second aspect, the present invention provides a magnesium-aluminum composite plate prepared by the aforementioned method for preparing the magnesium-aluminum composite plate.
[0019] In summary, the present invention has at least one of the following beneficial effects:
[0020] 1. The present invention provides a method for preparing a magnesium-aluminum composite plate, wherein metal powder is cold-sprayed on the composite surface of a pretreated magnesium plate. The metal powder remains in solid powder particles during the cold spraying process, is deformed by high-speed impact on the magnesium plate, and is fixed to the magnesium plate by heat converted from a part of the force, thereby avoiding the movement of the metal powder during the subsequent stacking and hot rolling composite process to cause powder agglomeration. At the same time, the fixation of the metal powder particles prevents the stress it bears during the composite process from being reduced due to its movement, rolling, splashing, etc., so that the metal powder is more easily metallurgically bonded to the interface of the aluminum plate and the magnesium plate, thereby further improving the effect of interface bonding.
[0021] 2. The present invention provides a method for preparing a magnesium-aluminum composite plate, wherein a cold spraying gun moves at a uniform speed along the rolling direction or the casting crystallization direction of the magnesium plate for spraying, and the temperature, pressure, particle size of the metal powder, spraying amount of the metal powder, movement path of the spraying gun, and temperature and deformation of the hot rolling are precisely controlled to make the metal powder evenly dispersed and distributed at intervals on the composite interface of the magnesium plate and the aluminum plate, and react with the magnesium plate and the aluminum plate to form a discontinuous intermetallic compound. In a subsequent embodiment, when the metal powder is copper powder, in addition to the Cu phase, a new intermetallic compound MgCu is detected on the interface of the magnesium-aluminum composite plate. 2 Phase and AlCu 3 The interface bonding strength of the magnesium-aluminum composite plate is increased by 20%. The interface bonding strength can reach more than 5.9 N / mm.
[0022] 3. The present invention provides a method for preparing a magnesium-aluminum composite plate, which uses cold spraying to fix the metal powder with the magnesium plate after spraying, so that the metal powder can be further dispersed and evenly distributed following the rolling deformation of the magnesium plate, thereby significantly increasing the spraying amount of the metal powder. In the subsequent embodiments, the vertical spacing between the adjacent parallel moving paths of the spray gun is 8-12 mm, and the copper powder spraying amount reaches 330-360 g / m2 When the copper powder is still distributed at intervals, it forms a discontinuous distribution of MgCu with the magnesium plate and the aluminum plate. 2 Phase and AlCu 3 phase, so that the interface bonding strength of the magnesium-aluminum composite plate can reach above 8.1N / mm. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the movement path of the spray gun for cold spraying in Example 1.
[0024] Figure 2 (a), (b), and (c) are pictures showing the effects of cold spraying of copper powder on the surfaces of magnesium plates of Example 1, Example 2, and Example 3, respectively.
[0025] Figure 3 (a), (b), and (c) are SEM images of the magnesium plates of Example 1, Example 2, and Example 3 after cold spraying of copper powder; Figure 3 (d), (e), and (f) are SEM images of the magnesium plate surface after peeling of the magnesium-aluminum composite plate of Example 1, Example 2, and Example 3, respectively.
[0026] Figure 4 1 is the XRD diagram of the magnesium plate side and the aluminum plate side of the magnesium-aluminum composite plate after peeling of Example 1, Example 2, and Example 3. DETAILED DESCRIPTION
[0027] The present invention provides a method for preparing a magnesium-aluminum composite plate and a magnesium-aluminum composite plate. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0028] The applicant disclosed a method for improving the interfacial bonding strength of an aluminum-magnesium composite plate in a patent document with application number 201910396674.0, in which metal powder is evenly sprayed on the surface of an aluminum plate or a magnesium plate by air flow spraying, and then the surface of the aluminum plate or the magnesium plate after surface treatment is stacked with the surface of the aluminum plate or the magnesium plate sprayed with metal powder, and the edges are welded by ultrasonic spot welding, and rolled and composited to obtain an aluminum-magnesium composite plate, and metal powder, such as copper powder, can react with aluminum and magnesium elements by diffusion during thermal deformation to generate discontinuously distributed intermetallic compounds Al 2 Cu phase, replacing the continuously distributed Mg 17 Al 12 Mg 2 A l3 The brittle phase and the discontinuous distribution of intermetallic compounds Al 2Cu improves the bonding strength of the aluminum plate and the magnesium plate. The applicant found in the subsequent research process that since the metal powder is only sprayed on the surface of the magnesium plate or the aluminum plate and then composited, it is very easy to cause powder agglomeration or even splashing due to shaking, impact, etc., which makes the powder particles at the interface of the magnesium-aluminum composite plate unevenly distributed, and ultimately the interface strength improvement of the magnesium-aluminum composite plate is limited. Based on this, the applicant has found through research that by cold spraying metal powder, the metal powder can be fixed on the surface of the magnesium plate to prevent the metal powder from moving during the composite process, which is beneficial to improving the uniformity of the distribution of the metal powder on the surface of the magnesium alloy. In addition, in addition to being able to react with the aluminum plate to form new intermetallic compounds, the metal powder can also react with the magnesium plate to form new intermetallic compounds. Since the metal powder is metallurgically bonded to the magnesium plate and the aluminum plate, and the new intermetallic compound is discontinuously and uniformly distributed on the composite surface of the magnesium-aluminum composite plate, the bonding strength of the interface of the magnesium-aluminum composite plate can be further improved. At the same time, the metal powder is fixed to the magnesium plate and can be further dispersed during the rolling process of the magnesium plate, which is beneficial to increase the amount of metal powder spraying while forming discontinuously distributed intermetallic compounds, achieving a better pinning effect, and further improving the bonding effect of the interface of the magnesium-aluminum composite plate.
[0029] The present invention provides a method for preparing a magnesium-aluminum composite plate, comprising the following preparation steps:
[0030] S1. Providing a magnesium plate and an aluminum plate, and pre-treating the surfaces of the magnesium plate and the aluminum plate, respectively, wherein the pre-treatment includes at least one of a surface cutting treatment, a surface grinding treatment or a surface cleaning treatment;
[0031] S2. cold spraying of metal powder on the pretreated surface of the magnesium plate;
[0032] S3. After stacking the cold-sprayed surface of the magnesium plate and the pre-treated surface of the aluminum plate, the magnesium plate and the aluminum plate are hot-rolled and composited to obtain a magnesium-aluminum composite plate.
[0033] In the embodiments of the present invention, the form of the magnesium plate is not particularly limited, and can be a plate, a strip or an ingot. The aluminum plate adopts a deformed plate. The composition of the magnesium plate and the aluminum plate is also not particularly limited, and can be a pure metal, or a binary, ternary or multi-element alloy system. As some specific examples, the magnesium plate (ingot) can be Mg-Mn system, Mg-Al system, Mg-Zn system, Mg-RE system, Mg-Zr system, etc. In some embodiments of the present invention, the magnesium plate can be ZK60, AZ31B, AZ40M, AZ41M, AZ61A, AZ91D, ZK61M, etc.; the aluminum plate can be a deformed plate with alloy grades of 1XXX, 2XXX, 3XXX, 4XXX...9XXX. In some embodiments of the present invention, the aluminum plate can be 1060, 3001, 5083, 6061, etc.
[0034] In step S1, in some embodiments of the present invention, the preprocessing step specifically includes the following steps:
[0035] I. Milling or turning the surface of the cast magnesium plate to remove the surface crystal layer;
[0036] II. Use 80-120 mesh sandpaper to roughly grind the pre-composite surface of the magnesium plate, and then use 180-400 mesh sandpaper for fine grinding. The thickness of a single surface is 0.05-0.2mm, but the total thickness reduction cannot exceed 10% of the initial thickness of the magnesium plate. Sandpaper grinding needs to be carried out along the rolling direction or casting crystallization direction of the magnesium plate;
[0037] III. Acid-base method is used to clean aluminum plates and polished magnesium plates. The cleaning process is divided into five steps: ① alkali cleaning (2-8% NaOH or KOH aqueous solution, cleaning temperature 35-50°C), ② 45-70°C hot water cleaning, ③ acid cleaning (1-3% HCl or HNO 3 ④ Clean with cold water at room temperature; ⑤ Clean with alcohol and blow dry the surface.
[0038] IV. The cleaned aluminum and magnesium plates need to be wrapped with plastic film and vacuum-packed for later use to prevent the cleaned surface from being contaminated or re-oxidized.
[0039] In step S2 of the present invention, the metal powder is at least one of a single metal powder, an alloy powder or a metal composite powder, and the composition of the metal powder includes at least one of copper, nickel, titanium, aluminum, iron, cobalt, chromium, zinc, magnesium, tungsten, molybdenum, manganese or rare earth (such as cerium, yttrium, ytterbium, erbium, etc.). The purity of the metal powder is ≥99%, the shape of the metal powder can be spherical or drop-shaped, and the average particle size of the powder is 10-120μm. In some embodiments of the present invention, the single metal powder is one of copper powder, nickel powder, titanium powder, aluminum powder, iron powder, cobalt powder, chromium powder, zinc powder, magnesium powder, tungsten powder, molybdenum powder, manganese powder or rare earth powder. In some embodiments of the present invention, the alloy powder includes at least one of aluminum-magnesium alloy powder, aluminum-zinc alloy powder, tungsten carbide powder, and high entropy alloy powder (for example, magnesium-aluminum-zinc-copper-manganese, magnesium-aluminum-zinc-copper-silicon, magnesium-aluminum-titanium-iron-nickel, aluminum-copper-zinc-iron-chromium, iron-cobalt-nickel-chromium-manganese, and iron-cobalt-nickel-chromium). Among them, the metal composite powder is a powder prepared by mechanically mixing two or more metal powders. The mechanical mixing method can adopt the conventional ball milling mixing in the field. In some embodiments of the present invention, the metal composite powder includes: copper-nickel or copper-zinc composite powder, wherein the copper powder accounts for 1-99% by mass; copper-magnesium or copper-aluminum composite powder, wherein the copper powder accounts for 40-99% by mass; nickel-magnesium or nickel-aluminum composite powder, wherein the nickel powder accounts for 30-99% by mass; nickel-cobalt or nickel-iron composite powder, wherein the nickel powder accounts for 2-99% by mass; copper-nickel-zinc or copper-nickel-cobalt composite powder, wherein the nickel + zinc or nickel + cobalt accounts for 1-99% by mass, and the mass proportion of a single metal is not less than 0.5%.
[0040] In the present invention, the cold spraying in step S2 refers to the use of high-pressure gas, such as nitrogen, helium, etc., at a relatively low temperature to accelerate the metal powder to several times the speed of sound, and after colliding with the magnesium plate in a solid form, it produces severe plastic deformation and is deposited and fixed on the magnesium plate. The cold spraying process is automatically carried out by a cold spraying system, which is mainly composed of a powder feeding system, a cold spray gun system, a high-pressure gas source, a gas temperature control system, a gas regulation control system, etc. Since it belongs to the conventional structure in the field, it will not be repeated here. In some embodiments of the present invention, the temperature of cold spraying is 400-900°C, preferably 600-800°C, and further preferably 700-800°C; the pressure of cold spraying is 2-5Mpa, preferably 3-5MPa; the spraying amount of metal powder is 30-400g / m 2 The relationship between the spraying amount of metal powder and the density ρ of the metal powder is: ①ρ≤5g / cm 3 The metal powder cold spraying amount is 30-200g / m 2 , preferably 100 to 200 g / m 2 ;②5g / cm 3 <ρ≤9g / cm 3The metal powder cold spraying amount is 50-360g / m 2 , preferably 150 to 360 g / m 2 , more preferably 330 to 360 g / m 2 ; ③ρ>9g / cm 3 The metal powder cold spraying amount is 90-400g / m 2 , preferably 200 to 400 g / m 2 , more preferably 350 to 400 g / m 2 The cold spraying gun moves at a constant speed along the rolling direction or casting crystallization direction of the magnesium plate for spraying, and the vertical spacing between adjacent parallel moving paths of the spray gun is 5 to 15 mm, preferably 8 to 12 mm, and more preferably 10 to 11 mm.
[0041] In step S3, the stacking is carried out by magnesium plate + aluminum plate or aluminum plate + magnesium plate + aluminum plate, the hot rolling composite temperature is 200-500°C, preferably 400-480°C; the total deformation of the hot rolling composite is more than 30%, preferably more than 50%. In some embodiments of the present invention, the correlation between the hot rolling process and the total thickness of the aluminum plate + magnesium plate is: the total thickness is less than or equal to 8mm, and can be rolled in a single pass or in two passes, and the rolling temperature is 400-480°C. For single-pass rolling, the holding time is 15-20min, and the rolling deformation is 50-70%. For two-pass rolling, the deformation of the first pass is 25-40%, the intermediate holding temperature is 400-460°C, the intermediate holding time is 5-10min, the deformation of the second pass is 40-70%, and the total deformation is greater than 60%. Before the second rolling, the edge cracks generated in the first pass of the magnesium-aluminum composite plate must be removed, and the shear width is 50-100mm; the total thickness is greater than 8mm It must be rolled in multiple passes, with a rolling temperature of 420-500℃, a holding time of 15-40min for the first pass, a deformation of 25-30%, a deformation of 40-50% for the intermediate rolling pass, and a deformation of 50-70% for the last pass. The intermediate holding temperature is 400-460℃, and the holding time is 5-10min. Before each rolling pass, the edge cracks on the magnesium-aluminum composite plate must be removed, and the shearing width is 50-100mm. In addition, the first composite method can use asynchronous rolling, and the ratio of the aluminum side roller speed to the magnesium side roller speed is 1:1.2-1.5. The second composite method can use synchronous rolling, and the speeds of the two rollers are consistent.
[0042] By precisely controlling the temperature, pressure, particle size of the metal powder, the spraying amount of the metal powder, the moving path of the spray gun, and the temperature and deformation of the hot rolling, the metal powder is evenly dispersed and spaced on the composite interface of the magnesium plate and the aluminum plate, and reacts with the magnesium plate and the aluminum plate to form a discontinuous phase. In some embodiments of the present invention, when the metal powder is copper powder, in addition to the Cu phase, a new intermetallic compound MgCu is detected on the bonding interface of the magnesium-aluminum composite plate. 2 Phase and AlCu 3 phase, overcoming the defect that copper powder is not easy to react with magnesium plate to form metallurgical bonding, and MgCu 2 Phase and AlCu 3 The phase has low brittleness and is distributed discontinuously on the interface, which further improves the "pinning" effect of the metal particles. In addition, the use of cold spraying allows the metal powder to be fixedly bonded to the magnesium plate after spraying, so that the metal powder can be further dispersed evenly following the rolling deformation of the magnesium plate, thereby significantly increasing the amount of metal powder sprayed to further improve the interface bonding effect.
[0043] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0044] Example 1
[0045] A method for preparing a magnesium-aluminum composite plate comprises the following preparation steps:
[0046] S1. Provide a 4.5mm×100mm×200mm (thickness×width×length) ZK60 magnesium plate and a 1.5mm×100mm×200mm (thickness×width×length) 5083 aluminum plate as the substrate. The magnesium plate is a rolled plate with the rolling direction along its length. Pre-treat the composite surface of the magnesium plate and the aluminum plate respectively, including the following steps: use 80-mesh sandpaper to grind along the length direction of the magnesium plate, and then use 180-mesh sandpaper for fine grinding to grind off 0.1mm of thickness; then use the acid-base method to clean the aluminum plate and the polished magnesium plate. The cleaning process is divided into five steps: ① alkali cleaning (3% NaOH aqueous solution, cleaning temperature 50℃), ② 70℃ hot water cleaning, ③ acid cleaning (1% HCl aqueous solution, room temperature cleaning), ④ room temperature cold water cleaning; ⑤ alcohol cleaning and drying the surface. The cleaned aluminum plate and magnesium plate are wrapped with plastic film and vacuum packaged for standby use.
[0047] S2. Use a cold spray system to cold spray copper powder on the pre-treated surface of the magnesium plate, and symmetrically cold spray copper powder with an average particle size of 50μm on the upper and lower surfaces of the magnesium plate, and the process parameters are completely consistent. The amount of copper powder cold sprayed on one side of the magnesium plate is 89g / m 2The cold spraying temperature is 750℃, the nitrogen pressure is 4MPa, and the movement path of the spray gun for spraying is as follows Figure 1 As shown in the figure, the spray gun moves at a constant speed along the rolling direction of the magnesium plate, that is, the length direction of the magnesium plate, and the vertical spacing between adjacent parallel moving paths of the spray gun is 10-11 mm. The distribution of copper powder on the surface of the magnesium plate after cold spraying is shown in the figure. Figure 2 As shown in (a), the copper powder is evenly distributed on the surface of the magnesium plate along the spraying path. Figure 3 (a) It can be further seen that the copper powder particles are distributed more evenly on the magnesium plate.
[0048] S3. After stacking the cold-sprayed surface of the magnesium plate and the pre-treated surface of the aluminum plate, hot-roll the magnesium plate and the aluminum plate to obtain a magnesium-aluminum composite plate. The stacking of this embodiment adopts the method of aluminum plate + magnesium plate + aluminum plate, and is fixed by rivets. Three rivets are fixed and connected at about 10mm from the front end of the three-layer plate, which plays a role in fixing the three-layer plate so that it does not dislocate when it is just bitten into the roller gap, and loses its function after successful biting. The hot-rolled composite adopts synchronous single-pass rolling, the rolling roller speed is 2m / min, the rolling temperature is 450℃, the insulation time is 20min, and the rolling deformation is 56%.
[0049] The prepared magnesium-aluminum composite plate was subjected to a peel strength test. A 10*80mm magnesium-aluminum composite plate was sampled and peeled off 25mm. One of the two peeled parts was flipped 180°. The two peeled parts were clamped and continued to be peeled off using a tensile testing machine until they were completely peeled off. The peel strength, i.e., the interface bonding strength of the magnesium-aluminum composite plate, was measured to be 5.9N / mm. After the magnesium-aluminum composite plate was peeled off, the microscopic morphology of the composite surface on one side of the magnesium plate was as follows: Figure 3 As shown in (d), no traces of copper powder particles rolling were found, and the copper powder particles were evenly distributed without agglomeration. Figure 3 (a) By comparison, it can be seen that after rolling, the spacing between the copper powders increases significantly. Since the cold-sprayed copper powders are not connected to each other, they can be separated by following the rolling deformation of the magnesium plate, which is conducive to promoting the uniform distribution of the copper powder on the surface of the magnesium plate. After the magnesium-aluminum composite plate is peeled off, XRD phase analysis is performed on the magnesium plate side and the aluminum plate side, respectively. Figure 4 As shown in the figure, in addition to Mg phase and Cu phase, Al phase was also detected on the surface of the magnesium plate side. 2 Cu 3 In addition to Al and Cu phases, MgCu was also detected on the composite surface of the aluminum plate. 2 phase, indicating that new intermetallic compounds MgCu and MgCu were formed during the rolling process. 2 Phase and Al 2 Cu 3Phase, the copper powder and the magnesium plate and aluminum plate are metallurgically bonded, rather than simply physically sandwiched in the middle. The metallurgical bonding can prevent the copper powder from becoming a stress concentration source for fracture. During the peeling process of the magnesium-aluminum composite plate, the fracture on the magnesium plate side occurs at the MgCu 2 The fracture of the aluminum plate occurred at the interface between the Al phase and the Mg matrix phase. 2 Cu 3 At the interface between the Al matrix phase and the new metal compound Al 2 Cu 3 Phase and MgCu 2 The phase plays a "pinning and rolling" role, which improves the interface bonding strength of the magnesium-aluminum composite plate.
[0050] Example 2
[0051] The difference between Example 2 and Example 1 is that, in step S2 of Example 2, the single-side spraying amount of cold-sprayed copper powder on the magnesium plate is 178 g / m 2 The remaining preparation steps are the same as those in Example 1. Figure 2 (b) is the distribution diagram of copper powder on the surface of magnesium plate. The copper powder is evenly distributed on the surface of magnesium plate along the spraying path. Figure 3 (b) It can be seen that the copper powder particles are distributed more evenly on the magnesium plate, and compared with Figure 3 (a), the number of copper powder particles on the surface of the magnesium plate increased significantly. The same peel strength test as in Example 1 was used to measure the interface bonding strength of the magnesium-aluminum composite plate to be 6.4 N / mm. After the magnesium-aluminum composite plate was peeled off, the SEM image of the composite surface on the magnesium plate side was as follows: Figure 3 As shown in (e), no traces of copper powder particles rolling were found, and the copper powder particles were evenly distributed without agglomeration. Figure 3 (b) By comparison, it can be seen that after rolling, the distance between the copper powders increases, and the uniformity of the copper powders on the entire magnesium plate surface increases. After the magnesium-aluminum composite plate is peeled off, the surface of the magnesium plate side and the surface of the aluminum plate side are respectively subjected to XRD phase analysis, such as Figure 4 As shown in the figure, in addition to Mg phase and Cu phase, Al phase was also detected on the surface of the magnesium plate side. 2 Cu 3 In addition to Al and Cu phases, MgCu was also detected on the composite surface of the aluminum plate. 2 phase, indicating that new intermetallic compounds MgCu and MgCu were formed during the rolling process. 2 Phase and Al 2 Cu 3 Phase, the copper powder and the magnesium plate and aluminum plate are metallurgically bonded, rather than simply physically sandwiched in the middle. The metallurgical bonding can prevent the copper powder from becoming a stress concentration source for fracture. During the peeling process of the magnesium-aluminum composite plate, the fracture on the magnesium plate side occurs at the MgCu2 The fracture of the aluminum plate occurred at the interface between the Al phase and the Mg matrix phase. 2 Cu 3 At the interface between the Al matrix phase and the new metal compound Al 2 Cu 3 Phase and MgCu 2 The phase plays a "pinning and rolling" role, which improves the interface bonding strength of the magnesium-aluminum composite plate.
[0052] Example 3
[0053] The difference between Example 3 and Example 1 is that, in step S2 of Example 3, the single-side spraying amount of cold-sprayed copper powder on the magnesium plate is 356 g / m 2 The remaining preparation steps are the same as those in Example 1. Figure 2 (c) is the distribution diagram of copper powder on the surface of magnesium plate. The copper powder is evenly distributed on the surface of magnesium plate along the spraying path. Figure 3 (c) It can be seen that the copper powder particles are distributed more evenly on the magnesium plate, and compared with Figure 3 (a), the number of copper powder particles on the surface of the magnesium plate increased significantly. The same peel strength test as in Example 1 was used to measure the interface bonding strength of the magnesium-aluminum composite plate to be 8.1 N / mm. After the magnesium-aluminum composite plate was peeled off, the SEM image of the side surface of the magnesium plate was as follows: Figure 3 As shown in (f), no traces of copper powder particles rolling were found, and the copper powder particles were evenly distributed without agglomeration. Figure 3 (c) By comparison, it can be seen that after rolling, the distance between the copper powders increases, and the uniformity of the copper powder on the entire magnesium plate composite surface is significantly increased. After the magnesium-aluminum composite plate is peeled off, the surface of the magnesium plate side and the surface of the aluminum plate side are respectively subjected to XRD phase analysis, such as Figure 4 As shown in the figure, in addition to Mg phase and Cu phase, Al phase was also detected on the surface of the magnesium plate side. 2 Cu 3 In addition to Al phase and Cu phase, MgCu was also detected on the surface of the aluminum plate. 2 phase, indicating that new intermetallic compounds MgCu and MgCu were formed during the rolling process. 2 Phase and Al 2 Cu 3 Phase, the copper powder and the magnesium plate and aluminum plate are metallurgically bonded, rather than simply physically sandwiched in the middle. The metallurgical bonding can prevent the copper powder from becoming a stress concentration source for fracture. During the peeling process of the magnesium-aluminum composite plate, the fracture on the magnesium plate side occurs at the MgCu 2 The fracture of the aluminum plate occurred at the interface between the Al phase and the Mg matrix phase. 2 Cu 3 At the interface between the Al matrix phase and the new metal compound Al2 Cu 3 Phase and MgCu 2 The phase plays a "pinning and rolling" role, which improves the interface bonding strength of the magnesium-aluminum composite plate.
[0054] Example 4
[0055] The difference between Example 4 and Example 3 is that, in step S2 of Example 4, nickel powder of equal mass is used instead of copper powder for cold spraying of the magnesium plate, the cold spraying temperature is 750°C, and the remaining preparation steps are the same as those in Example 1, and a magnesium-aluminum composite plate is prepared. It is measured that the magnesium-aluminum composite plate has good interface composite strength.
[0056] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a magnesium-aluminum composite plate, It is characterized in that The method comprises the following preparation steps: S1. Providing a magnesium plate and an aluminum plate, and pre-treating the surfaces of the magnesium plate and the aluminum plate, respectively, wherein the pre-treatment includes at least one of a surface cutting treatment, a surface grinding treatment or a surface cleaning treatment; S2. The pretreated surface of the magnesium plate is cold-sprayed with metal powder; S3. After stacking the cold-sprayed surface of the magnesium plate and the pre-treated surface of the aluminum plate, the magnesium plate and the aluminum plate are hot-rolled to obtain a magnesium-aluminum composite plate; the metal powder is uniformly dispersed and distributed at intervals on the composite interface of the magnesium plate and the aluminum plate, and reacts with the magnesium plate and the aluminum plate to form a discontinuous intermetallic compound; Wherein, in step S2, the metal powder includes at least one of a single metal powder, an alloy powder or a metal composite powder, and the composition of the metal powder includes at least one of copper, nickel, titanium, aluminum, iron, cobalt, chromium, zinc, magnesium, tungsten, molybdenum, manganese or rare earth; the temperature of the cold spraying is 400-900°C, and the pressure is 2-5Mpa; the average particle size of the metal powder is 10-120μm, and the spraying amount of the metal powder is 30-400g / m 2 The cold spraying gun moves at a uniform speed along the rolling direction or the casting crystallization direction of the magnesium plate for spraying, and the vertical spacing between adjacent parallel moving paths of the spray gun is 5-15 mm.
2. The method for preparing the magnesium-aluminum composite plate according to claim 1, It is characterized in that In step S3, the stacking is carried out in the form of magnesium plate + aluminum plate or aluminum plate + magnesium plate + aluminum plate, the temperature of the hot rolling composite is 200-500° C., and the total deformation of the hot rolling composite is more than 30%.
3. The method for preparing the magnesium-aluminum composite plate according to claim 1, It is characterized in that In step S2, the metal powder is copper powder or nickel powder, the temperature of the cold spraying is 600-800°C, and the pressure is 3-5Mpa.
4. The method for preparing the magnesium-aluminum composite plate according to claim 3, It is characterized in that In step S2, the average particle size of the copper powder or nickel powder is 10-120 μm, and the spraying amount of the copper powder or nickel powder is 50-360 g / m 2 The cold spraying gun moves at a uniform speed along the rolling direction or the casting crystallization direction of the magnesium plate for spraying, and the vertical spacing between adjacent parallel moving paths of the spray gun is 5-15 mm.
5. The method for preparing the magnesium-aluminum composite plate according to claim 4, It is characterized in that In step S2, the spraying amount of the copper powder or nickel powder is 330-360g / m 2 The vertical spacing between adjacent parallel moving paths of the spray gun is 8~12mm.
6. The method for preparing the magnesium-aluminum composite plate according to claim 3, It is characterized in that In step S3, the hot rolling composite temperature is 400-480°C, and the total rolling deformation is more than 50%; when the metal powder in step S2 is copper powder, the phase structure on the composite surface of the magnesium-aluminum composite plate includes Cu phase, MgCu 2 Phase and AlCu 3 Mutually.
7. A magnesium-aluminum composite plate prepared by the method for preparing a magnesium-aluminum composite plate according to any one of claims 1 to 6.