A transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst

By loading transition metals on zirconium phosphate carriers, an efficient bio-oil hydrodeoxygenation catalyst is prepared, which solves the problems of low bio-oil hydrodeoxygenation activity and high cost, achieves high conversion rate and high selectivity, and reduces production costs. .

CN116651476BActive Publication Date: 2024-10-15FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310854691.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-13
Publication Date
2024-10-15
Estimated Expiration
2043-07-13

AI Technical Summary

Technical Problem

The bio-oil hydrodeoxygenation catalyst has low activity, poor stability, and high cost of precious metal catalysts, making it difficult to achieve efficient hydrodeoxygenation when upgrading bio-oil.

Method used

Zirconium phosphate is used as a carrier to support transition metals (such as Fe, Co, Ni, Cu) to prepare oil hydrodeoxygenation catalysts through the incipient wetness impregnation method. The Zr/P ratio is adjusted to increase the acid strength, and the supported transition metals are used to improve catalytic activity and reduce costs. .

Benefits of technology

The bio-oil conversion rate is over 95%, the hydrocarbon selectivity is as high as 90%, the catalyst cost is reduced, the preparation process is simplified, and the use of precious metals is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst, a preparation method and an application thereof, and belongs to the technical field of bio-oil hydrodeoxygenation catalysts. Zirconium phosphate and a transition metal salt are used as raw materials, and a transition metal-loaded zirconium phosphate catalyst is obtained by initial wetness impregnation. The bio-oil conversion rate of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst obtained by the invention exceeds 95%, and the hydrocarbon selectivity is more than 90%, realizing the hydrodeoxygenation process of bio-oils such as palm oil and waste oils under mild conditions, and the active components of the catalyst have good dispersion and repeated cycle performance, and the application prospect is broad.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bio-oil hydrodeoxygenation catalysts, and in particular relates to a transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst, a preparation method and an application thereof. Background Art

[0002] With the rapid development of economy, the global consumption and demand for energy are increasing day by day. At present, the world's main energy resources are still fossil resources such as coal, natural gas and oil. However, the formation cycle of fossil resources is extremely long and the formation conditions are extremely harsh, so they are regarded as non-renewable resources. At the same time, the energy shortage caused by excessive consumption of fossil resources and the environmental problems caused by greenhouse gases emitted by their combustion seriously affect the development of human society. In order to solve the current energy crisis, the world's major powers have stepped up their exploration of renewable energy such as nuclear energy, solar energy, wind energy, tidal energy, geothermal energy, etc.

[0003] Biomass is a renewable organic carbon source, among which bio-oil has attracted extensive attention because of its carbon chain structure similar to petrochemical diesel, low cost, good renewability, and good environmental protection due to the fact that it does not contain nitrogen / sulfur. However, oil contains a large number of ester groups, carboxyl groups and unsaturated bonds. Direct use as fuel has problems such as low calorific value, high viscosity, poor stability, poor fluidity and low energy density, so it needs to be upgraded to improve its quality. Among them, the second-generation biodiesel produced by using bio-oil as raw material through hydrodeoxygenation technology has high calorific value and good fluidity, and can be mixed with petrochemical diesel in any proportion. It is an ideal liquid fuel. The core of the second-generation biodiesel is the development and research of efficient hydrodeoxygenation catalysts. Summary of the invention

[0004] The purpose of the present invention is to provide a bio-oil hydrodeoxygenation catalyst to solve the problems of low activity, poor stability and high cost of precious metal catalysts in the current bio-oil hydrodeoxygenation catalysts. The present invention uses zirconium phosphate as a carrier to load transition metal synthetic oil hydrodeoxygenation catalysts, the conversion rate of bio-oil exceeds 95%, and the hydrocarbon selectivity is as high as 90% or more.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst is prepared from zirconium phosphate and a transition metal salt by an incipient wetness impregnation method.

[0007] The zirconium phosphate has a zirconium-to-phosphorus ratio of 0.25 to 2.00.

[0008] The transition metal salt is one of acetates such as Fe, Co, Ni, Cu, etc.

[0009] The preparation method of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst comprises the following steps:

[0010] 1) Dissolve zirconium salt and ammonium salt in deionized water respectively, and after constant volume, mix and react in a beaker to obtain a solid acid suspension;

[0011] 2) After filtering the above suspension, the filter residue is placed in an oven for drying to obtain a white solid;

[0012] 3) Grinding and sieving the obtained solid;

[0013] 4) Place the sieved solid in a muffle furnace for roasting;

[0014] 5) stirring the calcined solid and the transition metal salt in deionized water;

[0015] 6) The obtained mixed solution is subjected to rotary evaporation to remove the solvent and then dried to obtain a solid.

[0016] 7) The obtained solid is placed in a muffle furnace for calcination.

[0017] 8) The obtained solid is placed in a tube furnace for reduction and passivation. The solid obtained after passivation is a transition metal-supported zirconium phosphate grease hydrodeoxygenation catalyst.

[0018] Among them, the loading amount of the transition metal used is 5~20%.

[0019] The application of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst in the hydrodeoxygenation reaction of bio-oil: the amount of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst used is 1-10% of the weight of the processed biomass oil, the reaction temperature for hydrodeoxygenation is 280-400°C, the hydrogen pressure is 2-6 MPa, and the reaction time is 2-10 h.

[0020] The beneficial effects of the present invention are:

[0021] (1) The acid strength of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst prepared by the present invention is easy to control, that is, by adjusting the Zr / P ratio, it is possible to avoid the ester cracking reaction that is aggravated by excessive acidity to produce small molecular byproducts.

[0022] (2) The zirconium phosphate solid acid prepared by the present invention is a multi-metal oxide formed by the Zr central atom and the P coordinating atom bridged by an oxygen atom, which has acidity and redox properties. The loaded transition metal is used as the hydrogenation active component, and the acidity of the zirconium phosphate is mainly used to improve the deoxidation performance of the catalyst.

[0023] (3) The preparation method of the present invention is simple, does not involve precious metals, has a relatively low cost, and exhibits high activity and alkane selectivity in the hydrodeoxygenation of bio-oils, among which the total selectivity of pentadecane / hexadecane is as high as 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The XRD spectra of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst obtained in Examples 1 to 3 are shown. DETAILED DESCRIPTION

[0025] In order to make the contents of the present invention easier to understand, the technical solutions of the present invention are further clearly and completely described below in conjunction with the accompanying drawings and specific implementation methods. The described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0026] Example 1

[0027] A method for preparing a transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst comprises the following steps:

[0028] (1) Weigh 1 mol NH4H2PO4 in a beaker and dilute to 4 mol / L with deionized water. This is called solution A. Weigh 1 mol ZrOCl2·8H2O in a beaker and dilute to 4 mol / L with deionized water. This is called solution B.

[0029] (2) Add equal volumes of solution A and solution B from step (1) into a beaker and stir at room temperature for 1 h and at 80 °C for 3 h.

[0030] (3) Filter and wash the suspension in step (2).

[0031] (4) The solid filtered in step (3) was placed in an oven at 100°C and dried for 12 h. The dried solid was ground and sieved.

[0032] (5) The solid that has passed the sieve in step (4) is placed in a muffle furnace and heated to 550°C at 5°C / min for 12 h. The resulting solid is recorded as ZrPO x (1).

[0033] (6) The solid (1.90 g) obtained by calcining in step (5) and 0.43 g of nickel acetate tetrahydrate were placed in a flask and stirred for 12 h.

[0034] (7) placing the mixed solution obtained in step (6) in a rotary evaporator at 80°C to remove the solvent;

[0035] (8) The solid obtained in step (7) was placed in a muffle furnace and calcined at 450 °C at a rate of 5 °C / min for 3 h.

[0036] (9) The sample obtained in step (8) was placed in a tube furnace, reduced at 550 °C at 5 °C / min for 3 h in a 10 vol% H2 / Ar atmosphere, and passivated at room temperature for 12 h in 2 vol% O2 / He. The nickel-loaded zirconium phosphate catalyst was obtained, denoted as 5Ni / ZrPO x (1).

[0037] Example 2

[0038] A method for preparing a transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst comprises the following steps:

[0039] (1) Weigh 1 mol NH4H2PO4 in a beaker and dilute to 4 mol / L with deionized water. This is called solution A. Weigh 1 mol ZrOCl2·8H2O in a beaker and dilute to 4 mol / L with deionized water. This is called solution B.

[0040] (2) Add equal volumes of solution A and solution B from step (1) into a beaker and stir at room temperature for 1 h and at 80 °C for 3 h.

[0041] (3) Filter and wash the suspension in step (2).

[0042] (4) The solid filtered in step (3) was placed in an oven at 100°C and dried for 12 h. The dried solid was ground and sieved.

[0043] (5) The solid that has passed the sieve in step (4) is placed in a muffle furnace and heated to 550°C at 5°C / min for 12 h. The resulting solid is recorded as ZrPO x (1).

[0044] (6) The solid (1.80 g) obtained by calcining in step (5) and 0.86 g of nickel acetate tetrahydrate were placed in a flask and stirred for 12 h.

[0045] (7) placing the mixed solution obtained in step (6) in a rotary evaporator at 80°C to remove the solvent;

[0046] (8) The solid obtained in step (7) was placed in a muffle furnace and calcined at 450 °C at a rate of 5 °C / min for 3 h.

[0047] (9) The sample obtained in step (8) was placed in a tube furnace, reduced at 550 °C at 5 °C / min for 3 h in a 10 vol% H2 / Ar atmosphere, and passivated at room temperature for 12 h in a 2 vol% O2 / He atmosphere. The nickel-loaded zirconium phosphate catalyst was obtained, denoted as 10Ni / ZrPO x (1).

[0048] Example 3

[0049] A method for preparing a transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst comprises the following steps:

[0050] (1) Weigh 1 mol NH4H2PO4 in a beaker and dilute to 4 mol / L with deionized water. This is called solution A. Weigh 1 mol ZrOCl2·8H2O in a beaker and dilute to 4 mol / L with deionized water. This is called solution B.

[0051] (2) Add equal volumes of solution A and solution B from step (1) into a beaker and stir at room temperature for 1 h and at 80 °C for 3 h.

[0052] (3) Filter and wash the suspension in step (2).

[0053] (4) The solid filtered in step (3) was placed in an oven at 100°C and dried for 12 h. The dried solid was ground and sieved.

[0054] (5) The solid that has passed the sieve in step (4) is placed in a muffle furnace and heated to 550°C at 5°C / min for 12 h. The resulting solid is recorded as ZrPO x (1).

[0055] (6) The solid (1.60 g) obtained by calcining in step (5) and 1.72 g of nickel acetate tetrahydrate were placed in a flask and stirred for 12 h.

[0056] (7) placing the mixed solution obtained in step (6) in a rotary evaporator at 80°C to remove the solvent;

[0057] (8) The solid obtained in step (7) was placed in a muffle furnace and calcined at 450 °C at a rate of 5 °C / min for 3 h.

[0058] (9) The sample obtained in step (8) was placed in a tube furnace, reduced at 550 °C at 5 °C / min for 3 h in a 10 vol% H2 / Ar atmosphere, and passivated at room temperature for 12 h in 2 vol% O2 / He. The nickel-loaded zirconium phosphate catalyst was obtained, denoted as 20Ni / ZrPO x (1).

[0059] Example 4

[0060] A method for preparing a transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst comprises the following steps:

[0061] (1) Weigh 2 mol NH4H2PO4 into a beaker and dilute to 8 mol / L with deionized water. This is called solution A. Weigh 1 mol ZrOCl2·8H2O into a beaker and dilute to 4 mol / L with deionized water. This is called solution B.

[0062] (2) Add equal volumes of solution A and solution B from step (1) into a beaker and stir at room temperature for 1 h and at 80 °C for 3 h.

[0063] (3) Filter and wash the suspension in step (2).

[0064] (4) The solid filtered in step (3) was placed in an oven at 100°C and dried for 12 h. The dried solid was ground and sieved.

[0065] (5) The solid that has passed the sieve in step (4) is placed in a muffle furnace and heated to 550°C at 5°C / min for 12 h. The resulting solid is recorded as ZrPO x (0.5).

[0066] (6) The solid (1.80 g) obtained by calcining in step (5) and 0.86 g of nickel acetate tetrahydrate were placed in a flask and stirred for 12 h.

[0067] (7) placing the mixed solution obtained in step (6) in a rotary evaporator at 80°C to remove the solvent;

[0068] (8) The solid obtained in step (7) was placed in a muffle furnace and calcined at 450 °C at a rate of 5 °C / min for 3 h.

[0069] (9) The sample obtained in step (8) was placed in a tube furnace, reduced at 550 °C at 5 °C / min for 3 h in a 10 vol% H2 / Ar atmosphere, and passivated at room temperature for 12 h in a 2 vol% O2 / He atmosphere. The nickel-loaded zirconium phosphate catalyst was obtained, denoted as 10Ni / ZrPO x (0.5).

[0070] Example 5

[0071] A method for preparing a transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst comprises the following steps:

[0072] (1) Weigh 1 mol NH4H2PO4 into a beaker and dilute to 4 mol / L with deionized water. This is called solution A. Weigh 2 mol ZrOCl2·8H2O into a beaker and dilute to 8 mol / L with deionized water. This is called solution B.

[0073] (2) Add equal volumes of solution A and solution B from step (1) into a beaker and stir at room temperature for 1 h and at 80 °C for 3 h.

[0074] (3) Filter and wash the suspension in step (2).

[0075] (4) The solid filtered in step (3) was placed in an oven at 100°C and dried for 12 h. The dried solid was ground and sieved.

[0076] (5) The solid that has passed the sieve in step (4) is placed in a muffle furnace and heated to 550°C at 5°C / min for 12 h. The resulting solid is recorded as ZrPO x (2).

[0077] (6) The solid (1.80 g) obtained by calcining in step (5) and 0.86 g of nickel acetate tetrahydrate were placed in a flask and stirred for 12 h.

[0078] (7) placing the mixed solution obtained in step (6) in a rotary evaporator at 80°C to remove the solvent;

[0079] (8) The solid obtained in step (7) was placed in a muffle furnace and calcined at 450 °C at a rate of 5 °C / min for 3 h.

[0080] (9) The sample obtained in step (8) was placed in a tube furnace, reduced at 550 °C at 5 °C / min for 3 h in a 10 vol% H2 / Ar atmosphere, and passivated at room temperature for 12 h in a 2 vol% O2 / He atmosphere. The nickel-loaded zirconium phosphate catalyst was obtained, denoted as 10Ni / ZrPO x (2).

[0081] Example 6

[0082] A method for preparing a transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst comprises the following steps:

[0083] (1) Weigh 1 mol NH4H2PO4 into a beaker and dilute to 4 mol / L with deionized water. This is called solution A. Weigh 4 mol ZrOCl2·8H2O into a beaker and dilute to 16 mol / L with deionized water. This is called solution B.

[0084] (2) Add equal volumes of solution A and solution B from step (1) into a beaker and stir at room temperature for 1 h and at 80 °C for 3 h.

[0085] (3) Filter and wash the suspension in step (2).

[0086] (4) The solid filtered in step (3) was placed in an oven at 100°C and dried for 12 h. The dried solid was ground and sieved.

[0087] (5) The solid that has passed the sieve in step (4) is placed in a muffle furnace and heated to 550°C at 5°C / min for 12 h. The resulting solid is recorded as ZrPO x (4).

[0088] (6) The solid (1.80 g) obtained by calcining in step (5) and 0.86 g of nickel acetate tetrahydrate were placed in a flask and stirred for 12 h.

[0089] (7) placing the mixed solution obtained in step (6) in a rotary evaporator at 80°C to remove the solvent;

[0090] (8) The solid obtained in step (7) was placed in a muffle furnace and calcined at 450 °C at a rate of 5 °C / min for 3 h.

[0091] (9) The sample obtained in step (8) was placed in a tube furnace, reduced at 550 °C at 5 °C / min for 3 h in a 10 vol% H2 / Ar atmosphere, and passivated at room temperature for 12 h in a 2 vol% O2 / He atmosphere. The nickel-loaded zirconium phosphate catalyst was obtained, denoted as 10Ni / ZrPO x (4).

[0092] from Figure 1 It can be seen from the XRD spectrum that there is an obvious nickel signal peak in the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst sample, and with the increase of metal content, the nickel signal peak becomes more and more obvious.

[0093] Test on the Hydrodeoxygenation Activity of Bio-oil in Suspended Bed

[0094] The transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst prepared in the example was tested for oil hydrodeoxygenation activity, and the specific operation was as follows: methyl palmitate was used as the bio-oil raw material, and its addition amount was 50.0 g, the addition amount of the catalyst was 2.0 g (addition amount was 4 wt%), the initial hydrogen pressure was 6 MPa, the temperature was raised to 360 ° C at a rate of 5 ° C / min for hydrodeoxygenation reaction, and the reaction time was 4 h. The test results are shown in Table 1.

[0095]

[0096] It can be seen from Table 1 that the introduction of nickel significantly improves the oil hydrodeoxygenation performance. With the increase of the loading amount, the catalytic activity shows a trend of first increasing and then decreasing, and the activity is highest when the nickel loading amount is 10%.

[0097]

[0098] It can be seen from Table 2 that changing the zirconium-phosphorus ratio has a great influence on the hydrodeoxygenation performance of the catalyst. When the zirconium-phosphorus ratio is 1, the conversion rate of methyl palmitate is 97.1% and the hydrocarbon selectivity is 95.4%.

[0099] Although the present invention has been described in detail through specific implementation methods, a person skilled in the art should understand that any changes in form and detail made on this basis that do not exceed the scope of protection of the claims shall fall within the scope of protection of the present invention.

Claims

1. A transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst, characterized in that: The transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst is prepared using zirconium phosphate and transition metal salt as raw materials by adopting the incipient wetness impregnation method. The zirconium phosphate has a zirconium-to-phosphorus ratio of 1; The loading of transition metal in the catalyst is 5-20%; The transition metal salt is one of the acetates of Fe, Co, Ni and Cu; The preparation method comprises the following steps: 1) Dissolving zirconium salt and ammonium salt in deionized water respectively, stirring and mixing to obtain a solid acid suspension; 2) Filter the suspension, dry the residue at 100°C, grind, pass through a 60-mesh sieve, and calcine at 550°C; 3) The calcined solid and transition metal salt are dissolved in deionized water, stirred and mixed, the solvent is removed by rotary evaporation, calcined at 450° C., reduced and passivated at 550° C., and a transition metal-loaded zirconium phosphate grease hydrodeoxygenation catalyst is obtained.

2. Use of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst as claimed in claim 1 in the hydrodeoxygenation reaction of biological oils and fats, characterized in that: The dosage of the transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst is 1-10% of the weight of the processed biomass oil, the reaction temperature for hydrodeoxygenation is 280-400°C, the hydrogen pressure is 2-6 MPa, and the reaction time is 2-10 h.