ABS composition and its preparation method and application
By using strip nano barium sulfate, compatible and lubricant in ABS materials, the problems of insufficient strength and surface gloss in high-load injection molded parts are solved, and efficient mechanical enhancement and aesthetic effect are achieved, which promotes the improvement of Lightweight application of materials.
Patent Information
- Application Number
- CN202310625563.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-30
AI Technical Summary
In injection molded parts that need to withstand large loads, the reinforcement effect of barium sulfate is limited. At the same time, the surface of the injection molded parts is lacking in gloss after being reinforcing with glass fiber, which cannot meet the aesthetics and strength requirements.
The strip-shaped nanobarium sulfate is used as a filler, combined with a compatibilizer and lubricant, and the ABS composition is prepared through melt blending technology to improve mechanical strength and processing performance and ensure the surface gloss of the injection molded parts.
It effectively improves the mechanical strength and surface gloss of ABS composition, meets the production requirements of large injection molded parts, reduces the filler content, and is conducive to the lightweight promotion of materials.
Smart Images

Figure BDA0004256968440000041 
Figure BDA0004256968440000061 
Figure BDA0004256968440000071
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and in particular to an ABS composition and a preparation method and application thereof. Background Art
[0002] With the rapid development of the automobile industry in recent years, lightweight, quality, energy-saving, environmental protection, and functionalization have become the main goals of the current automobile industry. As a general engineering plastic, ABS has the characteristics of low price, light weight, solvent resistance, easy recycling, and non-toxicity. It is one of the important lightweight materials for automobiles. However, for some automobile injection molding parts, the use of ABS material alone cannot meet the required strength. At this time, ABS needs to be modified. A commonly used ABS modification method is to add barium sulfate. Barium sulfate is a white powder that is non-toxic and odorless. It is a heavy metal salt. It can increase the weight of ABS by blending with ABS, and increase the density and hardness of ABS, thereby improving its mechanical properties.
[0003] However, for injection molded parts that need to withstand large loads, barium sulfate has limited reinforcing effect on ABS and cannot meet the use requirements. If glass fiber is used for reinforcement, the surface of the obtained injection molded parts lacks gloss and is not beautiful. Summary of the invention
[0004] The invention provides an ABS composition, a preparation method and an application thereof, which can further improve the mechanical strength of the ABS composition modified by barium sulfate while ensuring the surface gloss of an injection molded part.
[0005] In order to solve the above technical problems, one of the purposes of the present invention is to provide an ABS composition, comprising the following components in parts by weight: ABS: 65 parts to 86 parts; strip-shaped nano-barium sulfate: 10 parts to 35 parts; compatibilizer: 2.5 parts to 5 parts; lubricant: 0.5 parts to 1.5 parts; other additives: 0 parts to 2 parts.
[0006] By adopting the above scheme, the inventors adopted a special filler, namely, strip-shaped nano barium sulfate. This filler has a very small particle size ranging from 150-500nm, which can fully fill the tiny gaps and holes in the ABS substrate, and the special strip-shaped structure can significantly and effectively improve the mechanical strength of the composition, so as to meet the production requirements of injection molded parts that need to withstand large loads. In addition, the present invention also adds an appropriate amount of compatibilizer and lubricant, which can effectively improve the processing performance and melt fluidity of the composition, and further improve the combination between ABS and barium sulfate.
[0007] As a preferred embodiment, the strip-shaped nano-barium sulfate is a hollow strip-shaped nano-barium sulfate and / or a solid strip-shaped nano-barium sulfate.
[0008] As a preferred embodiment, the strip-shaped nano-barium sulfate is hollow strip-shaped nano-barium sulfate and solid strip-shaped nano-barium sulfate, the solid strip-shaped nano-barium sulfate is 10 parts by weight to 15 parts by weight, and the hollow strip-shaped nano-barium sulfate is 5 parts by weight to 15 parts by weight.
[0009] As a preferred embodiment, the weight ratio of the hollow strip-shaped nano-barium sulfate to the solid strip-shaped nano-barium sulfate is 1:1.5.
[0010] As a preferred embodiment, the surface of the strip-shaped nano-barium sulfate is modified by a silane coupling agent.
[0011] As a preferred embodiment, the melt flow rate of ABS is 2 to 10 g / 10 min at 220° C. and 10 kg.
[0012] As the compatibilizer of the above technical solution, conventional materials include SMA (styrene-anhydride-butadiene copolymer), MBS (butyl methyl acrylate-butadiene-styrene copolymer), ASA (acrylonitrile-butadiene-styrene-acrylate copolymer) and maleic anhydride grafted ABS, etc. As a preferred solution, the compatibilizer is maleic anhydride grafted ABS, and the grafting rate is 0.9%-1.15%.
[0013] As the lubricant of the above technical solution, conventionally there are stearates and some small molecule wax materials, which play a role in improving the fluidity and demoulding performance of plastic processing. However, as a preferred embodiment, the lubricant used is graphite oxide, and the lubricant is 1.5 parts by weight. In injection molding, the role of the lubricant is to reduce friction, reduce the viscosity of the melt, and promote melt flow. In the ABS composition with a high filling rate, the filler will increase the viscosity and flow resistance of the melt, resulting in an increase in the difficulty of composition processing and a decrease in surface quality. Therefore, it is very important to select a suitable lubricant to improve the processing performance and surface quality of the composition. The special layered structure of graphite oxide can play the role of lubricating and dispersing strip nano barium sulfate. However, the addition amount of graphite oxide should be controlled within a certain range, and excessive addition will affect the surface quality of the injection molded part. At the same time, the addition of graphite oxide should be fully mixed and dispersed to avoid uneven surface textures and black particles.
[0014] As a preferred embodiment, other additives include 0.2-0.4 parts by weight of a phenolic primary antioxidant, 0.2-0.4 parts by weight of a phosphite secondary antioxidant, and 0.4-0.8 parts by weight of a UV stabilizer.
[0015] In order to solve the above technical problems, the second object of the present invention provides a method for preparing an ABS composition, comprising the following steps: mixing ABS, a compatibilizer, and a lubricant to obtain a first premix; mixing strip-shaped nano barium sulfate and other additives to obtain a second premix; uniformly mixing the first premix and the second premix, adding them to an extrusion device, and performing melt blending and extrusion granulation, wherein the extrusion temperature of the extrusion device is 220°C-240°C to obtain an ABS composition.
[0016] In order to solve the above technical problems, the third object of the present invention provides an application of an ABS composition in the field of large injection moldings, such as manufacturing large automobile injection moldings, home appliance housings, etc.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The ABS composition of the present invention uses the technical solution of filling tiny gaps and holes in the ABS substrate with strip-shaped nano-barium sulfate, which effectively improves the mechanical strength of the composition, so as to meet the production requirements of injection molded parts that need to withstand large loads.
[0019] 2. The ABS composition of the present invention can more effectively improve the mechanical strength of the composition at the same addition amount through the efficient reinforcing characteristics of the strip-shaped nano-barium sulfate, which is beneficial to reduce the content of fillers and better promote the lightweight of materials.
[0020] 3. The preparation method of the ABS composition provided by the present invention is simple and easy to implement and suitable for mass production. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The following Table 1 lists the sources and types of raw materials used in the examples and comparative examples of the present application. Unless otherwise specified, the reagents were all commercially available.
[0023] Table 1 - Sources and models of raw materials in the examples and comparative examples of this application
[0024]
[0025] The preparation methods of hollow barium sulfate nanoparticles, solid barium sulfate nanoparticles and hollow spherical barium sulfate nanoparticles are as follows:
[0026] 1. Preparation method of hollow strip nano barium sulfate:
[0027] Step 1: prepare a barium carbonate slurry in a weight ratio of 1:5 between barium carbonate and water, add 0.05 weight parts of EDTA-2Na and 0.05 weight parts of trisodium phosphate to 10 weight parts of the barium carbonate slurry, and mix well to obtain a pre-reaction mixture;
[0028] Step 2: preparing 3 parts by weight of a sulfuric acid solution having a concentration of 8 wt % (parts by weight);
[0029] Step 3: Add 0.05 parts by weight of EDTA-2Na and 0.05 parts by weight of sodium octadecyl sulfate to 500 parts by weight of water to prepare a bottom water mixture;
[0030] Step 4: adding the pre-reaction mixture and the sulfuric acid solution dropwise to the bottom water mixture, and controlling the pH value to be between 2.0 and 2.2 during the addition;
[0031] Step 5: After the dropwise addition is completed, the mixture is stirred for 30 min at a temperature to fully stir the mixture to react to obtain a reaction mixture;
[0032] Step 6: Filter and wash the reaction mixture, and then dry it to obtain hollow strip-shaped nano-barium sulfate.
[0033] 2. A method for preparing solid strip-shaped nano-barium sulfate comprises the following steps:
[0034] Step 1: prepare a barium carbonate slurry in a weight ratio of 1:5 between barium carbonate and water, add 0.05 weight parts of EDTA-2Na and 0.625 weight parts of trisodium phosphate to 10 weight parts of barium sulfide slurry, and mix well to obtain a pre-reaction mixture;
[0035] Step 2: preparing 3 parts by weight of a sodium sulfate solution having a concentration of 8 wt % (parts by weight);
[0036] Step 3: Add 0.05 parts by weight of EDTA-2Na and 0.05 parts by weight of sodium octadecyl sulfate to 50 parts by weight of water to prepare a bottom water mixture;
[0037] Step 4: adding the pre-reaction mixture and the sodium sulfate solution dropwise to the bottom water mixture;
[0038] Step 5: After the dropwise addition is completed, the mixture is stirred for 30 min at a temperature to fully stir the mixture to react to obtain a reaction mixture;
[0039] Step 6: Filter and wash the reaction mixture, and then dry it to obtain solid strip-shaped nano-barium sulfate.
[0040] 3. The preparation method of hollow spherical nano-barium sulfate is prepared by referring to the method of Example 2 of the specific implementation method in patent document No. CN113697838B.
[0041] Examples 1-6
[0042] An ABS composition can be applied to the field of large injection molded parts such as automotive parts, home appliances, and daily products, including ABS, strip-shaped nano barium sulfate / hollow spherical nano barium sulfate, a compatibilizer, a lubricant, a phenolic primary antioxidant 1010, a phosphite secondary antioxidant 168, and an ultraviolet stabilizer 326. The content of each component is shown in Table 2. The preparation method comprises the following steps:
[0043] (1) mixing ABS, a compatibilizer, and a lubricant to obtain a first premix;
[0044] (2) mixing the nano-barium sulfate filler, the phenolic primary antioxidant 1010, the phosphite secondary antioxidant 168 and the ultraviolet stabilizer 326 to obtain a second premix;
[0045] (3) Then, the first premix and the second premix are uniformly mixed and added into a twin-screw extruder, and then melt-blended and extruded into granules. The extrusion temperature of the twin-screw extruder is 200° C. to 240° C., the first section is 200° C., the second to fourth sections are 240° C., the fifth to eighth sections are 220° C., and the ninth section of the die head is 230° C., thereby obtaining the ABS composition.
[0046] Table 2 - Content of each component in Examples 1-5
[0047]
[0048] Example 7
[0049] An ABS composition, wherein each step and the reagents and process parameters used in each step in the preparation method are the same as those in Example 1, except that the surface of the strip-shaped nano-barium sulfate is modified by a silane coupling agent, and the method is as follows: filtering the reaction mixture, washing it with water, re-slurrying it, adding 1.0 weight part of the silane coupling agent, adjusting the pH value to 3.5-4.0, stirring it for 1 hour, and dehydrating and drying it to obtain the modified strip-shaped nano-barium sulfate.
[0050] Comparative Example 1
[0051] An ABS composition, wherein each step, reagents used in each step and process parameters in the preparation method are the same as those in Example 1, except that ordinary barium sulfate is used as the filler.
[0052] Performance testing
[0053] 1. Tensile strength: tested in accordance with ISO 527-2-2016, with a tensile speed of 50 mm / min. The test results are shown in Table 3;
[0054] 2. Bending strength: tested in accordance with ISO 178. The test results are shown in Table 3.
[0055] 3. Izod notch impact strength: tested in accordance with ISO180-2000 standard, the test results are shown in Table 3;
[0056] 4. Surface condition of injection molded parts: The prepared ABS composition materials were used to respectively mold color plates, and the surface condition of the color plates was tested using a gloss tester. The higher the test value, the better the gloss and the smoother the surface. The test results are shown in Table 3.
[0057] 5. Density: Density of color plate injection molded parts is measured, and the test results are shown in Table 3.
[0058] Table 3 - Performance test results of Examples 1-6 and Comparative Examples 1-2
[0059]
[0060] Combining the performance test results of the embodiments and comparative examples in Table 3, it can be seen that the present invention uses strip-shaped nano barium sulfate as a filler, which is a strongly polar nano filler for filling, giving the ABS a reinforcing effect between polymer chains. At the same time, the strip-shaped filler can further increase the strength and hardness of the ABS, and the injection molding surface is glossy and has no obvious defects, meeting the appearance requirements of the injection molding product. Moreover, the relative density of the obtained material is lower than that of the traditional barium sulfate modified ABS, which is conducive to the lightweight promotion of the material.
[0061] It can be seen from the data of Example 2 that the higher the dosage of nano-barium sulfate is, the better it is. On the contrary, solid nano-barium sulfate strips can obtain more excellent mechanical reinforcement properties when the dosage is relatively low.
[0062] From the comparison of the data of Examples 3 and 4, it can be seen that when the ratio of hollow strip-shaped nano-barium sulfate to solid strip-shaped nano-barium sulfate is 1:1.5, the density is appropriately reduced while maintaining the mechanical properties, which is conducive to further lightweighting of the material.
[0063] It can be seen from the data of Example 5 that when graphite oxide is used as the lubricant, the mechanical properties of the composition can be further improved compared to the small molecule stearate lubricant.
[0064] It can be seen from the data of Example 6 that the hollow spherical nano-barium sulfate has a relatively lower density than the solid barium sulfate in Comparative Example 1, and the surface condition of the injection molded part is excellent, which is conducive to the lightweight of the product, while the mechanical strength is only slightly reduced.
[0065] It can be seen from the data of Example 7 that the surface of the strip-shaped nano-barium sulfate is modified by a silane coupling agent, which is also beneficial to further improve the dispersibility of the nano-barium sulfate and make the surface interaction between the polymer and the nano-barium sulfate closer, further improving the mechanical properties.
[0066] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. An ABS composition, characterized in that: The composition comprises the following components in parts by weight: ABS: 65 parts to 86 parts; Strip-shaped nano-barium sulfate: 10-35 parts; Compatibilizer: 2.5-5 parts; Lubricant: 0.5-1.5 parts; other additives: 0-2 parts, the strip-shaped nano-barium sulfate includes solid strip-shaped nano-barium sulfate; The preparation method of the solid strip-shaped nano-barium sulfate comprises the following steps: Step 1: prepare a barium carbonate slurry in a weight ratio of 1:5 between barium carbonate and water, add 0.05 weight parts of EDTA-2Na and 0.625 weight parts of trisodium phosphate to 10 weight parts of the barium carbonate slurry, and mix well to obtain a pre-reaction mixture; Step 2: preparing 3 parts by weight of a sodium sulfate solution with a concentration of 8 wt%; Step 3: Add 0.05 parts by weight of EDTA-2Na and 0.05 parts by weight of sodium octadecyl sulfate to 50 parts by weight of water to prepare a bottom water mixture; Step 4: adding the pre-reaction mixture and the sodium sulfate solution dropwise to the bottom water mixture; Step 5: After the dropwise addition is completed, the mixture is stirred at room temperature for 30 minutes to fully stir the mixture to react sufficiently to obtain a reaction mixture; Step 6: Filter and wash the reaction mixture, and then dry it to obtain solid strip-shaped nano-barium sulfate.
2. An ABS composition according to claim 1, characterized in that: The strip-shaped nano-barium sulfate includes hollow strip-shaped nano-barium sulfate and solid strip-shaped nano-barium sulfate.
3. An ABS composition according to claim 2, characterized in that: The solid strip-shaped nano-barium sulfate is 10 parts by weight to 15 parts by weight, and the hollow strip-shaped nano-barium sulfate is 5 parts by weight to 15 parts by weight.
4. An ABS composition according to claim 3, characterized in that: The weight ratio of the hollow strip-shaped nano-barium sulfate to the solid strip-shaped nano-barium sulfate is 1:1.
5.
5. An ABS composition according to claim 1, characterized in that: The surface of the strip-shaped nano-barium sulfate is modified by a silane coupling agent.
6. An ABS composition according to claim 1, characterized in that: The melt flow rate of the ABS is 2-10 g / 10 min at 220° C. and 10 kg.
7. An ABS composition according to claim 1, characterized in that: The lubricant is graphite oxide, and the amount of the lubricant is 1.5 parts by weight.
8. An ABS composition according to claim 1, characterized in that: The other auxiliary agents include 0.2-0.4 parts by weight of a phenolic primary antioxidant, 0.2-0.4 parts by weight of a phosphite secondary antioxidant and 0.4-0.8 parts by weight of an ultraviolet stabilizer.
9. A method for preparing an ABS composition, characterized in that: The method for preparing the ABS composition according to any one of claims 1 to 8 comprises the following steps: mixing ABS, a compatibilizer and a lubricant to obtain a first premix; mixing strip-shaped nano barium sulfate and other additives to obtain a second premix; uniformly mixing the first premix and the second premix, adding the mixture to an extrusion device, and performing melt blending and extrusion granulation, wherein the extrusion temperature of the extrusion device is 220° C. to 240° C., to obtain an ABS composition.
10. Use of the ABS composition according to any one of claims 1 to 8 in the field of automobile injection moldings.