A PLA masterbatch for 3D printing and its preparation method and application
By adding antioxidants and heat stabilizers to PLA resin, and using polyurethane coupling modified pigments, the problem of PLA resin masterbatch pigment agglomeration is solved, the melt index and mechanical properties are improved, and the gloss and gloss of 3D printed products are ensured. Smoothness.
Patent Information
- Application Number
- CN202310846159.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-07-11
AI Technical Summary
During the 3D printing process, the pigments of PLA resin masterbatch are easy to agglomerate, resulting in poor surface gloss and printing smoothness, and the melt index and mechanical properties are affected. Existing methods such as adding dispersants or lowering the extrusion temperature will cause The viscosity of the resin decreases or the molecular chain breaks, which affects the performance of the product.
By adding antioxidants and heat stabilizers to PLA resin, and using polyurethane coupling modified pigments, the chain extender reacts with the PLA resin molecular chain to increase the molecular weight and compatibility, control the melt index, and ensure uniform pigment dispersion and resin stability. sex.
It achieves reduced pigment particle size, stable melt index, and improved thermal stability, ensuring the multiple processing capabilities of PLA resin and the gloss and mechanical properties of 3D printed products.
Smart Images

Figure BDA0004332395760000061 
Figure BDA0004332395760000071 
Figure BDA0004332395760000072
Abstract
Description
Technical Field
[0001] The present application relates to the field of masterbatches, and more specifically, to a PLA masterbatch for 3D printing, a preparation method thereof, and an application thereof. Background Art
[0002] Masterbatch is an aggregate obtained by uniformly loading an extraordinary amount of pigment into a resin. It can be called a pigment concentrate, which is mainly composed of three basic elements: pigment, carrier and additive. Pigments are divided into organic pigments and inorganic pigments. Organic pigments include phthalocyanine red, phthalocyanine blue, phthalocyanine green, permanent violet, azo red, etc. Inorganic pigments include cadmium red, cadmium yellow, titanium dioxide, carbon black, iron oxide red, iron oxide yellow, etc. PLA resin (polylactic acid) has excellent biocompatibility and biodegradability. It is an ideal environmentally friendly material and is often used in the field of 3D printing. PLA resin has high tensile strength and compression modulus, but it is more prone to decomposition after excessive shearing and prolonged heating. Therefore, PLA resin cannot be over-sheared or processed multiple times during the production process of masterbatches for 3D consumables.
[0003] In the production and application of masterbatches for 3D consumables, if the pigments and fillers in the masterbatch agglomerate and the particles are too large, it will seriously affect the surface gloss of the consumables, the surface gloss of the printed products, and the smoothness of the printing process. At present, in order to promote the dispersion of pigments and fillers in the resin carrier and reduce the particle size, dispersants are added to the masterbatch, or the extrusion granulation temperature is reduced to increase the resin melt viscosity and strengthen the shearing effect on the pigments and fillers.
[0004] However, the addition of dispersants can easily reduce the internal friction of the resin, reduce viscosity, increase fluidity, and increase the melt index; the reduction of extrusion granulation temperature can easily cause the breakage of the resin molecular chain, resulting in a decrease in resin molecular weight, increased fluidity, and an increase in melt index. The increase in melt index may affect the application of masterbatches in 3D consumables products, causing printing defects; at the same time, the reduction in resin molecular weight may affect the mechanical properties of 3D printed products such as impact, stretching, and bending, thereby affecting the final performance of 3D printed products. Summary of the invention
[0005] In order to ensure uniform dispersion of pigments while making the melt index more stable, the present application provides a PLA masterbatch for 3D printing, a preparation method thereof, and an application thereof.
[0006] In the first aspect, the present application provides a PLA masterbatch for 3D printing, which adopts the following technical solution:
[0007] A PLA masterbatch for 3D printing, comprising the following components in parts by weight:
[0008] 60-90 parts of PLA resin particles,
[0009] Pigment 10-20 parts,
[0010] 2-5 parts of antioxidants,
[0011] Chain extender 0.5-2 parts,
[0012] 2-5 parts of heat stabilizer;
[0013] The pigment is a polyurethane coupling modified pigment.
[0014] By adopting the above technical scheme, during the melt processing, the active groups in the chain extender molecules react with the hydroxyl and carboxyl groups at the ends of the PLA resin molecular chains, and recouple the degraded molecular chains, which is beneficial to increasing the molecular weight of the PLA resin, increasing the melt viscosity, and controlling the melt index to be stable, which is beneficial to improving the thermal stability and processing stability, and can enable the PLA resin to be processed multiple times, strengthen shearing, and then help control the dispersed particle size of the pigment and filler to a lower level, while still stabilizing the melt index; by adding antioxidants and heat stabilizers, the stability of the PLA resin is further improved, the possibility of the PLA resin being decomposed by oxidation or heat is reduced, and the processing performance of the PLA resin is further enhanced, which is beneficial to ensuring the uniform shear dispersion of the pigment and the stability of the melt index;
[0015] By subjecting the pigment to polyurethane coupling modification, the long chain of polyurethane molecules is coupled to the surface of the pigment to form a coating on the pigment, thereby improving the compatibility of the pigment particles with the PLA resin, which is beneficial to improving the dispersion uniformity of the pigment and reducing the possibility of pigment particle agglomeration. At the same time, polyurethane has excellent stability and good heat resistance. During the melt processing, the long chain of polyurethane can cross-link and entangle with the PLA molecules to improve the stability of the PLA resin molecules, which is beneficial to further ensure the stability of the masterbatch melt index.
[0016] Preferably, the pigment modification method is specifically as follows:
[0017] Treating the pigment with a coupling agent to obtain a coupled modified pigment;
[0018] Mix polyether diol and diisocyanate, and react at 60-80°C for 3-5h to obtain a polyurethane prepolymer;
[0019] The polyurethane prepolymer and diethanolamine are dissolved in an organic solvent, the coupled modified pigment is immersed therein, reacted at 70-120° C. for 60-120 minutes, filtered, washed, and baked to obtain the polyurethane coupled modified pigment.
[0020] Preferably, the method for treating the pigment with a coupling agent is as follows:
[0021] The coupling agent is dissolved in an alcohol aqueous solution, and the pH is adjusted to 3-5 to obtain a coupling agent solution with a mass fraction of 5-10%. Then, 10-20% of the pigment of the coupling agent solution is immersed in the coupling agent solution, stirred for 20-60 minutes, filtered, washed, and dried to obtain a coupled modified pigment.
[0022] Preferably, the coupling agent is a silane coupling agent.
[0023] By adopting the above technical scheme, the coupling agent is used to modify the surface of the pigment, which is beneficial to improving the dispersion performance of the pigment and reducing the possibility of pigment agglomeration in the PLA resin system; under the action of diethanolamine, the polyurethane prepolymer undergoes a chain extension reaction, and reacts with the active group of the coupling agent on the surface of the pigment through the isocyanate group, and is grafted onto the pigment to coat and modify the pigment, thereby improving the compatibility between the pigment particles and the PLA resin, and the long-chain polyurethane molecules can form a cross-linked entanglement structure with the PLA resin molecules, thereby improving the stability of the PLA resin.
[0024] Preferably, the chain extender is a polymer chain extender.
[0025] Preferably, the chain extender is BASF ADR4368C.
[0026] By adopting the above technical solution, the polymer chain extender can react with the hydroxyl and carboxyl groups at the ends of the PLA resin molecular chains, thereby increasing the molecular weight of the resin to a certain extent and promoting the stability of the melt index.
[0027] Preferably, the antioxidant is selected from a combination of one or more of hindered phenol antioxidants, phosphite antioxidants and thioester antioxidants.
[0028] By adopting the above technical scheme, hindered phenol antioxidants have good antioxidant effect, high thermal stability, can capture free radicals, and reduce the possibility of thermal oxidative decomposition of PLA resin molecules; phosphite antioxidants and thioester antioxidants can inhibit and delay the generation of free radicals, decompose hydroperoxides, and improve antioxidant properties.
[0029] Preferably, the heat stabilizer is selected from a combination of one or more of barium stearate, calcium stearate and zinc stearate.
[0030] By adopting the above technical solution, the thermal stability of PLA resin is improved, the possibility of thermal decomposition of PLA resin during melt processing is reduced, which is conducive to ensuring the stability of melt index.
[0031] In a second aspect, the present application provides a method for preparing PLA masterbatch for 3D printing, using the following technical solution:
[0032] A method for preparing PLA masterbatch for 3D printing comprises the following steps:
[0033] Bake the PLA resin particles, pigment, antioxidant, chain extender, and thermal stabilizer at 80-90°C for 3-4 hours;
[0034] According to the proportion, the dried PLA resin particles, pigment, antioxidant, chain extender, and heat stabilizer are mixed and stirred for 2-3 minutes to obtain a mixture;
[0035] The mixture is added into a twin-screw extruder, melt-extruded into strips, pelletized, dried, and cooled to obtain PLA masterbatch for 3D printing.
[0036] Preferably, in the extrusion step, the extrusion temperature is 190-205° C., the extrusion speed is 300-340 r / min, and the feeding speed is 15-25 Hz.
[0037] By adopting the above technical solution, PLA masterbatch with stable melt index and good glossiness can be produced.
[0038] In a third aspect, the present application provides an application of PLA masterbatch for 3D printing, using the following technical solution:
[0039] The invention discloses an application of PLA masterbatch for 3D printing, and the application is related to 3D printing.
[0040] By adopting the above technical solution, 3D printing can be made smoother and the product glossiness can be better.
[0041] In summary, this application has the following beneficial effects:
[0042] 1. Since the present application adopts the method of adding a dispersant to the PLA masterbatch, it is beneficial to promote the increase of the molecular weight of the PLA resin during the melt processing, control the stability of the melt index, improve the thermal stability and processing stability, and enable the PLA resin to be processed multiple times, strengthen shear, and then help control the dispersed particle size of the pigment and filler to a lower level, while still stabilizing the melt index; 2. In the present application, the pigment is modified by polyurethane coupling, and the long chain of the polyurethane molecule is coupled to the surface of the pigment to form a coating on the pigment, thereby improving the compatibility of the pigment particles and the PLA resin, and then helping to improve the dispersion uniformity of the pigment and reduce the possibility of pigment particle agglomeration; at the same time, the polyurethane has excellent stability and good heat resistance. During the melt processing, the long chain of the polyurethane can be cross-linked and entangled with the PLA molecules to improve the stability of the PLA resin molecules, which is beneficial to further ensure the stability of the melt index of the masterbatch. DETAILED DESCRIPTION
[0043] The present application is further described in detail below with reference to the embodiments.
[0044] Preparation Example
[0045] Preparation Example 1
[0046] This preparation example provides a method for modifying a pigment, and the preparation method is as follows:
[0047] The coupling agent is dissolved in an ethanol solution with a volume fraction of 90%, and the pH is adjusted to 5 to obtain a coupling agent solution with a mass fraction of 8%. Then, 10% of the pigment by mass of the coupling agent solution is immersed in the coupling agent solution, and the mixture is stirred for 30 minutes, filtered, washed, and dried to obtain a coupled modified pigment.
[0048] The polyether diol and diisocyanate were mixed in a mass ratio of 5:2 and added into a reaction kettle, and reacted at 60° C. for 3 h to obtain a polyurethane prepolymer;
[0049] The polyurethane prepolymer and diethanolamine are dissolved in an organic solvent at a mass ratio of 5:1, and the coupled modified pigment is immersed therein at a bath ratio of 1:10. The reaction is carried out at 85°C for 2 hours, and the polyurethane coupled modified pigment is obtained by filtering, washing and baking.
[0050] In this preparation example, the coupling agent is silane coupling agent KH570, the polyether diol is polytetramethylene ether diol, the diisocyanate is isophorone diisocyanate, and the organic solvent is N,N-dimethylacetamide.
[0051] Preparation Example 2
[0052] The difference between this preparation example and preparation example 1 is that the pigment is only surface-modified by a coupling agent. The specific steps are as follows:
[0053] The coupling agent is dissolved in a 90% ethanol solution by volume, and the pH is adjusted to 5 to obtain a coupling agent solution with a mass fraction of 8%. Then, 10% of the pigment by mass of the coupling agent solution is immersed therein, stirred for 30 minutes, filtered, washed, and dried to obtain a coupled modified pigment.
[0054] Preparation Example 3
[0055] The difference between this preparation example and preparation example 1 is that the pigment is only surface-modified with polyurethane. The specific steps are as follows:
[0056] The polyether diol and diisocyanate were mixed in a mass ratio of 5:2 and added into a reaction kettle, and reacted at 60° C. for 3 h to obtain a polyurethane prepolymer;
[0057] The polyurethane prepolymer and diethanolamine are dissolved in an organic solvent at a mass ratio of 5:1, and the pigment is immersed therein at a bath ratio of 1:10. The reaction is carried out at 85°C for 2 hours, and the polyurethane modified pigment is obtained by filtering, washing and baking.
[0058] Example
[0059] Example 1
[0060] A PLA masterbatch for 3D printing includes the following components in weight: 8 kg PLA resin particles, 1.5 kg pigment, 0.3 kg antioxidant, 0.1 kg chain extender, and 0.3 kg heat stabilizer.
[0061] In this embodiment, the model of PLA resin particles is NatureWorks 4030D; the pigment is BASF K7090 phthalocyanine blue; the antioxidant is a hindered phenol antioxidant, specifically antioxidant 1010; the chain extender is a polymer chain extender, model BASF ADR4368C; and the heat stabilizer is barium stearate.
[0062] In this embodiment, the pigment is a polyurethane coupling modified pigment, and the modification method is the same as that in Preparation Example 1.
[0063] A PLA masterbatch for 3D printing comprises the following steps:
[0064] The PLA resin particles, pigment, antioxidant, chain extender, and thermal stabilizer were baked at 85°C for 3 h;
[0065] Add the above raw materials in a high-speed mixer, mix at high speed for 2-3 minutes at 45°C, and mix well to obtain a mixture;
[0066] The mixture was added into a twin-screw extruder and melt-extruded into strips, wherein the extrusion temperature was 200°C, the extrusion speed was 320r / min, and the feeding speed was 20HZ;
[0067] The extruded filaments are cooled in a water trough and transported to a pelletizer for pelletizing. The obtained PLA masterbatch is then placed in a dryer for drying. After cooling, the PLA masterbatch for 3D printing is obtained.
[0068] Example 2
[0069] The only difference between this embodiment and embodiment 1 is that the PLA masterbatch used for 3D printing includes the following components in mass: 9 kg PLA resin particles, 1 kg pigment, 0.5 kg antioxidant, 0.2 kg chain extender, and 0.5 kg heat stabilizer.
[0070] Example 3
[0071] The only difference between this embodiment and embodiment 1 is that the PLA masterbatch used for 3D printing includes the following components in mass: 6 kg PLA resin particles, 2 kg pigment, 0.2 kg antioxidant, 0.05 kg chain extender, and 0.2 kg heat stabilizer.
[0072] Example 4
[0073] The only difference between this embodiment and embodiment 1 is that the amount of the chain extender is 0.05 kg.
[0074] Example 5
[0075] The only difference between this embodiment and embodiment 1 is that the amount of the chain extender is 2 kg.
[0076] Example 6
[0077] The only difference between this embodiment and embodiment 1 is that the antioxidant is a combination of 0.15 kg of hindered phenol antioxidant and 0.15 kg of phosphite antioxidant, the hindered phenol antioxidant is antioxidant 1010, and the phosphite antioxidant is Irgafos168.
[0078] Example 7
[0079] The only difference between this embodiment and embodiment 1 is that the antioxidant is a combination of 0.15 kg of hindered phenol antioxidant and 0.15 kg of thioester antioxidant, the hindered phenol antioxidant is antioxidant 1010, and the phosphite antioxidant is Irganox PS802.
[0080] Example 8
[0081] The only difference between this embodiment and embodiment 1 is that the heat stabilizer is calcium stearate.
[0082] Example 9
[0083] The only difference between this embodiment and embodiment 1 is that the heat stabilizer is zinc stearate.
[0084] Example 10
[0085] The only difference between this embodiment and embodiment 1 is that the heat stabilizer is a combination of 0.15 kg calcium stearate and 0.15 kg zinc stearate.
[0086] Comparative Example
[0087] Comparative Example 1
[0088] The only difference between this comparative example and Example 1 is that no modification operation is performed on the pigment.
[0089] Comparative Example 2
[0090] The difference between this comparative example and Example 1 is that the pigment is only surface-modified by a coupling agent, and the modification method is the same as that in Preparation Example 2.
[0091] Comparative Example 3
[0092] The difference between this comparative example and Example 1 is that the pigment is only surface-modified with polyurethane, and the modification method is the same as that in Preparation Example 3.
[0093] Comparative Example 4
[0094] The only difference between this comparative example and Example 1 is that no chain extender is added.
[0095] Comparative Example 5
[0096] The difference between this comparative example and Example 1 is that the amount of the chain extender is 0.02 kg.
[0097] Comparative Example 6
[0098] The difference between this comparative example and Example 1 is that the amount of the chain extender is 0.23 kg.
[0099] Performance test test 1: Melt index: According to the methods of Examples 1-10 and Comparative Examples 1-6, melt extrusion was performed three times, and the PLA masterbatch obtained by the three extrusions was selected, and the melt index was tested respectively according to GB / T 3682-2000, and the test temperature was 190°C; the test results are recorded in Table 1.
[0100] Table 1
[0101]
[0102]
[0103] The PLA masterbatch obtained by the third extrusion in each embodiment and comparative example was mixed with PLA resin as 3D consumables, wherein the addition amount of PLA masterbatch was 5%, and a plastic standard sample was printed by 3D printing, and the following tests were performed:
[0104] Test 2: Mechanical test: Refer to GB / T 1040-92 to test the tensile properties of each plastic standard sample; refer to GB / T9341-2008 to test the bending properties of each plastic standard sample;
[0105] Test 3: Printing smoothness: Observe and evaluate the printing smoothness of the 3D printing process. Excellent smoothness means smooth printing without blockage; good means relatively smooth printing without blockage; average means relatively smooth printing with slight blockage; poor means non-smooth printing with blockage;
[0106] Test 4: Product gloss: Referring to GB / T 8807-1988, the gloss of each plastic standard sample was tested and evaluated: gloss 0-39% is poor, 40-59% is fair, 60-79% is good, and 80-100% is excellent.
[0107] The results are recorded in Table 2.
[0108] Table 2
[0109]
[0110]
[0111] It can be seen from Examples 1-3 and Tables 1 and 2 that the PLA masterbatch prepared according to the formula and method disclosed in the present application has a relatively stable melt index, and after being applied to 3D printing, it can make the plastic product have better mechanical properties and gloss.
[0112] In combination with Example 1, Comparative Examples 1-3 and Table 1 and Table 2, it can be seen that after the pigment is modified by polyurethane coupling, the 3D printed product can be given a better gloss, and the melt index is also more stable. This may be because the coupling agent treatment and polyurethane coating can improve the compatibility between the pigment particles and the PLA resin, promote the uniform dispersion of the pigment, reduce the possibility of pigment agglomeration, and improve the gloss of the product; at the same time, the long chain of polyurethane can cross-link with the PLA resin molecular chain, improve the stability of the PLA resin system, and promote the stability of the melt index. In addition, when only polyurethane is used for modification, the grafting effect of polyurethane is not good, and the use of coupling agent and polyurethane for joint modification can improve the grafting efficiency of polyurethane, which is conducive to further promoting the uniform dispersion of the pigment and the stability of the melt index.
[0113] Combining Example 1, Examples 4-5, Comparative Examples 4-6, and Tables 1 and 2, it can be seen that the addition of dispersants is conducive to promoting the stability of the melt index, which may be because the dispersants promote the increase of the molecular weight of the PLA resin and improve the thermal stability of the PLA resin. When the amount of dispersant added is too little, the dispersant has no obvious effect on the stabilization of the masterbatch melt index, and when the amount of dispersant added is too much, the molecular weight of the PLA resin is too large, the fluidity is reduced, and the smoothness during 3D printing is poor.
[0114] Combining Example 1, Examples 6-7 and Table 1, it can be seen that when the hindered phenol antioxidant and the phosphite antioxidant / thioester antioxidant act together, they can give the PLA masterbatch better thermal oxygen stability, which is beneficial to further ensure the stability of the melt index.
[0115] Combining Example 1, Examples 8-10 and Table 1, it can be seen that when a combination of calcium stearate and zinc stearate is selected as a heat stabilizer, the PLA masterbatch can be given better thermal stability, which is beneficial to further ensure the stability of the melt index.
[0116] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A PLA masterbatch for 3D printing, characterized in that: The composition comprises the following components in parts by weight: 60-90 parts of PLA resin particles, 10-20 parts of pigment, 2-5 parts of antioxidants, Chain extender 0.5-2 parts, 2-5 parts of heat stabilizer; The pigment is a polyurethane coupled modified pigment; The modification method of the pigment is specifically as follows: Treating the pigment with a coupling agent to obtain a coupled modified pigment; Mix polyether diol and diisocyanate, and react at 60-80°C for 3-5 hours to obtain a polyurethane prepolymer; Dissolve the polyurethane prepolymer and diethanolamine in an organic solvent, immerse the coupled modified pigment therein, react at 70-120°C for 60-120 minutes, filter, wash, and bake to obtain the polyurethane coupled modified pigment; The chain extender is a polymer chain extender; and the polyether diol is polytetramethylene ether diol.
2. The PLA masterbatch for 3D printing according to claim 1, characterized in that: The method of treating pigments with coupling agents is as follows: The coupling agent is dissolved in an alcohol-water solution, and the pH is adjusted to 3-5 to obtain a coupling agent solution with a mass fraction of 5-10%. Then, 10-20% of the pigment by mass of the coupling agent solution is immersed in the solution, stirred for 20-60 minutes, filtered, washed, and dried to obtain a coupled modified pigment.
3. The PLA masterbatch for 3D printing according to claim 1, characterized in that: The coupling agent is a silane coupling agent.
4. The PLA masterbatch for 3D printing according to claim 1, characterized in that: The antioxidant is selected from one or more combinations of hindered phenol antioxidants, phosphite antioxidants and thioester antioxidants.
5. The PLA masterbatch for 3D printing according to claim 1, characterized in that: The heat stabilizer is selected from a combination of one or more of barium stearate, calcium stearate, and zinc stearate.
6. A method for preparing a PLA masterbatch for 3D printing according to any one of claims 1 to 5, characterized in that: The following steps are involved: Bake the PLA resin particles, pigment, antioxidant, chain extender, and thermal stabilizer at 80-90°C for 3-4 hours; According to the proportion, the dried PLA resin particles, pigment, antioxidant, chain extender, and heat stabilizer are mixed and stirred for 2-3 minutes to obtain a mixture; The mixture is added to a twin-screw extruder, melt-extruded into strips, pelletized, dried, and cooled to obtain PLA masterbatch for 3D printing.
7. The method for preparing PLA masterbatch for 3D printing according to claim 6, wherein: In the extrusion step, the extrusion temperature is 190-205° C., the extrusion speed is 300-340 r / min, and the feeding speed is 15-25 Hz.
8. A use of a PLA masterbatch for 3D printing according to any one of claims 1 to 5, characterized in that: Application and 3D printing.