Waterborne epoxy coating that cures quickly in high humidity environment and preparation method thereof

By modifying the hydrated gel reaction of ultra-refined silicate cement powder and water, the problem of limited curing of aqueous epoxy coatings in high humidity environments is solved, and rapid curing and high adhesion strength are achieved, suitable for high humidity Application in the environment.

CN116656212BActive Publication Date: 2024-12-06天津大学浙江研究院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310717105.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-16
Publication Date
2024-12-06
Estimated Expiration
2043-06-16

AI Technical Summary

Technical Problem

Water-based epoxy coatings evaporate slowly in high humidity environments, resulting in limited curing and cannot be effectively applied in high humidity environments such as coastal areas.

Method used

By using the combination of modified ultra-fine silicate cement powder and resin and aqueous epoxy dispersion, the moisture in the wet coating film is consumed by modifying ultra-fine silicate cement powder and hydrated gel reaction. Achieve rapid curing.

Benefits of technology

The curing speed of aqueous epoxy coatings is significantly accelerated under high humidity environments, the coating adhesion strength is improved, and the drying time is significantly shortened under different humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116656212B_ABST
    Figure CN116656212B_ABST
Patent Text Reader

Abstract

The present application discloses a waterborne epoxy coating that can be rapidly cured in a high humidity environment and a preparation method thereof, wherein the waterborne epoxy coating comprises a component A and a component B, wherein the component A comprises a resin, a cosolvent and a modified ultrafine silicate cement powder, and the component A does not include water, and the component B comprises a waterborne epoxy dispersion and deionized water; wherein the particle size D90 of the modified ultrafine silicate cement powder is 10 to 15 μm, and the surface of the modified ultrafine silicate cement powder is grafted with an amino group. The waterborne epoxy coating prepared by adding modified ultrafine inorganic silicate cement powder in the present application can significantly improve the curing speed of the waterborne epoxy coating, especially the curing speed in a high humidity environment, and improve the adhesion strength of the coating after curing, breaking through the application technology bottleneck of the waterborne epoxy coating that cannot be cured in a high humidity environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of epoxy coatings, and specifically relates to a water-based epoxy coating that can be quickly cured in a high humidity environment and a preparation method thereof. Background Art

[0002] Epoxy coatings are the most important type of industrial protective coatings, accounting for up to 41%. Traditional solvent-based epoxy coatings produce a large amount of volatile organic compounds during the coating process, which damages the atmospheric environment. Due to the country's strict requirements on pollution emissions, water-based epoxy coatings with environmentally friendly and low-carbon characteristics have become a development hotspot.

[0003] Water volatilization is a prerequisite for the curing of conventional water-based epoxy coatings, which is greatly affected by environmental factors. Under high humidity conditions with a relative humidity of ≥85%, water evaporates slowly or even fails to evaporate, making water-based epoxy coatings unusable. The application of epoxy coatings is often carried out in harsh high-humidity environments such as coastal areas, which poses a challenge to the construction and application of water-based epoxy coatings.

[0004] In order to solve the drying and curing problem of waterborne epoxy coatings in the prior art, the reaction rate is accelerated from the perspective of increasing the activity of the reactive groups of the organic resin, thereby improving the drying and curing speed of the waterborne epoxy coatings. However, when the waterborne epoxy coatings are used in a high humidity environment, the curing of the waterborne epoxy coatings is still limited due to the slow volatilization rate of water in the coating. Summary of the invention

[0005] The purpose of the present application is to provide a water-based epoxy coating that can be quickly cured in a high humidity environment and a preparation method, so as to solve the problem that when the water-based epoxy coating in the prior art is applied to a high humidity environment with a relative humidity of ≥85%, the water volatilization rate is slow or even cannot volatilize, making the water-based epoxy coating unusable. The prior art improves the drying and curing speed of the water-based epoxy coating by increasing the activity of the reactive groups of the organic resin, but when used in a high humidity environment, the curing of the water-based epoxy coating is still limited due to the slow volatilization rate of water in the coating.

[0006] To achieve the above purpose, a technical solution adopted in this application is:

[0007] Provided is a waterborne epoxy coating that can be rapidly cured in a high humidity environment, comprising a component A and a component B, wherein the component A comprises a resin, a cosolvent and a modified ultrafine silicate cement powder, and the component A does not comprise water, and the component B comprises a waterborne epoxy dispersion and deionized water; wherein the particle size D90 of the modified ultrafine silicate cement powder is 10 to 15 μm, and an amino group is grafted on the surface of the modified ultrafine silicate cement powder.

[0008] In one or more embodiments, the weight ratio of component A to component B is (0.8-2):1, the mass fraction of the resin in component A is 10-25%, the mass fraction of the co-solvent is 10-20%, and the mass fraction of the modified ultrafine silicate cement powder is 10-35%; the mass fraction of the water-based epoxy dispersion in component B is 80-90%, and the mass fraction of the deionized water is 7.5-18.4%.

[0009] In one or more embodiments, the component A further comprises an anti-settling agent, a defoaming agent, a dispersant, a pigment and a body filler; the component A comprises the following components in parts by weight:

[0010] 10-25 parts of resin, 10-20 parts of cosolvent, 0.1-0.4 parts by weight of anti-settling agent, 0.2-0.5 parts by weight of defoamer, 0.8-1.4 parts by weight of dispersant, 18-24 parts by weight of pigment, 10-34.6 parts by weight of physical filler, and 10-35 parts by weight of modified ultrafine silicate cement powder.

[0011] In one or more embodiments, the resin is an organic amine resin, and the organic amine resin includes one or a combination of fatty amine and polyamide resin; the anti-settling agent includes one or a combination of organic bentonite and polyamide wax powder; the defoamer is an organosilicon defoamer or a polymer defoamer; the dispersant is a water-free non-ionic polymer dispersant; the pigment includes one or a combination of titanium dioxide, iron oxide red powder and iron oxide yellow powder; the physical filler includes one or a combination of feldspar powder and wollastonite powder.

[0012] In one or more embodiments, the component B further comprises an anti-flash rust additive; the component B comprises the following components in parts by weight:

[0013] 80-90 parts of waterborne epoxy dispersion, 7.5-18.4 parts of deionized water, 1.6-3 parts of anti-flash rust additive.

[0014] In one or more embodiments, the aqueous epoxy dispersion is an aqueous dispersion prepared from E20 type solid epoxy resin, and the anti-flash rust additive includes one or more combinations of organic zinc chelate mixed solvent, alkanolamine boric acid and phosphate.

[0015] To achieve the above purpose, another technical solution adopted by this application is:

[0016] A method for preparing the waterborne epoxy coating according to any one of the above embodiments is provided, comprising:

[0017] Put the silicate cement powder into a ball mill, spray the silane coupling agent anhydrous ethanol solution on the surface of the silicate cement powder, start the ball mill, ball mill to a particle size D90 of 10 to 15 μm, and dry to obtain modified ultrafine silicate cement powder;

[0018] Pour the resin and the co-solvent into a stirring kettle and stir, add an anti-settling agent, a defoamer, a dispersant, a pigment, a physical filler and the modified ultrafine silicate cement powder under stirring, stir evenly, filter and package to obtain component A of the waterborne epoxy coating;

[0019] The water-based epoxy dispersion and deionized water are added into a stirring kettle and stirred, and the anti-flash rust additive is added under stirring, and the mixture is stirred evenly, filtered and packaged to obtain component B of the water-based epoxy coating.

[0020] In one or more embodiments, in the step of spraying the anhydrous ethanol solution of silane coupling agent on the surface of silicate cement powder, the mass concentration of the silane coupling agent in the anhydrous ethanol solution of silane coupling agent is 5.0-20%, and the mass ratio of the anhydrous ethanol solution of silane coupling agent to the silicate cement powder is (1-2):100.

[0021] In one or more embodiments, the stirring rate in the step of adding the anti-settling agent, defoaming agent, dispersant, pigment, physical filler and the modified ultrafine silicate cement powder under stirring is 500-600 r / min, and the stirring rate in the step of stirring and filtering and packaging to obtain component A of the water-based epoxy coating is 1500-2000 r / min, and the stirring time is 20-30 min.

[0022] In one or more embodiments, the stirring rate in the step of adding the anti-flash rust additive under stirring is 80 to 120 r / min, the stirring rate in the step of stirring and evenly filtering and packaging to obtain component B of the water-based epoxy coating is 80 to 120 r / min, and the stirring time is 15 to 20 min.

[0023] Different from the prior art, the beneficial effects of this application are:

[0024] In the present application, the modified ultrafine silicate cement powder is dispersed in the anhydrous component A. During the coating construction, the components A and B are mixed and then coated. The modified ultrafine silicate cement powder can react with the water in the component B to form a hydration gel, thereby consuming the water in the wet coating film, so that the drying and curing process of the water-based coating does not depend on the volatilization of the water in the wet coating film, and the water-based epoxy coating can be quickly cured in a high humidity environment;

[0025] The modified ultrafine silicate cement powder in the present application is ultrafinely treated, and the particle size D90 is 10-15 μm, which can effectively improve the dispersion of cement powder in component A, increase the specific surface area of ​​cement powder, increase the contact surface with water after mixing with component B, promote the rate of hydration gel reaction, accelerate the water consumption rate, and accelerate the curing speed;

[0026] The surface of the modified ultrafine silicate cement powder of the present application is grafted with amino groups, which is more conducive to the dispersion of the modified ultrafine silicate cement powder in component A. After mixing with the aqueous epoxy dispersion of component B, the amino groups on the surface of the modified ultrafine silicate cement powder can also undergo an organic cross-linking reaction with the epoxy groups, further strengthening the interface between the cement powder and the epoxy polymer, and improving the adhesion strength of the coating after curing;

[0027] Under standard conditions of temperature 23±2°C and relative humidity 50±5%, the surface drying time of the waterborne epoxy coating of the present application can be accelerated by 83.3% compared with the traditional waterborne epoxy coating, and the actual drying time can be accelerated by 78%; under high humidity conditions of temperature 23±2°C and relative humidity 90±5%, the surface drying time of the waterborne epoxy coating of the present application can be accelerated by 97%, and the actual drying time can be accelerated by 90%;

[0028] Compared with traditional water-based epoxy coatings, the water-based epoxy coating of the present application can improve the coating adhesion strength by up to 122.9%. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic flow chart of an implementation method of a method for preparing a water-based epoxy coating of the present application. DETAILED DESCRIPTION

[0030] The present application will be described in detail below in conjunction with the various embodiments shown in the accompanying drawings. However, these embodiments do not limit the present application, and any structural, methodological, or functional changes made by a person of ordinary skill in the art based on these embodiments are all within the scope of protection of the present application.

[0031] Compared with traditional solvent-based epoxy coatings, water-based epoxy coatings can effectively avoid the generation of a large amount of volatile organic compounds during the coating process and are environmentally friendly and low-carbon.

[0032] However, during the coating operation, water evaporation is a prerequisite for the curing of water-based epoxy coatings. Under high humidity conditions with a relative humidity of ≥85%, water evaporation is slow or even impossible, making water-based epoxy coatings unusable. This seriously limits the application of water-based epoxy coatings in high humidity environments such as coastal areas.

[0033] In order to solve the above problems, the applicant has developed a water-based epoxy coating that can cure quickly in a high humidity environment. The coating can be applied in a wide range of humidity environments while being economical, and is suitable for wide application in the fields of ships, bridges, marine engineering equipment, etc.

[0034] Specifically, the waterborne epoxy coating of the present application includes component A and component B, wherein component A includes resin, cosolvent and modified ultrafine silicate cement powder, and component A does not include water, and component B includes waterborne epoxy dispersion and deionized water.

[0035] The particle size D90 of the modified ultrafine silicate cement powder is 10-15 μm, and the surface of the modified ultrafine silicate cement powder is grafted with amino groups.

[0036] The cosolvent of component A of the waterborne epoxy coating of the present application provides a medium for dispersing the resin and the modified ultrafine silicate cement powder, and does not contain water. By dispersing the modified ultrafine silicate cement powder in the resin and the cosolvent, since there is no water in component A, the modified ultrafine silicate cement powder is prevented from undergoing a hydration gel reaction during the coating liquid state, thereby ensuring the storage stability of the coating in the liquid state.

[0037] During coating construction, component A and component B are mixed and then applied. At this time, the modified ultrafine silicate cement powder can react with the water in component B to form a hydration gel, thereby consuming the moisture in the wet coating film, making the drying and curing process of the water-based paint independent of the volatilization of moisture in the wet coating film, and allowing the water-based epoxy paint to cure quickly in a high humidity environment.

[0038] At the same time, the modified ultrafine silicate cement powder in the present application is ultrafinely treated, and the particle size D90 is 10-15 μm, which can effectively improve the dispersion of cement powder in component A, increase the specific surface area of ​​cement powder, increase the contact surface with water after mixing with component B, promote the rate of hydration gel reaction, and accelerate the water consumption rate.

[0039] In addition, the surface of the modified ultrafine silicate cement powder in the present application is grafted with amino groups, which is more conducive to the dispersion of the modified ultrafine silicate cement powder in component A. After mixing with the aqueous epoxy dispersion of component B, the amino groups on the surface of the modified ultrafine silicate cement powder can also undergo an organic cross-linking reaction with the epoxy groups, further strengthening the interface between the cement powder and the epoxy polymer, and improving the adhesion strength of the coating after curing.

[0040] In one embodiment, the weight ratio of component A to component B is (0.8-2):1, the mass fraction of the resin in component A is 10-25%, the mass fraction of the cosolvent is 10-20%, and the mass fraction of the modified ultrafine silicate cement powder is 10-35%; the mass fraction of the water-based epoxy dispersion in component B is 80-90%, and the mass fraction of deionized water is 7.5-18.4%.

[0041] In one embodiment, component A further comprises an anti-settling agent, a defoaming agent, a dispersant, a pigment and a bulk filler.

[0042] Specifically, component A may include the following components in parts by weight:

[0043] 10-25 parts of resin, 10-20 parts of cosolvent, 0.1-0.4 parts by weight of anti-settling agent, 0.2-0.5 parts by weight of defoamer, 0.8-1.4 parts by weight of dispersant, 18-24 parts by weight of pigment, 10-34.6 parts by weight of physical filler, and 10-35 parts by weight of modified ultrafine silicate cement powder.

[0044] In one embodiment, the resin in component A may be an organic amine resin, and the organic amine resin includes one or a combination of aliphatic amine and polyamide resin.

[0045] In one embodiment, the anti-settling agent may include one or a combination of organic bentonite and polyamide wax powder.

[0046] In one embodiment, the defoaming agent may be a silicone defoaming agent or a polymer defoaming agent.

[0047] In one embodiment, the dispersant may be a non-ionic polymer dispersant that does not contain water, thereby avoiding a hydration gel reaction before coating.

[0048] In one embodiment, the pigment may include one or more combinations of titanium dioxide, iron oxide red, and iron oxide yellow.

[0049] In one embodiment, the bulk filler includes one or a combination of feldspar powder and wollastonite powder.

[0050] In one embodiment, component B further includes an anti-flash rust additive.

[0051] Specifically, component B may include the following components in parts by weight:

[0052] 80-90 parts of waterborne epoxy dispersion, 7.5-18.4 parts of deionized water, 1.6-3 parts of anti-flash rust additive.

[0053] In one embodiment, the waterborne epoxy dispersion is a waterborne dispersion prepared from E20 type solid epoxy resin, and the anti-flash rust additive includes one or more combinations of organic zinc chelate mixed solvent, alkanolamine boric acid and phosphate.

[0054] The present application also provides a method for preparing the above-mentioned waterborne epoxy coating. Specifically, please refer to Figure 1 , Figure 1 It is a schematic flow chart of an implementation method of a method for preparing a water-based epoxy coating of the present application.

[0055] The preparation method comprises:

[0056] S100, putting silicate cement powder into a ball mill, spraying anhydrous ethanol solution of silane coupling agent on the surface of the silicate cement powder, turning on the ball mill, ball milling to a particle size D90 of 10 to 15 μm, drying, and obtaining modified ultrafine silicate cement powder.

[0057] First, the silicate cement powder can be modified by using a ball mill to make it ultrafine. Simultaneously, a silane coupling agent can be used to modify the surface of the cement powder and graft amino groups to improve the dispersion ability of the silicate cement powder, so that the amino groups of the cement powder can undergo cross-linking reaction with the epoxy polymer during subsequent coating, thereby strengthening the interface strength and improving the coating adhesion strength.

[0058] In one embodiment, the mass concentration of the silane coupling agent in the anhydrous ethanol solution of the silane coupling agent can be 5.0-20%, and the mass ratio of the anhydrous ethanol solution of the silane coupling agent to the silicate cement powder can be (1-2):100, thereby ensuring the modification treatment effect.

[0059] S200, pour the resin and the co-solvent into a stirring kettle and stir, add the anti-settling agent, defoaming agent, dispersant, pigment, body filler and modified ultrafine silicate cement powder under stirring, stir evenly, filter and package to obtain component A of the waterborne epoxy coating.

[0060] After the modified ultrafine silicate cement powder is prepared, the resin and the co-solvent can be stirred first, and then the other components are poured into the co-solvent in turn and stirred evenly, filtered and packaged to obtain component A.

[0061] In one embodiment, when other components are added during stirring, the stirring rate may be 500-600 r / min; after the other components are added, the stirring rate in the uniform stirring step may be 1500-2000 r / min, and the stirring time may be 20-30 min.

[0062] S300, adding water-based epoxy dispersion and deionized water into a stirring kettle and stirring, adding anti-flash rust additive under stirring, stirring evenly, filtering and packaging, and obtaining component B of water-based epoxy coating.

[0063] Component B can be obtained by uniformly dispersing the waterborne epoxy dispersion and the anti-flash rust additive in deionized water.

[0064] The stirring rate when adding the anti-flash rust additive under stirring can be 80-120 r / min. After the anti-flash rust additive is added, the stirring rate in the stirring step can be 80-120 r / min, and the stirring time can be 15-20 min.

[0065] The present application also provides a construction method of the above-mentioned water-based epoxy resin, which is specifically:

[0066] Before painting, component A and component B are mixed in a weight ratio of (0.8-2) / 1. While stirring, component B is poured into component A. After stirring evenly, 3.0-8.0% by weight of deionized water is added for dilution. Then, an air spray gun is used for spraying. The spraying pressure is 0.2-0.4 MPa, and the coating dry film thickness is 90-110 μm.

[0067] The beneficial effects of the technical solution of the present application are further described below in conjunction with specific embodiments.

[0068] The sources of the raw materials involved in the following examples are as follows:

[0069] Polyamide resin: Aradur 3951 from Huntsman Advanced Chemical Materials (Guangdong) Co., Ltd.

[0070] Propylene glycol methyl ether: Dow Chemical (Zhangjiagang) Co., Ltd. DOWANOLPM;

[0071] Organic bentonite: BENGEL 828 from Deqian (Shanghai) Chemical Co., Ltd.;

[0072] Defoamer: BYK-066N from BYK Chemical Company, Germany;

[0073] Dispersant: ADDITOLVXW 6208 / 60 from Allnex Resins (China) Co., Ltd.

[0074] Titanium dioxide: R996 from Sichuan Longmang Group Co., Ltd.;

[0075] Feldspar powder: X-7 from Sibelco (Shanghai) Mining Co., Ltd.

[0076] Portland cement powder: Aalborg Portland (Anqing) Co., Ltd. Aalborg PW52.5;

[0077] Silane coupling agent: KH570 from Hangzhou Jessica Chemical Co., Ltd.;

[0078] Waterborne epoxy dispersion: ARALDITE PZ 3901 from Huntsman Advanced Chemical Materials (Guangdong) Co., Ltd.

[0079] Anti-flash rust additive: FA-179 from Deqian (Shanghai) Chemical Co., Ltd.

[0080] Embodiment 1:

[0081] A waterborne epoxy coating is prepared by the following steps:

[0082] Put the silicate cement powder into a ball mill, spray the surface of the silicate cement powder with a 20% mass concentration of anhydrous ethanol solution of silane coupling agent, the spraying weight is 1% of the silicate cement powder, start the ball mill, set the speed to 1000r / min, ball mill to a particle size D90 of 10μm, and dry it in an oven at 100℃ for 2h to obtain modified ultrafine silicate cement powder;

[0083] Pour polyamide resin and propylene glycol methyl ether into a stirring kettle and stir at a stirring rate of 500 r / min, add organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder under stirring, increase the stirring rate to 1500 r / min, stir for 30 minutes, and after stirring evenly, filter with a 100-mesh filter and package to obtain component A of waterborne epoxy coating, wherein the weight ratio of polyamide resin, propylene glycol methyl ether, organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder is 10:20:0.4:0.2:0.8:24:34.6:10;

[0084] Add waterborne epoxy dispersion and deionized water into a stirring kettle and stir at a stirring rate of 80 r / min, add anti-flash rust additive under stirring, continue stirring for 20 minutes, and after stirring evenly, filter through 100 mesh and then package to obtain component B of waterborne epoxy coating, wherein the weight ratio of waterborne epoxy dispersion, deionized water and anti-flash rust additive is 80:17:3;

[0085] Component A and component B are mixed in a weight ratio of 2:1 and placed in two separate containers to obtain a two-component waterborne epoxy coating.

[0086] Embodiment 2:

[0087] A waterborne epoxy coating is prepared by the following steps:

[0088] Put the silicate cement powder into a ball mill, spray the surface of the silicate cement powder with a 10% mass concentration of anhydrous ethanol solution of silane coupling agent, the spraying weight is 1.5% of the silicate cement powder, start the ball mill, set the speed to 1200r / min, ball mill to a particle size D90 of 12μm, and dry it in an oven at 120℃ for 1.5h to obtain modified ultrafine silicate cement powder;

[0089] Pour polyamide resin and propylene glycol methyl ether into a stirring kettle and stir at a stirring rate of 600 r / min, add organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder under stirring, increase the stirring rate to 2000 r / min, stir for 20 minutes, and after stirring evenly, filter with a 150-mesh filter and package to obtain component A of a waterborne epoxy coating, wherein the weight ratio of polyamide resin, propylene glycol methyl ether, organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder is 15:15:0.3:0.3:1:22:31.4:15;

[0090] Add waterborne epoxy dispersion and deionized water into a stirring kettle and stir at a stirring rate of 120 r / min, add anti-flash rust additive under stirring, continue stirring for 15 minutes, and after stirring evenly, filter through 150 mesh and then package to obtain component B of waterborne epoxy coating, wherein the weight ratio of waterborne epoxy dispersion, deionized water and anti-flash rust additive is 90:7.5:2.5;

[0091] Component A and component B are mixed in a weight ratio of 1.5:1 and placed in two separate containers to obtain a two-component waterborne epoxy coating.

[0092] Embodiment 3:

[0093] A waterborne epoxy coating is prepared by the following steps:

[0094] Put the silicate cement powder into a ball mill, spray the surface of the silicate cement powder with a 10% mass concentration of anhydrous ethanol solution of silane coupling agent, the spraying weight is 1.5% of the silicate cement powder, start the ball mill, set the speed to 1200r / min, ball mill to a particle size D90 of 12μm, and dry it in an oven at 120℃ for 1.5h to obtain modified ultrafine silicate cement powder;

[0095] Pour polyamide resin and propylene glycol methyl ether into a stirring kettle and stir at a stirring rate of 550 r / min, add organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder under stirring, increase the stirring rate to 1800 r / min, stir for 18 minutes, and after stirring evenly, filter with a 150-mesh filter and package to obtain component A of a waterborne epoxy coating, wherein the weight ratio of polyamide resin, propylene glycol methyl ether, organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder is 20:12.5:0.2:0.4:1.2:20:20.7:25;

[0096] Add waterborne epoxy dispersion and deionized water into a stirring kettle and stir at a stirring rate of 100 r / min, add anti-flash rust additive under stirring, continue stirring for 18 minutes, filter through 150 mesh and package after stirring evenly to obtain component B of waterborne epoxy coating, wherein the weight ratio of waterborne epoxy dispersion, deionized water and anti-flash rust additive is 80:18.2:1.8;

[0097] Component A and component B are mixed in a weight ratio of 1:1 and placed in two separate containers to obtain a two-component waterborne epoxy coating.

[0098] Embodiment 4:

[0099] A waterborne epoxy coating is prepared by the following steps:

[0100] Put the silicate cement powder into a ball mill, spray the surface of the silicate cement powder with a 5% mass concentration of anhydrous ethanol solution of silane coupling agent, the spraying weight is 2% of the silicate cement powder, start the ball mill, set the speed to 1500r / min, ball mill to a particle size D90 of 15μm, and dry it in an oven at 150℃ for 1h to obtain modified ultrafine silicate cement powder;

[0101] Pour polyamide resin and propylene glycol methyl ether into a stirring kettle and stir at a stirring rate of 550 r / min, add organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder under stirring, increase the stirring rate to 1800 r / min, stir for 18 minutes, and after stirring evenly, filter with a 150-mesh filter and package to obtain component A of waterborne epoxy coating, wherein the weight ratio of polyamide resin, propylene glycol methyl ether, organic bentonite, defoamer, dispersant, titanium dioxide, feldspar powder and modified ultrafine silicate cement powder is 25:10:0.1:0.5:1.4:18:10:35;

[0102] Add waterborne epoxy dispersion and deionized water into a stirring kettle and stir at a stirring rate of 100 r / min, add anti-flash rust additive under stirring, continue stirring for 18 minutes, filter through 150 mesh and package after stirring evenly to obtain component B of waterborne epoxy coating, wherein the weight ratio of waterborne epoxy dispersion, deionized water and anti-flash rust additive is 80:18.4:1.6;

[0103] Component A and component B are mixed in a weight ratio of 0.8:1 and placed in two separate containers to obtain a two-component waterborne epoxy coating.

[0104] Comparative Example 1:

[0105] A waterborne epoxy coating is prepared by the following steps:

[0106] Pour polyamide resin and propylene glycol methyl ether into a stirring kettle and stir at a stirring rate of 500 r / min, add organic bentonite, defoamer, dispersant, titanium dioxide and feldspar powder under stirring, increase the stirring rate to 1500 r / min, stir for 30 minutes, and after stirring evenly, filter with a 100-mesh filter and package to obtain component A of a water-based epoxy coating, wherein the weight ratio of polyamide resin, propylene glycol methyl ether, organic bentonite, defoamer, dispersant, titanium dioxide and feldspar powder is 10:20:0.4:0.2:0.8:24:44.6;

[0107] Add waterborne epoxy dispersion and deionized water into a stirring kettle and stir at a stirring rate of 80 r / min, add anti-flash rust additive under stirring, continue stirring for 20 minutes, and after stirring evenly, filter through 100 mesh and then package to obtain component B of waterborne epoxy coating, wherein the weight ratio of waterborne epoxy dispersion, deionized water and anti-flash rust additive is 80:17:3;

[0108] Component A and component B are mixed in a weight ratio of 2:1 and placed in two separate containers to obtain a two-component waterborne epoxy coating.

[0109] Comparative Example 2:

[0110] A waterborne epoxy coating is prepared by the following steps:

[0111] Pour polyamide resin and propylene glycol methyl ether into a stirring kettle and stir at a stirring rate of 550 r / min, add organic bentonite, defoamer, dispersant, titanium dioxide and feldspar powder under stirring, increase the stirring rate to 1800 r / min, stir for 18 minutes, and after stirring evenly, filter with a 150-mesh filter and package to obtain component A of a water-based epoxy coating, wherein the weight ratio of polyamide resin, propylene glycol methyl ether, organic bentonite, defoamer, dispersant, titanium dioxide and feldspar powder is 25:10:0.1:0.5:1.4:18:45;

[0112] Add waterborne epoxy dispersion and deionized water into a stirring kettle and stir at a stirring rate of 100 r / min, add anti-flash rust additive under stirring, continue stirring for 18 minutes, filter through 150 mesh and package after stirring evenly to obtain component B of waterborne epoxy coating, wherein the weight ratio of waterborne epoxy dispersion, deionized water and anti-flash rust additive is 80:18.4:1.6;

[0113] Component A and component B are mixed in a weight ratio of 0.8:1 and placed in two separate containers to obtain a two-component waterborne epoxy coating.

[0114] The raw material proportions of Examples 1 to 3 and Comparative Examples 1 to 2 are shown in the following table:

[0115]

[0116] Effect example:

[0117] Components A and B of Examples 1 to 3 and Comparative Examples 1 to 2 were mixed, stirred evenly, and then 5% by weight of deionized water was added for dilution. Then, the mixture was sprayed on a test steel plate using an air spray gun. The spraying pressure was 0.3 MPa, and the coating dry film thickness was 100 μm.

[0118] The test steel plate is an ordinary carbon structural steel plate in accordance with GB / T 9271-2008. It is sandblasted and derusted before the test. The rust removal level reaches Sa2.5 level specified in GB / T 8923.1, and the surface roughness reaches the fine (G) level specified in GB / T 13288.1.

[0119] The surface drying time and through drying time of the epoxy coatings of Examples 1 to 3 and Comparative Examples 1 to 2 under different humidity conditions were tested according to the provisions of GB / T 1728-1979, wherein the surface drying time was measured according to the finger touch method specified in GB / T 1728-1979, and the through drying time was measured according to the filter paper method specified in GB / T 1728-1979, to obtain the data in the following table.

[0120] The coating adhesion strength of the coatings of Examples 1 to 3 and Comparative Examples 1 to 2 was tested by the pull-off method specified in GB / T 5210-2006 to obtain the data in the following table.

[0121]

[0122] It can be seen from the data in the above table that the coatings of Examples 1 to 3 have a significantly improved drying speed compared to Comparative Examples 1 and 2 without the addition of modified ultrafine inorganic silicate cement powder. Among them, under standard conditions of temperature 23±2°C and relative humidity 50±5%, the surface drying time is reduced from 1.0 to 1.5h of the comparative example to 0.3 to 0.5h, and the actual drying time is reduced from 8 to 12h of the comparative example 1 to 3 to 5h; under high humidity conditions of temperature 23±2°C and relative humidity 90±5%, the surface drying time is reduced from 6 to 10h of the comparative example to 0.3 to 1h, and the actual drying time is reduced from 36 to 40h of the comparative example 1 to 4 to 8h.

[0123] Further, comparing Example 1 with Comparative Example 1, the surface drying time of Example 1 under standard conditions was accelerated by 50%, and the through drying time was accelerated by 37.5%. Under high humidity conditions, the surface drying time was accelerated by 83.3%, and the through drying time was accelerated by 77.8%.

[0124] Comparing Example 4 with Comparative Example 2, the surface drying time of Example 4 under standard conditions was accelerated by 83.3%, and the through drying time was accelerated by 78%. Under high humidity conditions, the surface drying time was accelerated by 97%, and the through drying time was accelerated by 90%.

[0125] It can be seen that the coatings of Examples 1 to 3 can be surface dried within 18 to 60 minutes even in a high humidity environment, which is significantly faster than the conventional water-based epoxy coatings of the comparative example.

[0126] In addition, the coating adhesion strength test shows that the adhesion strength of the coatings of Examples 1 to 3 is also significantly improved after curing, which can be greatly improved from 3.5 to 4.2 MPa of the comparative example to 6.9 to 7.8 MPa of the example.

[0127] Furthermore, compared with Example 1 and Comparative Example 1, the coating adhesion strength of Example 1 is increased by 122.9%; compared with Example 4 and Comparative Example 2, the coating adhesion strength of Example 4 is increased by 64.3%.

[0128] From the above experiments, it can be seen that the water-based epoxy coating prepared by adding modified ultrafine inorganic silicate cement powder can significantly improve the curing speed of the water-based epoxy coating, especially the curing speed in a high humidity environment, and improve the adhesion strength of the coating after curing, breaking through the application technology bottleneck of the water-based epoxy coating that cannot be cured in a high humidity environment.

[0129] The above description of the present disclosure is provided to enable any person of ordinary skill in the art to implement or use the present disclosure. Various modifications to the present disclosure will be apparent to those of ordinary skill in the art, and the general principles corresponding to the present disclosure may be applied to other variations without departing from the scope of protection of the present disclosure. Therefore, the present disclosure is not limited to the examples and designs described herein, but is consistent with the widest range of principles and novel features disclosed herein.

Claims

1. A water-based epoxy coating that cures quickly in a high humidity environment, characterized in that: The invention comprises a component A and a component B, wherein the component A comprises a resin, a cosolvent and a modified ultrafine silicate cement powder, and the component A does not comprise water, and the component B comprises an aqueous epoxy dispersion and deionized water; wherein the particle size D90 of the modified ultrafine silicate cement powder is 10 to 15 μm, and an amino group is grafted on the surface of the modified ultrafine silicate cement powder; the resin is an organic amine resin, and the organic amine resin comprises one or a combination of two of a fatty amine and a polyamide resin; the weight ratio of the component A to the component B is (0.8 to 2): 1, the mass fraction of the resin in the component A is 10 to 25%, the mass fraction of the cosolvent is 10 to 20%, and the mass fraction of the modified ultrafine silicate cement powder is 10 to 35%; the mass fraction of the aqueous epoxy dispersion in the component B is 80 to 90%, and the mass fraction of the deionized water is 7.5 to 18.4%; The surface drying time of the waterborne epoxy coating under high humidity conditions of 23±2° C. and 90±5% relative humidity is 0.3 to 1 hour, and the actual drying time is 4 to 8 hours.

2. The waterborne epoxy coating according to claim 1, characterized in that: The component A also includes an anti-settling agent, a defoaming agent, a dispersant, a pigment and a physical filler; the component A includes the following components in parts by weight: 10-25 parts of resin, 10-20 parts of cosolvent, 0.1-0.4 parts by weight of anti-settling agent, 0.2-0.5 parts by weight of defoamer, 0.8-1.4 parts by weight of dispersant, 18-24 parts by weight of pigment, 10-34.6 parts by weight of physical filler, and 10-35 parts by weight of modified ultrafine silicate cement powder.

3. The waterborne epoxy coating according to claim 2, characterized in that: The anti-settling agent includes one or a combination of organic bentonite and polyamide wax powder; the defoamer is a polymer defoamer; the dispersant is a water-free non-ionic polymer dispersant; the pigment includes one or a combination of titanium dioxide, iron oxide red powder and iron oxide yellow powder; the physical filler includes one or a combination of feldspar powder and wollastonite powder.

4. The waterborne epoxy coating according to claim 1, characterized in that: The B component also includes an anti-flash rust additive; the B component includes the following components in parts by weight: 80-90 parts of waterborne epoxy dispersion, 7.5-18.4 parts of deionized water, 1.6-3 parts of anti-flash rust additive.

5. The waterborne epoxy coating according to claim 4, characterized in that: The waterborne epoxy dispersion is a waterborne dispersion prepared from E20 type solid epoxy resin, and the anti-flash rust additive comprises one or more combinations of organic zinc chelate mixed solvent, alkanolamine boric acid and phosphate.

6. A method for preparing a waterborne epoxy coating that cures rapidly in a high humidity environment, characterized in that: The waterborne epoxy coating comprises a component A and a component B, wherein the component A comprises a resin, a cosolvent and a modified ultrafine silicate cement powder, and the component A does not include water, and the component A further comprises an anti-settling agent, a defoamer, a dispersant, a pigment and a physical filler, wherein the component A comprises the following components in parts by weight: 10 to 25 parts of resin, 10 to 20 parts of cosolvent, 0.1 to 0.4 parts by weight of an anti-settling agent, 0.2 to 0.5 parts by weight of a defoamer, 0.8 to 1.4 parts by weight of a dispersant, 18 to 24 parts by weight of a pigment, 10 to 34.6 parts by weight of a physical filler, and 10 to 35 parts by weight of a modified ultrafine silicate cement powder; The component B includes an aqueous epoxy dispersion and deionized water, and the component B also includes an anti-flash rust additive. The component B includes the following components in parts by weight: 80 to 90 parts of aqueous epoxy dispersion, 7.5 to 18.4 parts of deionized water, and 1.6 to 3 parts of anti-flash rust additive; The particle size D90 of the modified ultrafine silicate cement powder is 10-15 μm, and the surface of the modified ultrafine silicate cement powder is grafted with amino groups; the resin is an organic amine resin, and the organic amine resin includes one or a combination of two of fatty amine and polyamide resin; the weight ratio of the component A to the component B is (0.8-2):1, the mass fraction of the resin in the component A is 10-25%, the mass fraction of the co-solvent is 10-20%, and the mass fraction of the modified ultrafine silicate cement powder is 10-35%; the mass fraction of the waterborne epoxy dispersion in the component B is 80-90%, and the mass fraction of the deionized water is 7.5-18.4%; The surface drying time of the waterborne epoxy coating under high humidity conditions of 23±2°C and 90±5% relative humidity is 0.3 to 1h, and the actual drying time is 4 to 8h; The preparation method comprises: Put the silicate cement powder into a ball mill, spray the silane coupling agent anhydrous ethanol solution on the surface of the silicate cement powder, start the ball mill, ball mill to a particle size D90 of 10 to 15 μm, and dry to obtain modified ultrafine silicate cement powder; Pour the resin and the co-solvent into a stirring kettle and stir, add an anti-settling agent, a defoamer, a dispersant, a pigment, a physical filler and the modified ultrafine silicate cement powder under stirring, stir evenly, filter and package to obtain component A of the waterborne epoxy coating; The water-based epoxy dispersion and deionized water are added into a stirring kettle and stirred, and the anti-flash rust additive is added under stirring, and the mixture is stirred evenly, filtered and packaged to obtain component B of the water-based epoxy coating.

7. The preparation method according to claim 6, characterized in that: In the step of spraying the anhydrous ethanol solution of silane coupling agent on the surface of silicate cement powder, the mass concentration of silane coupling agent in the anhydrous ethanol solution of silane coupling agent is 5.0-20%, and the mass ratio of the anhydrous ethanol solution of silane coupling agent to the silicate cement powder is (1-2):

100.

8. The preparation method according to claim 6, characterized in that: The stirring rate of the step of adding the anti-settling agent, defoamer, dispersant, pigment, physical filler and the modified ultrafine silicate cement powder under stirring is 500-600 r / min, and the stirring rate of the step of stirring evenly, filtering and packaging to obtain component A of the water-based epoxy coating is 1500-2000 r / min, and the stirring time is 20-30 min.

9. The preparation method according to claim 6, characterized in that: The stirring rate of the step of adding the anti-flash rust additive under stirring is 80-120 r / min, and the stirring rate of the step of stirring evenly, filtering and packaging to obtain component B of the waterborne epoxy coating is 80-120 r / min, and the stirring time is 15-20 min.