Nano titanium dioxide with silicon dioxide coated on the surface and preparation method thereof

By using wollastonite as a silicon source, the temperature and acidity are controlled to carry out solid-liquid reaction, forming a uniform and dense silica cladding layer on the surface of nanotitanium dioxide, solving the problem of insufficient light stability and dispersion of nanotitanium dioxide in the prior art. More efficient light stability and dispersion are achieved, reducing costs and simplifying process operations.

CN116675248BActive Publication Date: 2024-12-03JIANGSU NAO NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310764577.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-27
Publication Date
2024-12-03
Estimated Expiration
2043-06-27

AI Technical Summary

Technical Problem

In the existing nanotitanium dioxide surface-coated silicon dioxide technology, the silicon source is expensive and complex in operation, making it difficult to ensure that the nanotitanium dioxide particles are surface treated in a fully dispersed state, resulting in poor uniformity and denseness of the coating layer, which affects it. Photostability and dispersion.

Method used

Wollastonite is used as the silicon source, and solid-liquid reaction is carried out by controlling the temperature and acidity, so as to promote heterogeneous nucleation of silica on the surface of nano-titanium dioxide, forming a uniform and continuous silica coating layer to ensure that nano-titanium dioxide particles are fully dispersed. Surface treatment is carried out in a state to reduce adhesion and agglomeration, and improve light stability and dispersion.

Benefits of technology

The light stability and dispersion of nanotitanium dioxide are significantly improved, the raw material cost is reduced, and the process operation is simplified, forming a uniform and dense silica coating layer, enhancing the shielding ability of medium-wave ultraviolet rays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004305675110000061
    Figure BDA0004305675110000061
  • Figure BDA0004305675110000071
    Figure BDA0004305675110000071
  • Figure HDA0004305675120000011
    Figure HDA0004305675120000011
Patent Text Reader

Abstract

The present invention belongs to the field of inorganic nanomaterials, and specifically relates to a nano titanium dioxide with a surface coated with silicon dioxide and a preparation method thereof. The present invention uses wollastonite as a silicon source, controls the solid-liquid reaction rate by controlling the temperature and acidity, and causes the silicon dioxide generated slowly by wollastonite to promote heterogeneous nucleation on the surface of the nano titanium dioxide, forming a uniform and continuous silicon dioxide coating layer, thereby greatly improving the light stability and dispersibility of the titanium dioxide. The mass ratio of silicon dioxide to titanium dioxide in the prepared nano titanium dioxide with a surface coated with silicon dioxide is 0.1 to 0.3:1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inorganic nano materials, and particularly relates to an inorganic surface treatment method of nano titanium dioxide, and specifically relates to nano titanium dioxide with a surface coated with silicon dioxide and a preparation method thereof. Background Art

[0002] Nano titanium dioxide can absorb, scatter and reflect ultraviolet rays. It is an excellent medium-wave ultraviolet shielding material and is widely used in cosmetics, plastics, rubber, chemical fiber, coatings and other fields. Titanium dioxide is an N-type semiconductor. When ultraviolet rays with a wavelength less than 400nm irradiate titanium dioxide, the electrons in the valence band can absorb ultraviolet rays and be excited to the conduction band, and electron-hole pairs are generated at the same time. Some electron-hole pairs will migrate to the surface, causing the hydroxyl groups and adsorbed water on the surface of titanium dioxide to produce hydroxyl free radicals. Hydroxyl free radicals have strong oxidizing ability and will oxidize and decompose the surrounding organic matter. Due to the small particle size of nano titanium dioxide, the time for holes and electrons to reach the crystal surface from the inside of the crystal is shortened, reducing the probability of holes and electrons recombination, so nano titanium dioxide has higher photocatalytic activity. When nano titanium dioxide is added to an organic system, it is very easy to cause degradation and discoloration of the surrounding organic medium under the irradiation of ultraviolet rays. Therefore, in order to enhance the photostability of nano titanium dioxide, it is necessary to perform inorganic surface treatment on it. Inorganic surface treatment uses nano-titanium dioxide particles as the core, and establishes a barrier between the nano-titanium dioxide particles and the surrounding medium through inorganic doping or surface densification coating, thereby improving the photostability of nano-titanium dioxide. Coating the surface of nano-titanium dioxide with a silicon dioxide layer is an effective method to inhibit its photoactivity. At present, the silicon sources used for silicon coating the surface of nano-titanium dioxide are ethyl orthosilicate, sodium silicate and potassium silicate, etc., which are relatively expensive and have a complicated operation process. In particular, it is difficult to ensure that the nano-titanium dioxide particles are surface treated in a fully dispersed state, resulting in poor uniformity and density of the silicon dioxide coating layer on the surface of nano-titanium dioxide. The photostability and dispersibility of nano-titanium dioxide need to be further improved. Summary of the invention

[0003] In view of the problems existing in the background technology, the present invention proposes a nano titanium dioxide with a surface coated with silicon dioxide and a preparation method thereof, that is, a method for depositing a uniform and dense silicon dioxide coating layer on the surface of nano titanium dioxide. The silicon dioxide is an amorphous structure, wherein the mass ratio of silicon dioxide to titanium dioxide is 0.1 to 0.3:1.

[0004] The technical solution adopted by the present invention is as follows:

[0005] A method for preparing nano titanium dioxide with a surface coated with silicon dioxide comprises the following steps:

[0006] (1) Add nano-titanium dioxide and wollastonite to deionized water to prepare a slurry with a solid content of 15-30%, and grind at a temperature of 10-30° C. for 2-3 hours to prepare a nano-titanium dioxide and wollastonite dispersion slurry.

[0007] (2) The temperature of the dispersion slurry obtained in step (1) is maintained at 40-50° C., and an acid solution is added while sand milling to adjust the pH value of the system to 4-5. The sand milling reaction time is 2-4 hours, and then the temperature is raised to 70-90° C., the pH value of the system is adjusted to 2-3, and the sand milling reaction time is 3-5 hours.

[0008] The temperature is controlled at 40-50°C, and the acid solution is slowly added to make the wollastonite react slowly to avoid excessive heat release. The temperature is further controlled at 70-90°C, and the pH value is adjusted to 2-3 to make the wollastonite react completely and promote heterogeneous nucleation of silicon dioxide on the surface of nano-titanium dioxide.

[0009] (3) Filtering and washing with deionized water. When the conductivity of the filtrate is less than 100 μS / cm, the washing is completed. The obtained filter cake is dried and crushed to obtain nano-titanium dioxide with dense silicon coating on the surface.

[0010] Furthermore, the amount of wollastonite used in step (1) is based on the mass of silicon dioxide in the wollastonite, and the mass ratio of silicon dioxide to titanium dioxide is 0.1 to 0.3:1.

[0011] Furthermore, the concentration of the acid solution in step (2) is 1 to 3 mol / L.

[0012] Furthermore, the acid in step (2) is one or both of hydrochloric acid and nitric acid.

[0013] Beneficial effects of the present invention:

[0014] 1. The present invention uses wollastonite as a silicon source, controls the solid-liquid reaction rate by controlling temperature and acidity, and causes wollastonite to slowly generate silicon dioxide, which promotes heterogeneous nucleation on the surface of nano-titanium dioxide to form a uniform and continuous silicon dioxide coating layer, thereby greatly improving the light stability of titanium dioxide.

[0015] 2. The present invention performs the acid hydrolysis reaction of wollastonite and the coating reaction of silicon dioxide deposited on the surface of nano-titanium dioxide while sand grinding, thereby ensuring that the nano-titanium dioxide particles are surface treated in a fully dispersed state, reducing the adhesion and agglomeration between the nano-titanium dioxide particles, improving the uniformity and density of the surface silicon coating, and being beneficial to improving the light stability and dispersibility of titanium dioxide.

[0016] 3. The raw material cost of the present invention is low and the process operation is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a high-resolution transmission electron microscope photograph of Example 2;

[0018] Figure 2 This is a high-resolution transmission electron microscope photograph of Comparative Example 1. DETAILED DESCRIPTION

[0019] The sand mill used in the embodiments and comparative examples is a 1-SDM vertical sand mill produced by Qingdao Lianrui Precision Machinery Co., Ltd.

[0020] The nano-titanium dioxide used in the examples and comparative examples is rutile nano-titanium dioxide powder with an average primary particle size of 15 nanometers, produced by Jiangsu Naou New Materials Co., Ltd.

[0021] The wollastonite powder used in the examples and comparative examples has the following components: SiO2 48% to 53%, CaO 43% to 45%, particle size: 200 mesh, and is produced by: Xinyu Nanfang Wollastonite Co., Ltd.

[0022] Example 1

[0023] 1. Add 12 kg of 0.5 mm diameter zirconia balls, 2250 g of deionized water, 377.1 g of nano-titanium dioxide powder and 72.9 g of wollastonite powder (containing 37.7 g of SiO2) to a sand mill lined with zirconia, prepare a slurry with a solid content of 15%, and sand mill for 2 hours at 10°C to prepare a nano-titanium dioxide and wollastonite dispersion slurry.

[0024] 2. Maintain the temperature of the dispersed slurry obtained in step 1 at 40°C, add 1 mol / L hydrochloric acid solution while sand grinding, adjust the pH value of the system to 4, and sand grinding reaction time for 2 hours, then heat to 70°C, adjust the pH value of the system to 2, and sand grinding reaction time for 3 hours.

[0025] 3. Filter and wash with deionized water. When the conductivity of the filtrate is 90 μS / cm, the washing is completed. The obtained filter cake is dried and crushed to obtain nano-titanium dioxide with silicon on the surface. The mass ratio of silicon dioxide to titanium dioxide is 0.1:1.

[0026] Example 2

[0027] 1. Add 9 kg of 0.5 mm diameter zirconia balls, 2100 g of deionized water, 567.6 g of nano-titanium dioxide powder and 330.6 g of wollastonite powder (containing SiO2 171.1 g) to a sand mill lined with zirconia in turn to prepare a slurry with a solid content of 30%. Sand mill at 30°C for 3 hours to prepare a nano-titanium dioxide and wollastonite dispersion slurry.

[0028] 2. Maintain the temperature of the dispersed slurry obtained in step 1 at 50°C, add 3 mol / L hydrochloric acid solution while sand grinding, adjust the pH value of the system to 5, and sand grinding reaction time for 4 hours, then raise the temperature to 90°C, adjust the pH value of the system to 3, and sand grinding reaction time for 5 hours.

[0029] 3. Filter and wash with deionized water. When the conductivity of the filtrate is 86 μS / cm, the washing is completed. The obtained filter cake is dried and crushed to obtain nano-titanium dioxide with silicon on the surface. The mass ratio of silicon dioxide to titanium dioxide is 0.3:1.

[0030] Example 3

[0031] 1. Add 11 kg of 0.5 mm diameter zirconia balls, 2400 g of deionized water, 432.6 g of nano-titanium dioxide powder and 167.4 g of wollastonite powder (containing 86.6 g of SiO2) to a sand mill lined with zirconia, prepare a slurry with a solid content of 20%, and sand mill for 2.5 hours at 20°C to prepare a nano-titanium dioxide and wollastonite dispersion slurry.

[0032] 2. Maintain the temperature of the dispersed slurry obtained in step 1 at 45°C, add 2 mol / L hydrochloric acid solution while sand grinding, adjust the pH value of the system to 4.5, and sand grinding reaction time for 3 hours, then raise the temperature to 80°C, adjust the pH value of the system to 2.5, and sand grinding reaction time for 4 hours.

[0033] 3. Filter and wash with deionized water. When the conductivity of the filtrate is 70 μS / cm, the washing is completed. The obtained filter cake is dried and crushed to obtain nano-titanium dioxide with silicon on the surface. The mass ratio of silicon dioxide to titanium dioxide is 0.2:1.

[0034] Comparative Example 1

[0035] 1. Add 11 kg of 0.5 mm diameter zirconia balls, 2400 g of deionized water, and 600 g of nano-titanium dioxide powder to a sand mill lined with zirconia to prepare a slurry with a solid content of 20%. Adjust the pH value of the system to 10 with 10% sodium hydroxide solution. Sand mill for 2.5 hours at 20°C to prepare a nano-titanium dioxide dispersion slurry.

[0036] 2. The dispersion obtained in step 1 was transferred into a stirred reactor, heated to 90°C, and 6 liters of 0.5 mol / L sodium silicate solution were slowly added to the dispersion while stirring, and 1 mol / L hydrochloric acid solution was slowly added at the same time, and the pH value of the system was maintained at 9.5-10.5. The stirring reaction time was 6 hours. After the sodium silicate solution was added, the stirring was continued for 1 hour, and then the pH value of the system was adjusted to 6 with hydrochloric acid solution while stirring, and the stirring was continued for 2 hours.

[0037] 3. Filter and wash with deionized water. When the conductivity of the filtrate is 60 μS / cm, the washing is completed. The obtained filter cake is dried and crushed to obtain nano-titanium dioxide with silicon on the surface. The mass ratio of silicon dioxide to titanium dioxide is 0.3:1.

[0038] Determination of photostability of nano-titanium dioxide

[0039] Mix the sample to be tested with 1,3-butanediol at a mass ratio of 1:1, apply it on a glass slide at a certain thickness, cover it with a cover glass, and measure its L, a, and b values ​​with an SC-80C colorimeter. Try to avoid sunlight for the above operation. Place the sample plate under a high-pressure mercury lamp (250W) for 1 hour, then take it out and use a colorimeter to measure the L after illumination. * 、a * , b * Value, and use the following formula to calculate the color difference △E of the sample before and after illumination.

[0040] △E=[(LL * ) 2 +(aa * ) 2 +(bb * ) 2 ] 1 / 2 .

[0041] Where L is the brightness coordinate, a and b are the chromaticity coordinates. +a is the red direction, -a is the green direction; +b is the yellow direction, -b is the blue direction. The larger the △E, the higher the photocatalytic activity of nano-titanium dioxide, that is, the worse the photostability.

[0042] Table 1 is a comparison of the color difference of the products obtained in the embodiment and the comparative example. It can be seen from Table 1 that the products obtained by the present invention have excellent light stability, which also shows that the technology of the present invention can form a uniform, continuous and dense silica coating layer on the surface of titanium dioxide, which is consistent with the transmission electron microscopy observation.

[0043] Table 1 Color difference of different products

[0044]

[0045] Determination of the Dispersion of Nano-TiO2

[0046] Weigh 1g of powder and place it in a 200mL beaker, and add 100mL of deionized water. Use a JYD-650 ultrasonic cell crusher to ultrasonically crush 40 times to prepare a powder dispersion. Dilute the dispersion to 40mg / L, use a quartz cuvette with a light path of 1cm to test, use deionized water as a reference, and measure the transmittance at 250-800nm ​​on a Lamda950 UV-visible spectrophotometer (PE Company, USA, with an integrating sphere). The transmittance at 308nm is measured using T 308 It is said that the reflection is the shielding ability of nano titanium dioxide against medium-wave ultraviolet rays (UVB). 308 The smaller it is, the better the ability to shield UVB is; the transmittance at 524nm is expressed by T 524 It indicates that the reflection is the ability of nano-titanium dioxide to transmit visible light. 524 The larger the value, the better the light transmittance. The transmittance of nano-titanium dioxide to visible light and the shielding of nano-titanium dioxide to UVB are closely related to its dispersibility. Under the same original particle size, the better the dispersibility of nano-titanium dioxide, the higher the T 308 The smaller the T 524 The bigger.

[0047] Table 2 shows the light transmittance of the products obtained in the embodiments and comparative examples in water. It can be seen from Table 2 that the products obtained in the present invention have a very strong shielding ability against UVB (T 308 =0), and has good transmittance to visible light, indicating that this product has excellent dispersibility.

[0048] Table 2 Light transmittance of different products

[0049]

[0050] Figure 1 This is a high-resolution transmission electron microscope photograph of Example 2. Figure 2 This is a high-resolution transmission electron microscope photo of Comparative Example 1. From the high-resolution transmission electron microscope photo, it can be seen that the surface of the nano-titanium dioxide in the embodiment has a uniform and dense silicon dioxide coating layer, while the uniformity, continuity and density of the silicon dioxide coating layer in the comparative example are poor.

Claims

1. A method for preparing nano titanium dioxide with surface coated with silicon dioxide, characterized in that: The specific steps include: (1) Adding nano-titanium dioxide and wollastonite to deionized water to prepare a slurry with a solid content of 15 to 30%, and sand-milling for 2 to 3 hours at a temperature of 10 to 30° C. to prepare a dispersion slurry of nano-titanium dioxide and wollastonite; the amount of wollastonite is converted according to the mass of silicon dioxide in the wollastonite, and the mass ratio of silicon dioxide to titanium dioxide is 0.1 to 0.3:1; (2) adding an acid solution to the dispersion slurry obtained in step (1) at a temperature of 40 to 50° C. and under sand milling conditions to adjust the pH value of the system to 4 to 5, and the sand milling reaction time is 2 to 4 hours; controlling the reaction temperature to 70 to 90° C., adding an acid solution to adjust the pH value of the system to 2 to 3, and the sand milling reaction time is 3 to 5 hours; the concentration of the acid solution is 1 to 3 mol / L; (3) Filtering and washing with water until the conductivity of the filtrate is less than 100 μS / cm, drying and crushing the obtained filter cake to obtain nano-titanium dioxide with surface coated with silicon dioxide.

2. The method for preparing nano titanium dioxide with surface coated with silicon dioxide according to claim 1, characterized in that: The acid solution in step (2) is one or both of hydrochloric acid and nitric acid.

3. A nano-titanium dioxide with a surface coated with silicon dioxide prepared by the method according to any one of claims 1 to 2.

4. The nano titanium dioxide with surface coated with silicon dioxide according to claim 3, characterized in that: Silicon dioxide is uniformly and densely deposited on the surface of nano-titanium dioxide to form a silicon dioxide coating layer; the silicon dioxide is an amorphous structure.