Gel electrolyte precursor, hydrogel film, gel electrolyte, sodium-zinc mixed ion battery and preparation method thereof

By constructing a gel electrolyte with amide groups, the problems of zinc dendrite growth and electrolyte leakage in sodium-zinc mixed ion batteries are solved, high ionic conductivity and good high-voltage stability are achieved, and the battery cycle is improved. longevity and overall performance.

CN116693761BActive Publication Date: 2024-10-01CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310175740.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2024-10-01
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

Due to the growth of zinc dendrites, electrolyte leakage and slow ion diffusion kinetics in sodium-zinc mixed ion batteries, the interfacial layer deposition is uneven, the strength is low, the ionic conductivity of the solid electrolyte is low, the cost of highly concentrated electrolyte is high, and the application effect is poor. ideal.

Method used

Silicone coupling agents, alginates and monomers with amide groups are used to construct gel electrolytes through photocuring methods to form semi-solid electrolytes, regulate the deposition of zinc ions, improve mechanical strength and ionic conductivity, and inhibit branching. crystal growth.

Benefits of technology

It achieves high ionic conductivity, good high-voltage stability and cycle life, effectively regulates zinc ion deposition, and improves the overall performance of sodium-zinc mixed ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116693761B_ABST
    Figure CN116693761B_ABST
Patent Text Reader

Abstract

The present invention relates to a gel electrolyte precursor, a hydrogel film, a gel electrolyte, a sodium-zinc mixed ion battery and a preparation method thereof, wherein the preparation method of the gel electrolyte precursor comprises: step 1: taking a certain volume of water and adding it to a container, adding a siloxane coupling agent, the siloxane coupling agent having a double bond and a methoxy group at the same time, adjusting the system pH value between 8-9 by an alkaline solution, and continuously stirring and hydrolyzing at 40-45°C; step 2: adding alginate to the solution, heating the system to 50-60°C and stirring the reaction; step 3: adding a monomeric substance with an amide group to the mixed solution, adding a photoinitiator after dissolving, and continuously stirring at room temperature to obtain a gel electrolyte precursor solution. The preparation method of the present invention is simple and easy, the gel electrolyte is semi-solid, has high ionic conductivity and good high voltage resistance stability, can regulate metal ions (such as zinc ions) to deposit on the interface, and the battery assembled using the gel electrolyte of the present invention has a high cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of ion batteries, and in particular to a gel electrolyte precursor, a hydrogel membrane, a gel electrolyte, a sodium-zinc mixed ion battery and a preparation method thereof. Background Art

[0002] With the rapid development of the global economy, the shortage of traditional fossil energy and environmental pollution problems have become increasingly prominent, causing the energy configuration to gradually shift from non-renewable energy such as coal, oil, and natural gas to clean energy such as solar energy, wind energy, and ocean energy. However, the development of clean energy depends on changes in the natural environment and cannot be used efficiently. Therefore, the development of efficient electrochemical energy storage devices is an urgent task to achieve a continuous and stable supply of energy. However, lithium-ion batteries are currently dominated by organic electrolytes, which have the risk of electrolyte leakage and flammability and explosion. In addition, lithium resources are limited and battery costs are high. Therefore, the development of aqueous sodium-ion and aqueous zinc-ion batteries has received widespread attention recently. They can avoid the defects of organic electrolytes and are expected to develop into the next generation of ion batteries. Metallic zinc negative electrode materials are abundant in resources, have high theoretical capacity (820mAh / g) and low equilibrium potential (-0.763V versus the standard hydrogen electrode), and have good stability in water. Therefore, it is one of the most widely studied negative electrode materials in aqueous batteries. Aqueous sodium-ion batteries have lower costs and higher power, and are an ideal large-scale energy storage technology. Combining zinc negative electrodes with high-rate sodium positive electrode materials can be well applied to large-scale energy storage occasions with high safety and reliability requirements, frequent charging and discharging, and high operation and maintenance costs. However, due to the growth of zinc dendrites, electrolyte leakage, and slow ion diffusion dynamics, the development of sodium-zinc mixed ion batteries has been restricted. At present, the overall performance of the battery is mainly improved by artificial modification layers, solid electrolytes, and high-concentration electrolytes. However, due to the uneven deposition and low strength of the interface layer under aqueous conditions, the low ion conductivity of the solid electrolyte, and the high cost of high-concentration electrolytes, the application effect has not been ideal. Summary of the invention

[0003] In view of the problems existing in current mixed ion batteries (such as sodium-zinc mixed ion batteries), the main purpose of the present invention is to provide a gel electrolyte precursor, a hydrogel film, a gel electrolyte, a sodium-zinc mixed ion battery and a preparation method thereof. The preparation method of the present invention is simple and easy to implement. The prepared gel electrolyte is semi-solid, has high ionic conductivity and good high voltage stability, can regulate the deposition of metal ions (such as zinc ions) on the interface, and the battery assembled using the gel electrolyte of the present invention has a high cycle life. To achieve the above-mentioned invention purpose, the technical solution provided by the present invention is as follows:

[0004] A first aspect of the present invention provides a method for preparing a gel electrolyte precursor, comprising the following steps:

[0005] Step 1: Take a certain volume of water and add it into a container, add a siloxane coupling agent, the siloxane coupling agent has both double bonds and methoxy groups, the concentration of the siloxane coupling agent is 0.005-0.05 g / ml, adjust the pH value of the system to between 8 and 9 with an alkaline solution, and continue stirring and hydrolyzing at 40-45°C for 1-4 hours;

[0006] Step 2: Add alginate to the solution, wherein the mass ratio of the silicone coupling agent to the alginate is (0.3-3):1, and heat the system to 50-60° C. and stir for reaction for 2-4 hours;

[0007] Step 3: Add monomeric substances with amide groups to the mixed solution in a molar ratio of (10-30):1 to alginate, add a photoinitiator after dissolution, wherein the mass of the photoinitiator is 2.5-7.5% of the mass of the monomeric substances with amide groups, then add a cross-linking agent, wherein the mass of the cross-linking agent is 1-4% of the mass of the monomeric substances with amide groups, and continue stirring at room temperature for 1-3 hours to obtain a solution of a gel electrolyte precursor.

[0008] Preferably, in step 2, the mass ratio of the silicone coupling agent to the alginate is (0.4-2.5):1.

[0009] Preferably, in step 3, the photoinitiator comprises 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0010] A second aspect of the present invention provides a gel electrolyte precursor, which is prepared according to the preparation method described above.

[0011] The third aspect of the present invention provides a hydrogel film, which is obtained by injecting the solution of the gel electrolyte precursor described above into a mold and polymerizing it under ultraviolet light, wherein the mold has a thickness of 0.3-1.5 mm and is polymerized under ultraviolet light with a wavelength of 320-400 nm for 1-2 hours.

[0012] The fourth aspect of the present invention provides a gel electrolyte, which is obtained by drying the hydrogel film described above and immersing it in a mixed electrolyte, wherein the hydrogel film after polymerization is taken out, then placed in an oven and dried at 50-80°C for 20-60 minutes, and finally immersed in a mixed electrolyte containing zinc salt and sodium salt for 2-3 days.

[0013] Preferably, the concentration of the zinc salt is 0.5-2 M, and the concentration of the sodium salt is 0.5-2 M. More preferably, the concentration of the zinc salt is 0.5-1.5 M, and the concentration of the sodium salt is 0.5-1.5 M.

[0014] Preferably, the zinc salt in the mixed electrolyte includes ZnSO4, Zn(TFSI)2, and Zn(Cl)2, and the sodium salt includes Na2SO4, NaTFSI, and NaCl.

[0015] A fifth aspect of the present invention provides a sodium-zinc mixed ion battery, comprising:

[0016] a gel electrolyte layer comprising a gel electrolyte;

[0017] A positive electrode sheet disposed on a first surface of the gel electrolyte layer; and

[0018] A negative electrode sheet is disposed on the second surface of the gel electrolyte layer.

[0019] The sixth aspect of the present invention provides a method for preparing the sodium-zinc mixed ion battery described above,

[0020] The following steps are involved:

[0021] Step A: Preparation of positive electrode sheet: Prussian blue positive electrode active material, binder, and conductive agent are stirred into slurry in a weight ratio of 7-8:1-2:1, coated on titanium foil, dried in a vacuum oven, and then cut into thin sheets as positive electrode sheets. The loading amount of the positive electrode active material is 0.8-1.2 mg / cm 2 ;

[0022] Step B: Battery assembly: Cut the gel electrolyte into thin slices and grind the zinc sheet with fine sandpaper before assembly. The assembly order is positive electrode shell, positive electrode sheet, gel electrolyte, zinc sheet, gasket, shrapnel, and negative electrode shell.

[0023] The beneficial effects of the present invention are as follows: the present invention adopts monomeric substances with amide groups (such as acrylamide monomers, including N-hydroxymethyl acrylamide) and uses alginate (such as sodium alginate) as a reinforcement. Through the method of photocuring, vinyl silane is used to cross-link the alginate chain and the monomeric substances with amide groups (such as acrylamide monomers, including N-hydroxymethyl acrylamide) chains. The advantage of this design is that the interface chemical bonding between the monomeric substances with amide groups (such as acrylamide monomers, including N-hydroxymethyl acrylamide) chains and the alginate (such as sodium alginate) chains is constructed in situ by the hydrolyzed siloxane coupling agent (such as vinyl trimethoxysilane). In addition, metal ions (such as zinc ions) can cross-link different alginate (such as sodium alginate) chains to form ionic bonds. These interactions effectively improve the mechanical strength of the gel electrolyte. The negatively charged surface -NH-CH2-OH and -COO -A transport channel for metal ions (such as zinc ions) is constructed, so that the gel electrolyte has high ionic conductivity, and the surface carboxyl groups regulate the deposition of metal ions (such as zinc ions) on the interface, inhibiting dendrite growth.

[0024] The features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The synthetic route of gel electrolyte.

[0026] Figure 2 Characterization of mechanical properties and morphology.

[0027] Figure 3 For infrared and XPS characterization.

[0028] Figure 4 For lsv and impedance testing.

[0029] Figure 5 Symmetrical battery testing and characterization of zinc sheet morphology after cycling.

[0030] Figure 6 This is a battery performance test chart. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and beneficial effects of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. Examples of the embodiments are shown in the accompanying drawings. It should be understood that the specific embodiments described in the following embodiments of the present invention are only exemplary descriptions of the specific embodiments of the present invention, and are intended to be used to explain the present invention, but do not constitute a limitation of the present invention.

[0032] The endpoints and any value of the scope disclosed in this article are not limited to this accurate scope or value, and these scopes or values ​​should be understood as comprising values ​​close to these scopes or values.For numerical range, between the endpoint values ​​of each scope, between the endpoint values ​​of each scope and a separate point value, and between separate point values, can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered as specifically disclosed in this article.In the description of the application, unless otherwise stated, the meaning of similar words such as "multiple / multiple" is two / kinds or more than two / kinds.In addition, the terms "include", "comprise" and any distortion thereof are intended to cover non-exclusive inclusions.

[0033] A first aspect of the present invention provides a method for preparing a gel electrolyte precursor, comprising the following steps:

[0034] Step 1: Take a certain volume of water and add it into a container, add a siloxane coupling agent, the siloxane coupling agent has both double bonds and methoxy groups, the concentration of the siloxane coupling agent is 0.005-0.05 g / ml, adjust the pH value of the system to between 8 and 9 with an alkaline solution, and continue stirring and hydrolyzing at 40-45°C for 1-4 hours;

[0035] Step 2: Add alginate to the solution, wherein the mass ratio of the silicone coupling agent to the alginate is (0.3-3):1, and heat the system to 50-60° C. and stir for reaction for 2-4 hours;

[0036] Step 3: Add monomeric substances with amide groups to the mixed solution in a molar ratio of (10-30):1 to alginate, add a photoinitiator after dissolution, wherein the mass of the photoinitiator is 2.5-7.5% of the mass of the monomeric substances with amide groups, then add a cross-linking agent, wherein the mass of the cross-linking agent is 1-4% of the mass of the monomeric substances with amide groups, and continue stirring at room temperature for 1-3 hours to obtain a gel electrolyte precursor solution.

[0037] In the present invention, the type of the siloxane coupling agent in step 1 can be selected from a wide range, as long as it is a siloxane coupling agent with both a double bond and a methoxy group, such as vinyl trimethoxysilane and allyl trimethoxysilane. In some preferred embodiments, in order to obtain a better coupling effect and better reactivity when reacting with sodium alginate to form a chemical bond, the siloxane coupling agent is vinyl trimethoxysilane.

[0038] In the present invention, the concentration of the siloxane coupling agent in step 1 is 0.005-0.05 g / ml, preferably 0.01 g / ml.

[0039] In the research of the present invention, the inventors found that acrylic acid, as a comparative sample, was less reactive than vinyl trimethoxysilane in forming chemical bonds with sodium alginate.

[0040] In the present invention, the alkaline solution in step 1 can be selected within a wide range, and is selected according to the ion battery system to which the gel electrolyte precursor is applied. In some embodiments of the present invention, the gel electrolyte prepared by the gel electrolyte precursor is applied to a sodium-zinc mixed ion battery system. In order to prevent the introduction of other impurities, the alkaline solution is preferably sodium hydroxide. In other embodiments of the present invention, the gel electrolyte prepared by the gel electrolyte precursor is applied to other mixed ion battery systems, such as lithium-zinc and potassium-zinc battery systems, and lithium hydroxide or potassium hydroxide salts can be used. It is worth noting that the ion battery system to which the gel electrolyte precursor is applied includes the mixed electrolyte described later. In order to prevent the introduction of other impurities, a salt suitable for the corresponding ion battery system can also be selected, such as ZnSO4+Li2SO4 (ZnSO4+K2SO4).

[0041] In the present invention, the hydrolysis is carried out under continuous stirring at 40-45°C in step 1, preferably at 40°C.

[0042] In the present invention, the hydrolysis is continued with stirring for 1-4 hours, preferably 3 hours in step 1.

[0043] In the present invention, step 2 is mainly to form a more stable interfacial chemical bond, and alginate increases the gel strength. In step 2, the mass ratio of the silicone coupling agent to the alginate is (0.3-3):1, and preferably the mass ratio of the silicone coupling agent to the sodium alginate is (0.4-2.5):1. More preferably, the mass ratio of the silicone coupling agent to the sodium alginate is 3:7, 7:3 or 5:5.

[0044] In the present invention, the alginate in step 2 can be selected according to the ion battery system. In some preferred embodiments, in order to further form a more stable interfacial chemical bond, the alginate further increases the gel strength, and the alginate is preferably sodium alginate and / or zinc alginate. In some more preferred embodiments, in order to further form a more stable interfacial chemical bond, the alginate further increases the gel strength, and the alginate is sodium alginate.

[0045] In the present invention, the monomer substance with an amide group in step 3 has the function of locking in water and retaining moisture. The monomer substance contains a double bond and can be selected in a wide range. In order to obtain a better effect of locking in water and retaining moisture, an acrylamide monomer is preferred, and the acrylamide monomer includes N-hydroxymethyl acrylamide and acrylamide.

[0046] In the present invention, the photoinitiator in step 3 can be selected from a wide range, such as 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0047] In the present invention, the crosslinking agent can be selected from a wide range, such as N,N methylenebisacrylamide, ethylene glycol diacrylate, 1,6-hexanediol diacrylate. In some preferred embodiments, in order to obtain a better crosslinking effect, the crosslinking agent is N,N methylenebisacrylamide.

[0048] In the present invention, the mass of the photoinitiator is 2.5-7.5% of the mass of the monomeric substance with an amide group or a carboxyl group, preferably 5%.

[0049] In the present invention, the mass of the cross-linking agent is 1-4%, preferably 2.5%, of the mass of the monomers with amide groups or carboxyl groups.

[0050] A second aspect of the present invention provides a gel electrolyte precursor, which is prepared according to the preparation method described above.

[0051] The gel electrolyte precursor of the present invention can be used as an intermediate raw material of a battery, which is more convenient to transport or store, and can be used to produce a gel electrolyte under appropriate circumstances. The gel electrolyte precursor of the present invention can be applied to different mixed ion battery systems, such as a sodium-zinc mixed ion battery system, a lithium-zinc mixed ion battery system, and a potassium-zinc mixed ion battery system, preferably a sodium-zinc mixed ion battery system.

[0052] The third aspect of the present invention provides a hydrogel film, which is obtained by injecting the solution of the gel electrolyte precursor described above into a mold and polymerizing it under ultraviolet light, wherein the mold has a thickness of 0.3-1.5mm, preferably 0.5-1.2mm, and is polymerized under ultraviolet light with a wavelength of 320-400nm, preferably 365nm, for 1-2h.

[0053] The hydrogel membrane of the present invention can be used as an intermediate raw material of a battery, which is more convenient to transport or store, and can be used to produce a gel electrolyte under appropriate circumstances. The hydrogel membrane of the present invention can be applied to different mixed ion battery systems, such as a sodium-zinc mixed ion battery system, a lithium-zinc mixed ion battery system, and a potassium-zinc mixed ion battery system, preferably a sodium-zinc mixed ion battery system.

[0054] The fourth aspect of the present invention provides a gel electrolyte, which is a semi-solid gel electrolyte with high ionic conductivity and good high voltage stability, and can regulate the deposition of metal ions (especially zinc ions) on the interface and inhibit dendrite growth. The above-mentioned hydrogel film is dried and immersed in a mixed electrolyte to obtain the gel electrolyte, wherein the hydrogel film after polymerization is taken out, and then placed in an oven at 50-80°C for 20-60 minutes, and finally immersed in a mixed electrolyte containing zinc salt and sodium salt for 2-3 days.

[0055] In the fourth aspect of the present invention, in order to make the gel electrolyte obtain a more stable semi-solid state, further have higher ionic conductivity and better high voltage stability, better regulate the deposition of metal ions (especially zinc ions) on the interface, inhibit dendrite growth and other effects, preferably, the hydrogel film after polymerization is taken out and then placed in an oven for drying at 65°C.

[0056] In the fourth aspect of the present invention, in order to make the gel electrolyte obtain a more stable semi-solid state, further have higher ionic conductivity and better high voltage stability, better regulate the deposition of metal ions (especially zinc ions) on the interface, inhibit dendrite growth and other effects, preferably, the hydrogel film after polymerization is taken out and then placed in an oven for drying for 40 minutes.

[0057] In the fourth aspect of the present invention, due to the high external ion concentration of the hydrogel membrane during immersion, the ions will penetrate into the interior of the hydrogel membrane through the action of osmotic pressure, and finally reach a penetration / escape equilibrium state with the external electrolyte. The prepared gel electrolyte has high ionic conductivity and good high voltage stability, can regulate the deposition of metal ions (especially zinc ions) on the interface, and inhibit dendrite growth. The battery assembled using the gel electrolyte of the present invention has a high cycle life.

[0058] In the present invention, the composition of the mixed electrolyte depends on different mixed ion battery systems, such as sodium zinc mixed ion battery system, lithium zinc mixed ion battery system, potassium zinc mixed ion battery system, etc. By soaking in different mixed electrolytes, it can be applied to different mixed ion battery systems, such as soaking in sodium chloride + magnesium chloride electrolyte, it can be applied to sodium magnesium mixed ion battery. That is to say, the mixed electrolyte can also be composed of sodium chloride + magnesium chloride, sodium chloride + aluminum chloride, etc. according to the ion battery system, and the content can be 1M + 1M, or 2M + 2M, and the content is mainly adjusted appropriately according to the solubility of the salt.

[0059] In order to prevent the introduction of other impurities, avoid the entire reaction mechanism from becoming complicated, and likely to have a negative impact on the conductivity and stability of the gel electrolyte, components suitable for the corresponding mixed ion battery system are selected. In some preferred embodiments, the mixed electrolyte is used to prepare the gel electrolyte in the sodium-zinc mixed ion battery system, and the mixed electrolyte can be selected from sodium salts and zinc salts commonly used in mixed ion batteries, such as zinc salts including ZnSO4, Zn(TFSI)2, and Zn(Cl)2, and the sodium salts include Na2SO4, NaTFSI, and NaCl.

[0060] The solubility of salt in water is limited. Too low a concentration will result in the inability to achieve ion equilibrium, which will have a negative impact on the ionic conductivity and stability of the gel electrolyte, the deposition of zinc ions on the interface, and the cycle life of the battery assembled with the gel electrolyte. Therefore, salts with higher solubility can be used as the experimental system, but the solubility of the electrolyte cannot be too high. Too high a salt concentration will increase the viscosity inside the gel, which will hinder ion diffusion and affect the rate performance of the battery. In addition, salt is more likely to precipitate and crystallize at low temperatures, which limits the scope of use of the battery.

[0061] In the present invention, preferably, the concentration of the zinc salt is 0.5-2 M, and the concentration of the sodium salt is 0.5-2 M. More preferably, the concentration of the zinc salt is 0.5-1.5 M, and the concentration of the sodium salt is 0.5-1.5 M.

[0062] In some other embodiments, the mixed electrolyte is used to prepare a gel electrolyte in a lithium-zinc mixed ion battery system, and the mixed electrolyte may contain lithium salts and zinc salts commonly used in mixed ion batteries, such as ZnSO4+Li2SO4.

[0063] In some other embodiments, the mixed electrolyte is used to prepare a gel electrolyte in a potassium-zinc mixed ion battery system, and the mixed electrolyte may contain potassium salts and zinc salts commonly used in mixed ion batteries, such as Zn(FSI)2+KFSI.

[0064] In a fifth aspect of the present invention, a sodium-zinc mixed ion battery is provided, comprising:

[0065] a gel electrolyte layer comprising a gel electrolyte;

[0066] A positive electrode sheet disposed on a first surface of the gel electrolyte layer; and

[0067] A negative electrode sheet is disposed on the second surface of the gel electrolyte layer.

[0068] In a sixth aspect of the present invention, a method for preparing a sodium-zinc mixed ion battery is provided, comprising the following steps:

[0069] Step A: Preparation of positive electrode sheet: Prussian blue positive electrode active material, binder, and conductive agent are stirred into slurry in a weight ratio of 7-8:1-2:1, coated on titanium foil, dried in a vacuum oven, and then cut into thin sheets as positive electrode sheets. The loading amount of the positive electrode active material is 0.8-1.2 mg / cm 2 ;

[0070] Step B: Battery assembly: Cut the gel electrolyte into thin slices and grind the zinc sheet with fine sandpaper before assembly. The assembly order is positive electrode shell, positive electrode sheet, gel electrolyte, zinc sheet, gasket, shrapnel, and negative electrode shell.

[0071] In the present invention, the binder in step A is PVDF and its analogs, preferably PVDF.

[0072] In the present invention, the conductive agent in step A is commonly used in batteries, preferably, the conductive agent is at least one of carbon black conductive agents (such as conductive carbon black, SP (Super-P)). In addition, preferably, in order to increase the conductive effect, carbon nanotubes can also be added.

[0073] In the sixth aspect of the present invention, the temperature for drying in the vacuum oven in step A can be selected within a wide range, preferably, drying at 80-100°C, more preferably, drying at 80°C.

[0074] In the sixth aspect of the present invention, the drying time in the vacuum oven in step A can be selected within a wide range, preferably, the drying time is 10-15 hours, and more preferably, the drying time is 12 hours.

[0075] In the sixth aspect of the present invention, the slices cut in step A are preferably circular, more preferably have a diameter of 10-14 mm, and most preferably 12 mm.

[0076] In the sixth aspect of the present invention, the slices cut from the gel electrolyte in step B are preferably circular, more preferably have a diameter of 17-19 mm, and most preferably 18 mm.

[0077] The present invention will be described in detail below by way of examples. In the following examples, the drugs and medicaments are all conventional commercial products.

[0078] Example 1: This embodiment of the present invention provides a method for preparing a gel electrolyte

[0079] A method for preparing a gel electrolyte comprises the following steps:

[0080] Step 1: Take 15 ml of water and add it into a container, add 0.15 g of vinyl trimethoxysilane, adjust the pH value of the system to between 8 and 9 with an alkaline solution, and continue stirring and hydrolyzing at 45°C for 3 hours;

[0081] Step 2: Add 0.35 g of sodium alginate to the solution, heat the system to 55°C and stir for 3 hours;

[0082] Step 3: Add 3.572 g of monomer N-hydroxymethyl acrylamide to the mixed solution, add 17.86 mg of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone and 8.93 mg of N,N-methylenebisacrylamide after dissolving, and continue stirring at room temperature for 2 h to obtain a gel electrolyte precursor solution;

[0083] Step 4: inject the gel electrolyte precursor solution into a mold with a thickness of 0.8 mm, and polymerize it under 365 nm ultraviolet light for 1 h to obtain a hydrogel film;

[0084] Step 5: After the polymerization is completed, the hydrogel film is taken out and placed in an oven for drying at 65°C for 40 minutes, and finally immersed in a 1M ZnSO4 + 1M Na2SO4 mixed electrolyte for 2 days to obtain a gel electrolyte a.

[0085] Example 2: The present invention provides a method for preparing a gel electrolyte

[0086] A method for preparing a gel electrolyte precursor comprises the following steps:

[0087] Step 1: Take 10 ml of water and add it into a container, add 0.35 g of vinyl trimethoxysilane, adjust the pH value of the system to between 8 and 9 with an alkaline solution, and continue stirring and hydrolyzing at 40°C for 3 hours;

[0088] Step 2: Add 0.36 g of sodium alginate to the solution, heat the system to 50°C and stir for 2 h;

[0089] Step 3: Add 1.786 g of monomer N-hydroxymethyl acrylamide to the mixed solution, add 0.893 mg of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone and 4.465 mg of N,N-methylenebisacrylamide after dissolving, and continue stirring at room temperature for 1 hour to obtain a gel electrolyte precursor solution;

[0090] Step 4: Inject the precursor solution into a mold with a thickness of 0.5 mm and polymerize it under 365 nm ultraviolet light for 2 h to obtain a hydrogel film;

[0091] Step 5: After the polymerization is completed, the hydrogel electrolyte is taken out and placed in an oven at 50°C (preferably 65°C) for drying for 60 minutes, and finally immersed in a 0.5M ZnSO4+0.5M Na2SO4 mixed electrolyte for 3 days to obtain a gel electrolyte b.

[0092] Example 3: The present invention provides a method for preparing a gel electrolyte

[0093] A method for preparing a gel electrolyte comprises the following steps:

[0094] Step 1: Take 20 ml of water and add it into a container, add 0.817 g of vinyl trimethoxysilane, adjust the pH value of the system to between 8 and 9 with an alkaline solution, and continue stirring and hydrolyzing at 40°C for 3 hours;

[0095] Step 2: Add 0.35 g of sodium alginate to the solution, heat the system to 60°C and stir for 4 hours;

[0096] Step 3: Add 5.358 g of monomer N-hydroxymethyl acrylamide to the mixed solution, add 26.79 mg of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone and 13.395 mg of N,N-methylenebisacrylamide after dissolving, and continue stirring at room temperature for 3 hours to obtain a gel electrolyte precursor solution;

[0097] Step 4: injecting the precursor solution into a mold with a thickness of preferably 1.2 mm, and polymerizing it under 365 nm ultraviolet light for 2 h to obtain a hydrogel film;

[0098] Step 5: After the polymerization is completed, the hydrogel electrolyte is taken out and placed in an oven for drying at 80°C for 20 minutes, and finally immersed in a 1.5M ZnSO4+1.5M Na2SO4 mixed electrolyte to obtain gel electrolyte c.

[0099] Example 4: The present invention provides a method for preparing a sodium-zinc mixed ion battery

[0100] A method for preparing a sodium-zinc mixed ion battery comprises the following steps:

[0101] Step A: Preparation of positive electrode sheet: Prussian blue positive electrode active material, binder PVDF, and conductive carbon black Super-P are stirred into slurry in a weight ratio of 8:1:1, coated on titanium foil, dried in a vacuum oven at 80°C for 12 hours, and then cut into circular sheets with a diameter of 12 mm as positive electrode sheets. The loading amount of the positive electrode active material is 0.8-1.2 mg / cm 2 ;

[0102] Step B: Battery assembly: Cut the gel electrolyte a into circular sheets with a diameter of 18 mm. Grind the zinc sheet with fine sandpaper before assembly. The assembly order is positive electrode shell, positive electrode sheet, gel electrolyte a, zinc sheet, gasket, shrapnel, and negative electrode shell.

[0103] Test Example 1:

[0104] This test example provides the mechanical properties and morphology characterization of the gel electrolyte prepared in Example 1

[0105] This experiment uses a S-4800 scanning electron microscope with a shooting size of 1 micron. The experimental process is to first freeze-dry the gel electrolyte in a freeze dryer, and then cut the freeze-dried film sample into 3*3mm 2 The sheet was then attached to the conductive adhesive for testing.

[0106] Result analysis: Figure 2 A is an optical image of a hydrogel electrolyte, which can be bent and stretched, and has high permeability and transparency. The morphology of the hydrogel electrolyte was characterized by SEM. Its interior is a multi-porous structure with a pore diameter of about 1 micron. The uniform pore distribution is conducive to the migration of electrolyte ions, thus giving it excellent ionic conductivity. Figure 2 B is a test of the mechanical properties of the gel electrolyte. When not immersed in electrolyte, there is no ionic bond in the hydrogel and the elongation at break is less than 40%. In the absence of a silicone coupling agent, the elongation at break of the gel electrolyte during stretching can reach about 80%. Although the elongation at break decreases after adding vinyl silane, the tensile strength increases to 0.062Mpa. High mechanical strength is beneficial for inhibiting the growth of dendrites.

[0107] Test Example 2

[0108] This test example provides infrared and XPS characterization of the gel electrolyte prepared in Example 1.

[0109] This experiment uses a Bruker Tensor 27 infrared spectrometer for testing. The sample size of the gel electrolyte is 5*5mm, and ATR attenuated total reflection is used for testing. During the test, the sample surface is smooth and the sample needs to be in close contact with the reflection surface of the total reflection crystal. The sample is placed on the reflection surface of the total reflection crystal for measurement.

[0110] This experiment uses an ESCALAB 250XI X-ray photoelectron spectrometer. During the test, the gel electrolyte is first placed in a freeze dryer for freeze drying to avoid the presence of water in the material. The freeze-dried electrolyte membrane is cut into 4*4mm square pieces and then sent for sample testing.

[0111] Result analysis: Figure 3A proved the valence bond structure of the gel electrolyte by infrared spectroscopy, which are the infrared spectra of the hydrogel electrolyte before and after immersion in the electrolyte. The peak at 1530 belongs to the amide II band formed by the coupling of CN and NH in the secondary amide. The peak intensity is very obvious because the hydrogen bond interaction between HN···HO molecules increases the NH vibration intensity. The infrared peak at 1658 belongs to the -COOH vibration. Compared with the carboxyl vibration of the hydrogel that has not been immersed in the electrolyte, the vibration peak intensity of the carboxyl group increases significantly after immersion in the electrolyte, indicating that the sodium alginate chains are cross-linked by zinc ions. Figure 3 In B, the high-resolution Si 2p spectrum shows two different peaks at 102.5 and 101.8, indicating that Si exists in two different chemical states, proving that vinyl silane is successfully grafted onto SA.

[0112] Test Example 3

[0113] This test example provides the LSV and impedance test of the sodium-zinc mixed ion battery prepared in Example 4.

[0114] In this experiment, LSV and impedance were tested by Shanghai Chenhua ChI760e workstation. LSV was tested using a three-electrode system. A steel sheet / / gel electrolyte / / zinc foil battery was assembled. The steel sheet was used as the working electrode, and the zinc sheet was used as the counter electrode and reference electrode. The impedance was measured at 1 mV s -1 The constant scan rate, the test voltage window is 1-3V, and the decomposition voltage of the test electrolyte is

[0115] Impedance was measured by assembling a steel sheet / / gel electrolyte / / steel sheet battery at open circuit voltage. The impedance test frequency range was 0.01 Hz to 100,000 Hz.

[0116] Result analysis: Figure 4 AThe electrochemical stability window of the gel electrolyte was determined by linear sweep voltammetry. The oxidative decomposition voltage of the gel electrolyte exceeded 2.5V, which was much higher than that of the mixed liquid electrolyte, indicating that it had good electrochemical stability. Steel\\steel batteries were assembled and the ionic conductivity of the gel electrolyte was determined by AC impedance spectroscopy. The impedance values ​​of the liquid electrolyte, the hydrogel before immersion in the electrolyte, and the gel electrolyte after immersion in the electrolyte were 0.54Ω, 8.79Ω, and 0.91Ω, respectively. The ionic conductivity of the gel electrolyte was calculated to be as high as 43mS / cm.

[0117] Test Example 4

[0118] This test example provides a symmetrical battery test of the sodium-zinc hybrid ion battery prepared in Example 4 and the characterization of the zinc sheet morphology after cycling.

[0119] Symmetrical cells: Assembled zinc / / gel electrolyte / / zinc cells and cycled them at different current densities, with the cutoff condition for each cycle being the surface deposited capacity.

[0120] Morphology characterization: The cycled battery was disassembled, and the cycled zinc sheet was first rinsed with deionized water, and then cut into 3*3mm thin sheets after drying. The side of the zinc sheet close to the electrolyte was placed under an S-4800 scanning electron microscope to observe its microscopic morphology.

[0121] Result analysis: Cyclic stability of zinc ion deposition and stripping in different electrolyte systems, Figure 5 A at 0.3 mA / cm -2 At a low current density, the cycle stability in the liquid electrolyte is poor due to dendrite growth, while in the gel electrolyte system, it can cycle for 1400 hours, and the polarization voltage does not increase during the cycle. In addition, at a current density of 1mA / cm-2, based on the gel electrolyte system, it can also stably cycle for 700 hours. The inhibition of zinc dendrite growth is mainly due to the electrostatic interaction between the negatively charged carboxyl groups on the skeleton of the gel electrolyte and the zinc ions, which limits the two-dimensional diffusion of zinc ions and makes the deposition of zinc ions more uniform. SEM characterization of the zinc sheet after 100 cycles, such as Figure 5 As shown in Figure C, there are no dendrites on the surface of the zinc sheet after cycling in the gel electrolyte, while there are vertically grown dendrites on the surface of the zinc sheet after cycling in the liquid electrolyte. Figure 5 D is at 1mA / cm -2 XRD diagram of the zinc sheet after 10 cycles at a current density of . In the liquid electrolyte, due to the hydrogen evolution reaction on the zinc negative electrode side, the alkaline concentration on the surface of the zinc sheet increases, and a layer of hydrated basic zinc sulfate by-product is formed on its surface. This substance inhibits the migration of zinc ions. However, in the gel electrolyte system, no basic zinc sulfate by-product is formed on its surface, which also shows that it has a good inhibitory effect on the hydrogen evolution side reaction.

[0122] Test Example 5

[0123] This test example provides the battery performance of the sodium-zinc mixed ion battery prepared in Example 4.

[0124] The battery was assembled in the order of positive electrode shell, positive electrode sheet, gel electrolyte, zinc sheet, gasket, shrapnel, and negative electrode shell. The battery was tested by the Land test system in Wuhan. 1) Cycle: The battery was charged and discharged at a constant current density (including long cycles at 1C and 25C, 1C = 100mA g -1 ), the cut-off voltage during the cycle is 0.7-1.6V;).

[0125] Result analysis: HQ-NaFe was used as the positive electrode material to assemble the battery. The charging and discharging mechanism of the battery is as follows: Figure 6 As shown in A, zinc ions are deposited and stripped on the negative electrode side, while sodium ions are embedded and removed on the positive electrode side. Figure 6 B is at a low current of 1C. Compared with the liquid electrolyte, the gel electrolyte system can stably cycle 600 times. After the first 100 cycles, the capacity retention rate is 93%, and the average CE reaches 99%. Figure 6 C Under a high current of 25C, the battery also has an initial discharge capacity of 72mAh / g, and can be charged and discharged for 6K cycles. After 6K cycles, the capacity is still 40mAh / g.

[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and do not constitute a limitation on the content of the present invention. Although the present invention has been listed in detail through the above embodiments, those skilled in the art can still make various changes in form and details according to the technical contents described in the summary of the invention and the embodiment part, without departing from the spirit and scope of the present invention defined by the attached claims.

Claims

1. A method for preparing a gel electrolyte precursor, It is characterized in that The steps include: Step 1: Take a certain volume of water and add it into a container, add a siloxane coupling agent, the siloxane coupling agent has both double bonds and methoxy groups, the concentration of the siloxane coupling agent is 0.005-0.05 g / ml, adjust the pH value of the system to between 8 and 9 with an alkaline solution, and continue stirring and hydrolyzing at 40-45°C for 1-4 hours; Step 2: Add alginate to the solution, wherein the mass ratio of the silicone coupling agent to the alginate is (0.3-3):1, and heat the system to 50-60° C. and stir for reaction for 2-4 hours; Step 3: Add monomeric substances with amide groups to the mixed solution in a molar ratio of (10-30):1 to alginate, add a photoinitiator after dissolution, wherein the mass of the photoinitiator is 2.5-7.5% of the mass of the monomeric substances with amide groups, then add a cross-linking agent, wherein the mass of the cross-linking agent is 1-4% of the mass of the monomeric substances with amide groups, and continue stirring at room temperature for 1-3 hours to obtain a gel electrolyte precursor solution.

2. The method for preparing a gel electrolyte precursor according to claim 1, It is characterized in that In step 2, the mass ratio of the silicone coupling agent to the alginate is (0.4-2.5):

1.

3. The method for preparing a gel electrolyte precursor according to claim 1, It is characterized in that In step 3, the photoinitiator includes 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

4. A gel electrolyte precursor, It is characterized in that Prepared according to the preparation method according to any one of claims 1 to 3.

5. A hydrogel film, It is characterized in that The gel electrolyte precursor solution according to claim 4 is injected into a mold and polymerized under ultraviolet light, wherein the mold has a thickness of 0.3-1.5 mm and is polymerized under ultraviolet light with a wavelength of 320-400 nm for 1-2 hours.

6. A gel electrolyte, It is characterized in that The hydrogel film according to claim 5 is obtained by drying and immersing it in a mixed electrolyte, wherein the hydrogel film after polymerization is taken out, placed in an oven and dried at 50-80°C for 20-60 minutes, and finally immersed in a mixed electrolyte containing zinc salt and sodium salt for 2-3 days.

7. The gel electrolyte according to claim 6, It is characterized in that The concentration of the zinc salt is 0.5-2M, and the concentration of the sodium salt is 0.5-2M.

8. The gel electrolyte according to claim 6, It is characterized in that The zinc salt in the mixed electrolyte includes ZnSO 4 、Zn(TFSI) 2 、Zn(Cl) 2 , the sodium salt includes Na 2 SO 4 、Na(TFSI),NaCl.

9. A sodium-zinc mixed ion battery, include: a gel electrolyte layer comprising a gel electrolyte; a positive electrode sheet disposed on the first surface of the gel electrolyte layer; as well as A negative electrode sheet is disposed on the second surface of the gel electrolyte layer.

10. The method for preparing a sodium-zinc mixed ion battery according to claim 9, characterized in that: The following steps are involved: Step A: Preparation of positive electrode sheet: Prussian blue positive electrode active material, binder, and conductive agent are stirred into slurry in a weight ratio of 7-8:1-2:1, coated on titanium foil, dried in a vacuum oven, and then cut into thin sheets as positive electrode sheets. The loading amount of the positive electrode active material is 0.8-1.2 mg / cm 2 ; Step B: Battery assembly: Cut the gel electrolyte into thin slices and grind the zinc sheet with fine sandpaper before assembly. The assembly order is positive electrode shell, positive electrode sheet, gel electrolyte, zinc sheet, gasket, shrapnel, and negative electrode shell.