Sodium ion composite solid electrolyte, preparation method and sodium ion battery

Through the composite material of the inorganic active filler Na5MSi4O12 and polymer matrix, the preparation process of sodium ion solid electrolyte is simplified, the problems of complex process and high cost in the existing technology are solved, and high performance and low cost sodium ion composite solid electrolyte are achieved. .

CN118899515APending Publication Date: 2024-11-05SHANGHAI XUANYI NEW ENERGY DEV CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410936794.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The preparation process of existing sodium ion solid electrolytes is complex, with high production costs, and it is difficult to have high ionic conductivity and good processability.

Method used

The sodium ion composite solid electrolyte is prepared by wet ball milling and a one-time sintering process using composite materials of the inorganic active filler Na5MSi4O12 and polymer matrix and sodium salt, which simplifies the process and reduces costs.

Benefits of technology

The sodium ion composite solid electrolyte with high ionic conductivity, good electrochemical stability and high mechanical strength is achieved, which simplifies the preparation process and reduces production costs, making it suitable for large-scale manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899515A_ABST
    Figure CN118899515A_ABST
Patent Text Reader

Abstract

The invention discloses a sodion composite solid electrolyte, which comprises a polymer matrix, a sodium salt and an inorganic active filler, the chemical general formula of the inorganic active filler is Na5MSi4O12, M is one or more of La, Al, Sm, Eu, Gd, Sc and Y; the particle size of the inorganic active filler is 80-600 nm, the mass ratio of the polymer matrix to the sodium salt is (0.25-50): 1, and the inorganic active filler accounts for 0.1-80 wt.% of the total mass of the polymer matrix, the sodium salt and the inorganic active filler. The invention also discloses a preparation method of the sodium ion composite solid electrolyte and a sodium ion battery. The sodium ion composite solid electrolyte disclosed by the invention has good ionic conductivity and mechanical property, the production process is greatly simplified, and stable circulation of a sodium ion battery is also facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion composite solid electrolyte, a preparation method and a sodium ion battery. Background Art

[0002] Sodium-ion batteries have received extensive attention in recent years due to their abundant sodium resources, low cost, and similar working principles to lithium-ion batteries. However, sodium-ion batteries based on organic liquid electrolytes have serious safety issues, such as easy leakage of electrolytes, poor thermal stability, and easy combustion and explosion. In contrast, solid-state sodium batteries based on solid electrolytes exhibit advantages such as high safety, wide operating temperature, and easy direct stacking. Direct use of metallic sodium as the negative electrode can further improve the energy density of the battery.

[0003] At present, the most widely studied sodium ion solid electrolytes mainly include inorganic solid electrolytes, polymer solid electrolytes and composite solid electrolytes. Among them, inorganic solid electrolytes usually have high ionic conductivity, high ion migration number, good thermal stability and wide electrochemical stability window, but the high hardness makes it have poor processability and poor interface contact with the electrode. In contrast, polymer electrolytes have good viscoelasticity and flexibility, strong processability and low cost, and are easy to form a close interface contact with the electrode material. However, their ionic conductivity and ion migration number are relatively low, which makes it difficult to meet the requirements of battery operation. By combining inorganic solid electrolytes and polymer solid electrolytes, the resulting composite solid electrolyte can have the advantages of both under certain conditions.

[0004] Composite solid electrolytes are generally electrolytes obtained by combining inorganic fillers and polymer solid electrolytes. Inorganic fillers can be divided into inert fillers and active fillers. Inert fillers do not transport ions, and they mainly include Al2O3, SiO2, and ZrO2. Compared with inert fillers, active materials can participate in the ion conduction process to improve ion conductivity. Currently, there are mainly oxide solid electrolyte fillers (such as NASICON type electrolytes) and sulfide solid electrolyte fillers. Among them, the main preparation method of oxide solid electrolytes is the traditional solid phase sintering method. Its production process is complicated and usually requires secondary high-temperature sintering, which has a high production cost; while sulfide solid electrolytes have poor air stability, which brings great difficulties to the preparation process. In order to further promote the practical application of sodium-ion solid-state batteries, it is crucial to develop and prepare new sodium-ion composite solid electrolyte materials with good processability and high ionic conductivity. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a sodium ion composite solid electrolyte, a preparation method and a sodium ion battery.

[0006] In a first aspect, an embodiment of the present invention discloses a sodium ion composite solid electrolyte, comprising a polymer matrix, a sodium salt and an inorganic active filler, wherein the chemical formula of the inorganic active filler is: Na5MSi4O 12 , wherein M is one or more of La, Al, Sm, Eu, Gd, Sc, and Y; the particle size of the inorganic active filler is 80 to 600 nm, the mass ratio of the polymer matrix and the sodium salt is (0.25 to 50): 1, and the inorganic active filler accounts for 0.1 to 80 wt.% of the total mass of the polymer matrix, the sodium salt and the inorganic active filler.

[0007] Using the above technical solution, the present invention proposes an inorganic active filler with the general chemical formula: Na5MSi4O 12 The sodium ion composite solid electrolyte has high ionic conductivity, good electrochemical stability and high mechanical strength, which solves the problem of lack of high-performance sodium ion composite solid electrolytes and is conducive to simplifying the preparation process.

[0008] According to another specific embodiment of the present invention, the particle size of the inorganic active filler is 100-400 nm, the mass ratio of the polymer matrix and the sodium salt is (0.5-20):1, and the inorganic active filler accounts for 6-40 wt.% of the total mass of the polymer matrix, the sodium salt and the inorganic active filler.

[0009] According to another specific embodiment of the present invention, the chemical formula of the inorganic active filler is: Na5R 1-x La x SiO 12 , R is one of Sm, Eu, Gd, and Y, and the range of x is 0.05≤x≤0.3.

[0010] According to another specific embodiment of the present invention, the thickness of the sodium ion composite solid electrolyte is 50-150 μm.

[0011] According to another specific embodiment of the present invention, the polymer matrix is ​​one or more of polyacrylonitrile, poly(vinylidene fluoride-co-hexafluoropropylene), polyethylene oxide, polyvinylidene fluoride, polymethyl methacrylate and polyacrylamide, and the sodium salt is one or more of NaClO4, NaTFSI, NaPF6, NaCF3SO3 and NaFSI.

[0012] In a second aspect, an embodiment of the present invention discloses a method for preparing a sodium ion composite solid electrolyte, which is used to prepare a sodium ion composite solid electrolyte as in any embodiment of the first aspect, comprising the following steps:

[0013] Preparation of powder A: Weigh Na2CO3, SiO2 and M metal oxide, mix by wet ball milling, and dry to obtain powder A;

[0014] Preparation of inorganic active filler: sintering the powder A once, and dry-milling the product after the once sintering to obtain the inorganic active filler;

[0015] Preparation of suspension: dissolving the polymer matrix and sodium salt in a solvent, adding an inorganic active filler and stirring to obtain a suspension;

[0016] Preparation of sodium ion composite solid electrolyte: casting the suspension into a mold and vacuum drying to obtain a sodium ion composite solid electrolyte;

[0017] Among them, M metal oxide is one or more of La2O3, Al2O3, Sm2O3, Eu2O3, Gd2O3, Sc2O3, and Y2O3.

[0018] By adopting the above technical scheme and introducing a new inorganic active filler, on the one hand, the crystallinity of the polymer matrix can be reduced, and a fast ion migration channel can be formed near the particles to promote the migration of sodium ions; on the other hand, it can directly participate in the sodium ion transmission process and synergistically improve the migration rate of sodium ions. The preparation method of the present invention is simple, including secondary ball milling, primary sintering, and the composite of the inorganic active filler and the polymer matrix, wherein the inorganic active filler only needs one sintering to be prepared, which can reduce the production cost of the sodium ion composite solid electrolyte and is conducive to large-scale manufacturing.

[0019] According to another specific embodiment of the present invention, in the preparation of powder A, Na2CO3, SiO2 and M metal oxide are weighed in a molar ratio of 5:8:1.

[0020] According to another specific embodiment of the present invention, the wet ball milling time is 12 to 16 hours; the total dry ball milling time is 10 to 20 hours; the primary sintering temperature is 800 to 950° C., and the sintering time is 8 to 15 hours; and the vacuum drying time is 12 to 24 hours.

[0021] According to another specific embodiment of the present invention, during the preparation of the suspension, the concentration of the polymer in the solvent is 0.1-0.5 g / mL; and the dissolution temperature is 30-60°C.

[0022] In a third aspect, an embodiment of the present invention further discloses a sodium ion battery, comprising a sodium ion composite solid electrolyte as in any embodiment of the first aspect, or comprising a sodium ion composite solid electrolyte obtained by the preparation method as in any embodiment of the second aspect.

[0023] By adopting the above technical scheme, the sodium ion composite solid electrolyte provided by the present invention has good practicality, can provide the ionic conductivity required for the operation of the sodium ion battery, and can maintain good interface contact and stability between the electrodes, which helps to achieve stable circulation of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the sodium ion composite solid electrolyte of the present invention;

[0025] Figure 2 This is the constant current charge and discharge curve of the sodium ion battery of Application Example 1 of the present invention;

[0026] Figure 3 The cycle performance of the sodium ion battery of Application Example 1 of the present invention.

[0027] 1. Polymer matrix, 2. Sodium salt, 3. Inorganic active filler DETAILED DESCRIPTION

[0028] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0029] It should be noted that in this specification, similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings.

[0030] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0031] The inventors carefully studied the sodium ion composite solid electrolyte and its preparation method in the prior art and found that the inorganic active fillers in the prior art usually use oxide solid electrolyte fillers (such as NASICON type electrolytes) and sulfide solid electrolytes, among which the main preparation method of oxide solid electrolyte materials in the prior art is the traditional solid phase sintering method, which has a complex production process and usually requires a secondary high-temperature sintering process to prepare inorganic active fillers, and the production cost is high; the sulfide solid electrolyte has poor air stability and is difficult to operate in the air, which greatly increases the difficulty of the preparation process. The inventors hope to develop and prepare a new sodium ion composite solid electrolyte with good processability and high ionic conductivity, so as to obtain a sodium ion composite solid electrolyte that only needs one sintering in the preparation process while ensuring high room temperature ionic conductivity.

[0032] First, refer to Figure 1 The embodiment of the present invention discloses a sodium ion composite solid electrolyte, comprising a polymer matrix 1, a sodium salt 2 and an inorganic active filler 3, wherein the chemical formula of the inorganic active filler 3 is: Na5MSi4O 12 , wherein M is one or more of La, Al, Sm, Eu, Gd, Sc, and Y; the particle size of the inorganic active filler 3 is 80 to 600 nm (including endpoint values); the mass ratio of the polymer matrix 1 and the sodium salt 2 is (0.25 to 50): 1; the inorganic active filler 3 accounts for 0.1 to 80 wt.% (including endpoint values) of the total mass of the polymer matrix 1, the sodium salt 2, and the inorganic active filler 3.

[0033] Continue to refer Figure 1 , the sodium salt 2 is uniformly dissolved in the polymer matrix 1, and the inorganic active filler 3 is uniformly dispersed in the polymer matrix 1. The sodium ion composite solid electrolyte of the present invention has the characteristics of both oxide solid electrolyte and polymer solid electrolyte, can achieve higher ion conductivity, and retain the flexibility and adhesion of the polymer, has good processing characteristics, and is conducive to achieving close contact between the electrolyte and the electrode.

[0034] In addition, the present invention proposes for the first time an inorganic active filler 3 having the general chemical formula: Na5MSi4O 12 The sodium ion composite solid electrolyte has high ionic conductivity, good electrochemical stability and high mechanical strength, solves the problem of lack of high-performance sodium ion composite solid electrolyte, and is conducive to simplifying the preparation process. By regulating the particle size and added mass ratio of the inorganic active filler 3, and the mass ratio of the polymer matrix 1 and the sodium salt 2, the sodium ion composite solid electrolyte of the present invention also improves its own mechanical properties and is easier to form a film.

[0035] Further, the particle size of the inorganic active filler 3 is 100-400 nm (including the endpoint value), the mass ratio of the polymer matrix 1 and the sodium salt 2 is (0.5-20): 1, and the inorganic active filler 3 accounts for 6-40 wt.% (including the endpoint value) of the total mass of the polymer matrix 1, the sodium salt 2 and the inorganic active filler 3. It is beneficial to form a continuous ion transmission path between the inorganic active filler 3 and the polymer matrix 1. When the particle size of the inorganic active filler 3 is small, such as 300 nm, the uniformly dispersed nanoparticles will increase the ion conductive interface, which is beneficial to improve the ion conductivity of the composite solid electrolyte. When the mass ratio of the above-mentioned inorganic active filler is too low, the amorphous region of the polymer matrix 1 is small, and the ion transmission is still limited; when the mass ratio of the inorganic active filler reaches a critical value, on the one hand, the crystallization of the polymer matrix is ​​effectively inhibited, and the movement of the local chain segments is increased. On the other hand, the polymer matrix / inorganic active filler interface and the ion-conductive active filler can guide the migration of sodium ions and construct a continuous and rapid ion transmission path; when an excessive amount of inorganic active filler 3 is added to the composite solid electrolyte, the interface ion channel is disturbed, which may also hinder the movement of the polymer matrix 1 chain segments and reduce the ion transmission in the polymer matrix 1 region, resulting in a decrease in ionic conductivity. In addition, excessive addition of inorganic active filler 3 may cause agglomeration, hinder the movement of the polymer matrix 1 chain segments, and reduce the ion transmission in the polymer matrix 1 region. The setting range of the mass ratio of the polymer matrix 1 and the sodium salt 2 will also affect the ionic conductivity of the sodium ion composite solid electrolyte. Therefore, only when the above three conditions are met at the same time, that is, when the particle size of the above-mentioned inorganic active filler 3, the mass ratio of the polymer matrix 1 and the sodium salt 2, and the inorganic active filler 3 accounts for the total mass of the polymer matrix 1, the sodium salt 2 and the inorganic active filler 3 are met, can better ionic conductivity be obtained.

[0036] The inventors have also found through experimental research that when M in the inorganic active filler is a mixture of R and La, specifically, the chemical formula of the inorganic active filler is: Na5R 1-x La x SiO 12 , wherein R is one of Sm, Eu, Gd, and Y, and when the range of x is 0.05≤x≤0.3, the ionic conductivity of the sodium ion composite solid electrolyte of the present invention can be further improved.

[0037] The thickness of the sodium ion composite solid electrolyte of the present invention is 50-150 μm, thereby reducing the thickness of the electrolyte membrane as much as possible while ensuring good film forming properties and mechanical strength.

[0038] The polymer matrix 1 of the present invention is one or more of polyacrylonitrile (PAN), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA) and polyacrylamide (PAM), and the sodium salt 2 is one or more of sodium perchlorate (NaClO4), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), sodium hexafluorophosphate (NaPF6), sodium trifluoromethylsulfonate (NaCF3SO3) and sodium bis(trifluoromethylsulfonyl)imide (NaFSI).

[0039] In a second aspect, an embodiment of the present invention discloses a method for preparing a sodium ion composite solid electrolyte, comprising the following steps:

[0040] Preparation of powder A: Weigh Na2CO3, SiO2 and M metal oxide, mix by wet ball milling, and dry to obtain powder A;

[0041] Preparation of inorganic active filler: sintering the powder A once, and dry-milling the product after the once sintering to obtain the inorganic active filler;

[0042] Preparation of suspension: dissolving the polymer matrix and sodium salt in a solvent, adding an inorganic active filler and stirring to obtain a suspension;

[0043] Preparation of sodium ion composite solid electrolyte: casting the suspension into a mold and vacuum drying to obtain a sodium ion composite solid electrolyte;

[0044] Among them, M metal oxide is one or more of La2O3, Al2O3, Sm2O3, Eu2O3, Gd2O3, Sc2O3, and Y2O3.

[0045] By adopting the above technical scheme and introducing a new type of inorganic active filler, the inorganic active filler can be prepared by only one sintering, and the inorganic active filler does not form a dense structure during the one sintering. At this time, it is easier to obtain nanoparticles by ball milling, which greatly simplifies the production process, can reduce the production cost of sodium ion composite solid electrolytes, and is conducive to large-scale manufacturing.

[0046] In the preparation of powder A, Na2CO3, SiO2 and M metal oxide are weighed in a molar ratio of 5:8:1. Thus, a sodium ion solid electrolyte with stable properties and high room temperature ionic conductivity can be obtained without adding more sodium salt and only requiring a lower primary sintering temperature.

[0047] The ball milling time of wet ball milling is 12 to 16 hours (including the endpoint value); the dry ball milling adopts step-type ball milling, with a single ball milling of 2 hours and a total ball milling time of 10 to 20 hours (including the endpoint value); the temperature of the first sintering is 800 to 950°C (including the endpoint value), and the sintering time is 8 to 15 hours (including the endpoint value); the vacuum drying time is 12 to 24 hours (including the endpoint value). Furthermore, the vacuum drying temperature is 50 to 80°C. The inorganic active filler of the present invention does not require secondary sintering during preparation, has a lower sintering temperature and a short sintering time, and the entire preparation cycle is short and simple, which greatly reduces the preparation cost of the composite solid electrolyte.

[0048] During the preparation of the suspension, the polymer concentration in the solvent is 0.1-0.5 g / mL (including the endpoint value); the dissolution temperature is 30-60°C (including the endpoint value). Good dispersibility of the inorganic active filler 3 in the polymer matrix 1 is a prerequisite for obtaining any good structure or performance. The above-mentioned polymer concentration and dissolution temperature are conducive to uniform dispersion of the inorganic active filler 3 and obtaining a composite solid electrolyte with good overall performance. Among them, the type of solvent is determined according to the degree of solubility of the polymer matrix.

[0049] In a third aspect, an embodiment of the present invention further discloses a sodium ion battery, comprising the sodium ion composite solid electrolyte. The sodium ion composite solid electrolyte provided by the present invention has good practicality, can provide the ionic conductivity required for the operation of the sodium ion battery, and can maintain good interface contact and stability with the electrodes, thereby ensuring the stable cycle of the sodium ion battery.

[0050] Among them, the sodium ion battery also includes a positive electrode and a negative electrode, and the above-mentioned sodium ion composite solid electrolyte is located between the positive electrode and the negative electrode. The positive electrode contains positive electrode active material particles, a conductive additive and a binder, and the negative electrode can be a sodium metal element or a sodium alloy, or it can contain negative electrode active material particles, a conductive additive and a binder. The positive electrode active material particles refer to sodium-embedded compounds that can reversibly embed and remove sodium ions, such as polyanionic materials, layered metal oxide materials and Prussian blue materials. The negative electrode active material particles refer to sodium-embedded materials that can reversibly embed and remove sodium ions, such as carbon materials, metal oxides and transition metal sulfides. The conductive additive is generally selected from one of Super P (SP), Ketjen black (KB), acetylene black (AB), carbon nanotubes (CNT) and graphene. The binder is generally selected from one of polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC) and sodium alginate (SA).

[0051] Furthermore, the mass ratio of the positive electrode active material particles, the conductive aid and the binder is (0.7-0.9): (0.05-0.2): (0.05-0.1); the mass ratio of the negative electrode active material particles, the conductive aid and the binder is (0.7-0.9): (0.05-0.2): (0.05-0.1), for example 0.7:0.2:0.1.

[0052] In the present invention, the preparation method of the positive electrode is specifically as follows: the positive electrode active material particles, the conductive aid and the binder are weighed according to the above mass ratio, a solvent is added to make them uniformly dispersed and mixed, and then the obtained slurry is coated on the surface of the aluminum foil, and after drying, it is cut into electrode sheets of a certain size for use.

[0053] In the present invention, the method for preparing the sodium metal element or the sodium alloy negative electrode is: cutting the sodium metal into sheets, or pressing the alloy powder into sheets for use. The method for preparing the sodium embedded material negative electrode is specifically: weighing the negative electrode active material particles, the conductive additive and the binder according to the above mass ratio, adding a solvent to evenly disperse and mix, then coating the obtained slurry on the surface of aluminum foil or copper foil, and cutting it into electrode sheets of a certain size after drying for standby use. Among them, the solvent is generally selected from deionized water or N-methylpyrrolidone (NMP) according to the type of binder.

[0054] In the present invention, the area of ​​the sodium ion composite solid electrolyte membrane>the area of ​​the negative electrode≥the area of ​​the positive electrode to ensure that the positive electrode capacity is fully utilized. In addition, in order to ensure the good electrochemical performance of the sodium ion battery, the above-mentioned sodium ion composite solid electrolyte is adhered to the surface of at least one of the positive electrode and the negative electrode of the sodium ion battery. The above-mentioned adhesion, for example, refers to the sodium ion composite solid electrolyte suspension being directly cast on the surface of the positive electrode or the negative electrode and then dried, or it can be that the sodium ion composite solid electrolyte is pasted on the surface of the positive electrode or the negative electrode through an ion conductive glue. The composite solid electrolyte adheres to the surface of the positive electrode or the negative electrode, which helps to reduce the interface resistance between the electrolyte and the electrode, and ensure the normal operation of the sodium ion battery.

[0055] The present invention provides a method for preparing a sodium ion battery, comprising the following steps:

[0056] S1: uniformly mixing positive electrode active material particles or negative electrode active material particles, a conductive additive and a binder in a solvent to prepare a viscous slurry;

[0057] S2: evenly coating the slurry on aluminum foil or copper foil, placing the coated foil in a vacuum oven after the solvent evaporates to completely dry the electrode, and cutting the electrode into fixed sizes for later use;

[0058] S3: placing the electrode obtained in step S2 in a polytetrafluoroethylene mold, casting the suspension obtained in the preparation method of the sodium ion composite solid electrolyte on the surface of the electrode, and completely drying under vacuum;

[0059] S4 removes the oxide layer on the surface of the metallic sodium, and cuts it into metallic sodium discs with a fixed diameter after rolling;

[0060] S5 assembles the battery in the order of positive electrode, composite solid electrolyte and negative electrode in a glove box filled with argon.

[0061] Example 1

[0062] PAN-NaClO4-Na5SmSi4O 12 The preparation of sodium ion composite solid electrolyte membrane is as follows:

[0063] (1) Preparation of powder A: Anhydrous Na2CO3, SiO2 and Sm2O3 were weighed in a molar ratio of 5:8:1 and wet ball milled. Anhydrous ethanol was used as a dispersant. The mass ratio of the total mass of anhydrous Na2CO3, SiO2 and Sm2O3 to anhydrous ethanol was 1:2. The ball-to-material ratio was 15:1. The ball milling speed was 600 rpm and the ball milling time was 15 hours. Powder A was obtained after ball milling.

[0064] (2) Preparation of inorganic active filler: Powder A was dried at 120 °C for 12 h and sintered once at a heating rate of 5 °C min -1 The sintering temperature was 800℃, the sintering time was 8 hours, and then it was naturally cooled to room temperature, and dry ball milling was performed. The ball-to-material mass ratio was 15:1, the ball milling speed was 600rpm, and the step-type ball milling was used. The single ball milling was 2 hours, and the total cycle was 7 times. The total ball milling time was 14 hours, and the particle size was about 300nm.

[0065] (3) Preparation of suspension: PAN and NaClO4 were weighed in a mass ratio of 0.85:1, and solvent N,N-dimethylformamide (DMF) was added. The polymer concentration in the solvent was 0.1 g / mL. After stirring at 60°C until completely dissolved, 20 wt.% Na5SmSi4O 12 Add and stir for 24 hours until the mixture is uniform;

[0066] (4) Preparation of sodium ion composite solid electrolyte: The above suspension was cast on the surface of a polytetrafluoroethylene mold and completely dried under vacuum at 60°C for 24 hours to obtain a PAN-NaClO4-Na5SmSi4O4 composite electrolyte with a thickness of about 90 μm. 12 Sodium ion composite solid electrolyte membrane.

[0067] Example 2

[0068] PEO-NaTFSI-Na5SmSi4O 12 The preparation of sodium ion composite solid electrolyte membrane is as follows:

[0069] (1) Preparation of powder A: Anhydrous Na2CO3, SiO2 and Sm2O3 were weighed in a molar ratio of 5:8:1 and wet ball milled. Anhydrous ethanol was used as a dispersant. The mass ratio of the total mass of anhydrous Na2CO3, SiO2 and Sm2O3 to anhydrous ethanol was 1:2. The ball-to-material ratio was 15:1. The ball milling speed was 600 rpm and the ball milling time was 15 hours. Powder A was obtained after ball milling.

[0070] (2) Preparation of inorganic active filler: Powder A was dried at 120 °C for 12 h and sintered once at a heating rate of 5 °C min -1 The sintering temperature was 800℃, the sintering time was 8 hours, and then it was naturally cooled to room temperature, and then dry ball milling was carried out, the ball-to-material mass ratio was 15:1, the ball milling speed was 600rpm, and the step-type ball milling was used. The single ball milling took 2 hours, and the total cycle was 7 times. The total ball milling time was 14 hours, and the particle size was about 300nm.

[0071] (3) Preparation of suspension: PEO and NaTFSI were weighed in a mass ratio of 1.75:1, and deionized water was added as solvent. The polymer concentration in the solvent was 0.15 g / mL. After stirring at 60°C until completely dissolved, 5 wt.% Na5SmSi4O 12 Add and stir for 24 hours until the mixture is uniform;

[0072] (4) Preparation of sodium ion composite solid electrolyte: The above suspension was cast on the surface of a polytetrafluoroethylene mold and completely dried under vacuum at 60°C for 24 hours to obtain a PEO-NaTFSI-Na5SmSi4O3 composite electrolyte with a thickness of about 100 μm. 12 Sodium ion composite solid electrolyte membrane.

[0073] Example 3

[0074] PEO-NaTFSI-Na5Sm 0.95 La 0.05 SiO 12 The preparation of sodium ion composite solid electrolyte membrane is as follows:

[0075] (1) Preparation of powder A: Anhydrous Na2CO3, SiO2, Sm2O3 and La2O3 were weighed in a molar ratio of 5:8:0.95:0.05, and wet ball milled. Anhydrous ethanol was used as a dispersant. The mass ratio of the total mass of anhydrous Na2CO3, SiO2, Sm2O3 and La2O3 to anhydrous ethanol was 1:2. The ball-to-material ratio was 15:1. The ball milling speed was 600 rpm. The ball milling time was 15 hours. After ball milling, powder A was obtained.

[0076] (2) Preparation of inorganic active filler: Powder A was dried at 120 °C for 12 h and sintered once at a heating rate of 5 °C min -1 The sintering temperature was 800℃, the sintering time was 8 hours, and then it was naturally cooled to room temperature, and then dry ball milling was carried out, the ball-to-material mass ratio was 15:1, the ball milling speed was 600rpm, and the step-type ball milling was used. The single ball milling was 2 hours, and the total cycle was 8 times. The total ball milling time was 16 hours, and the particle size was about 300nm.

[0077] (3) Preparation of suspension: PEO and NaTFSI were weighed in a mass ratio of 1.75:1, and deionized water was added as solvent. The polymer concentration in the solvent was 0.15 g / mL. After stirring at 60°C until completely dissolved, Na5Sm with a mass fraction of 5 wt.% was weighed. 0.95 La 0.05 SiO 12 Add and stir for 24 hours until the mixture is uniform;

[0078] (4) Preparation of sodium ion composite solid electrolyte: The above suspension was cast on the surface of a polytetrafluoroethylene mold and completely dried under vacuum at 60°C for 24 hours to obtain a PEO-NaTFSI-Na5Sm 0.95 La 0.05 SiO 12 Sodium ion composite solid electrolyte membrane.

[0079] Example 4

[0080] The difference from Example 2 is that the total dry ball milling time in step (2) is 10 hours, the particle size of the inorganic active filler 3 is about 600 nm, and the PEO-NaTFSI-Na5SmSi4O 12 Sodium ion composite solid electrolyte membrane.

[0081] Comparative Example 1

[0082] (1) Preparation of suspension: PEO and NaTFSI were weighed in a mass ratio of 1.75:1, deionized water was added as solvent, and the polymer concentration in the solvent was 0.15 g / mL, and stirred at 60 °C until completely dissolved;

[0083] (2) Preparation of polymer solid electrolyte membrane: The above suspension was cast on the surface of a polytetrafluoroethylene mold and completely dried under vacuum at 60° C. for 24 hours to obtain a PEO-NaTFSI polymer solid electrolyte membrane with a thickness of about 100 μm.

[0084] Comparative Example 2

[0085] (1) Preparation of suspension: PEO and NaTFSI were weighed in a mass ratio of 1.75:1, and deionized water was added as solvent. The polymer concentration in the solvent was 0.15 g / mL. After stirring at 60°C until completely dissolved, 5 wt.% of purchased inorganic active filler Na3Zr2Si2PO4 with a particle size of about 300 nm was weighed. 12 Add and stir for 24 hours until the mixture is uniform;

[0086] (2) Preparation of sodium ion composite solid electrolyte: The above suspension was cast on the surface of a polytetrafluoroethylene mold and completely dried under vacuum at 60°C for 24 hours to obtain a PEO-NaTFSI-Na3Zr2Si2PO4 with a thickness of about 100 μm. 12 Sodium ion composite solid electrolyte membrane.

[0087] Application Example 1

[0088] Na4Fe(PO4)2P2O7 / PAN-NaClO4-Na5SmSi4O 12 / Na preparation of solid-state sodium batteries.

[0089] (1) Na4Fe(PO4)2P2O7, Super P and CMC binder were uniformly mixed in deionized water in a mass ratio of 7:2:1 to prepare a viscous slurry;

[0090] (2) The slurry was evenly coated on aluminum foil. After the deionized water on the surface evaporated, the aluminum foil coated with the material was transferred to a 60°C vacuum oven to completely dry the electrode. The electrode was then cut into discs with a diameter of 1 cm as the positive electrode;

[0091] (3) The above positive electrode is placed in a polytetrafluoroethylene mold, and the PAN-NaClO4-Na5SmSi4O 12 Step (3) casting the suspension on the positive electrode surface and completely drying it under vacuum at 60°C;

[0092] (4) In a glove box filled with argon, the oxide layer on the surface of the sodium metal was removed, rolled into thin sheets, and then cut into sodium metal discs with a diameter of 1.2 cm as the negative electrode;

[0093] (5) Paste the sodium metal disc on the side of the electrolyte membrane without the positive electrode, ensuring that the edge of the negative electrode exceeds the edge of the positive electrode, and finally package it with a CR2032 button battery.

[0094] In order to further highlight the effect of the present invention, Table 1 summarizes the ionic conductivity of different embodiments and comparative examples. Among them, the ionic conductivity is measured by AC impedance method, stainless steel sheet is used as blocking electrode, the test frequency range is 1Hz~5MHz, and the applied bias voltage is 20mV. It can be seen from the table that the sodium ion composite solid electrolyte of each embodiment of the present invention is compared with the solid electrolyte without inorganic active filler in comparative example 1 and the inorganic active filler Na3Zr2Si2PO4 in the prior art in comparative example 2. 12 The composite solid electrolyte of the present invention has a greatly improved ionic conductivity. At the same time, in Example 2 and Example 4, since the particle size of the inorganic active filler in Example 4 is about 600nm, the ionic conductivity of Example 4 is lower than that of Example 2. And since Example 3 satisfies the chemical formula of the inorganic active filler: Na5R 1-x La x SiO 12 , R is one of Sm, Eu, Gd, and Y, and the range of x is 0.05≤x≤0.3. The ionic conductivity of Example 3 is further improved.

[0095] Table 1 Ionic conductivity of different embodiments and comparative examples

[0096] <![CDATA[Ionic conductivity (S cm -1 )]]> Example 1 <![CDATA[2.3×10 -4 ]]> Example 2 <![CDATA[1.9×10 -4 ]]> Example 3 <![CDATA[2.5×10 -4 ]]> Example 4 <![CDATA[1.1×10 -4 ]]> Comparative Example 1 <![CDATA[1.2×10 -5 ]]> Comparative Example 2 <![CDATA[8.6×10 -5 ]]>

[0097] like Figure 2 and Figure 3 As shown in the figure, the constant current charge-discharge curve and cycle performance of the sodium ion battery of the first embodiment of the present invention at a constant temperature of 60°C are respectively shown, wherein "Voltage" represents voltage, "Specific Capacity" represents specific capacity, and "Cycle Number" represents the number of cycles. It can be seen that the PAN-NaClO4-Na5SmSi4O prepared by the first embodiment of the present invention 12 Application Example 1 of the electrolyte assembly: a sodium ion battery can provide 98 mA hg when subjected to a constant current charge and discharge test at a rate of 0.5 C. -1 The reversible specific capacity (calculated based on the mass of the positive electrode active material) of the present invention can be stably cycled for more than 300 times, which proves that the sodium ion composite solid electrolyte provided by the present invention has good practicality, can provide the ionic conductivity required for the operation of the sodium ion battery, and can maintain good interface contact and stability with the electrodes, thereby ensuring the stable cycle of the sodium ion battery.

[0098] In summary, the sodium ion composite solid electrolyte of the present invention introduces a new type of oxide sodium ion conductor with high ionic conductivity as an inorganic active filler. On the one hand, the addition of the inorganic active filler 3 can reduce the crystallinity of the polymer matrix 1 and form a fast ion transmission channel near the particles; on the other hand, the inorganic active filler 3 of the present invention can partially participate in the migration of sodium ions, and play a role in synergistically improving the ionic conductivity of the composite solid electrolyte. The sodium ion composite solid electrolyte of the present invention retains the flexibility and adhesion of the polymer matrix 1, ensures good interface contact with the electrodes, and helps to achieve the normal operation and stable cycle of the sodium ion battery. And in the preparation process, no secondary sintering is required, with a lower sintering temperature and a short sintering time, which reduces the preparation cost of the composite solid electrolyte and is conducive to large-scale production.

[0099] Although the present invention has been illustrated and described with reference to certain preferred embodiments of the present invention, it should be understood by those skilled in the art that the above is a further detailed description of the present invention in conjunction with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. Those skilled in the art may make various changes in form and details, including making several simple deductions or substitutions, without departing from the spirit and scope of the present invention.

Claims

1. A sodium ion composite solid electrolyte, characterized in that: The invention comprises a polymer matrix, a sodium salt and an inorganic active filler, wherein the inorganic active filler has a chemical formula of: Na5MSi4O 12 , wherein M is one or more of La, Al, Sm, Eu, Gd, Sc, and Y; the particle size of the inorganic active filler is 80 to 600 nm, the mass ratio of the polymer matrix to the sodium salt is (0.25 to 50): 1, and the inorganic active filler accounts for 0.1 to 80 wt.% of the total mass of the polymer matrix, the sodium salt and the inorganic active filler.

2. The sodium ion composite solid electrolyte according to claim 1, characterized in that The particle size of the inorganic active filler is 100-400 nm, the mass ratio of the polymer matrix to the sodium salt is (0.5-20):1, and the inorganic active filler accounts for 6-40 wt.% of the total mass of the polymer matrix, the sodium salt and the inorganic active filler.

3. The sodium ion composite solid electrolyte according to claim 2, characterized in that The general chemical formula of the inorganic active filler is: Na5R 1-x La x SiO 12 , R is one of Sm, Eu, Gd, and Y, and the range of x is 0.05≤x≤0.

3.

4. The sodium ion composite solid electrolyte according to claim 1, characterized in that The thickness of the sodium ion composite solid electrolyte is 50 to 150 μm.

5. The sodium ion composite solid electrolyte according to claim 1, characterized in that The polymer matrix is ​​one or more of polyacrylonitrile, poly(vinylidene fluoride-co-hexafluoropropylene), polyethylene oxide, polyvinylidene fluoride, polymethyl methacrylate and polyacrylamide, and the sodium salt is one or more of NaClO4, NaTFSI, NaPF6, NaCF3SO3 and NaFSI.

6. A method for preparing a sodium ion composite solid electrolyte, characterized in that: The method for preparing the sodium ion composite solid electrolyte according to any one of claims 1 to 4 comprises the following steps: Preparation of powder A: Weigh Na2CO3, SiO2 and M metal oxide, mix by wet ball milling, and dry to obtain powder A; Preparation of inorganic active filler: sintering the powder A once, and dry-milling the product after the once sintering to obtain the inorganic active filler; Preparation of suspension: dissolving the polymer matrix and the sodium salt in a solvent, adding the inorganic active filler and stirring to obtain a suspension; Preparation of sodium ion composite solid electrolyte: casting the suspension in a mold, and vacuum drying to obtain a sodium ion composite solid electrolyte; Wherein, the M metal oxide is one or more of La2O3, Al2O3, Sm2O3, Eu2O3, Gd2O3, Sc2O3, and Y2O3.

7. The method for preparing the sodium ion composite solid electrolyte according to claim 6, characterized in that: In the preparation of the powder A, the Na2CO3, SiO2 and M metal oxide are weighed in a molar ratio of 5:8:

1.

8. The method for preparing the sodium ion composite solid electrolyte according to claim 6, characterized in that: The ball milling time of the wet ball milling is 12 to 16 hours; the total ball milling time of the dry ball milling is 10 to 20 hours; the temperature of the primary sintering is 800 to 950° C., and the sintering time is 8 to 15 hours; and the vacuum drying time is 12 to 24 hours.

9. The method for preparing the sodium ion composite solid electrolyte according to claim 6, characterized in that: During the preparation of the suspension, the polymer concentration in the solvent is 0.1-0.5 g / mL; and the dissolution temperature is 30-60°C.

10. A sodium ion battery, characterized in that: The invention comprises the sodium ion composite solid electrolyte as claimed in any one of claims 1 to 5, or comprises the sodium ion composite solid electrolyte obtained by the preparation method according to any one of claims 6 to 9.

Citation Information

Cited By

  • Preparation method of PEO-based polymer solid electrolyte

    CN119601764A

  • Polymer solid electrolyte and solid sodium battery based on polymer solid electrolyte

    CN119601766A

  • Semi-solid sodium ion battery as well as preparation method and application thereof

    CN121484183A

  • Semi-solid sodium-ion battery and preparation method and application thereof

    CN121484183B

  • Sodium-based composite solid electrolyte membrane and preparation method and application thereof

    CN122494778A